Nozzle for special-shaped cross-section glass fiber and method for producing special-shaped cross-section glass fiber

By providing an inclined portion at the end of the short wall portion of the special-shaped cross-section glass fiber nozzle hole, the deformation problem caused by the surface tension of the molten glass is solved, and fiber manufacturing with a high flatness is achieved.

CN115803293BActive Publication Date: 2024-11-08NIPPON ELECTRIC GLASS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202180042666.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2020-06-16
Filing Date
2021-05-18
Publication Date
2024-11-08
Estimated Expiration
2041-05-18

AI Technical Summary

Technical Problem

When manufacturing the special-shaped cross-sectional glass fiber, the surface area of ​​the molten glass becomes smaller due to the surface tension, making it difficult to form fibers with high flatness.

Method used

Design a nozzle for glass fiber with a special-shaped cross-section, the nozzle hole has a flat shape, a short wall part in the long-diameter direction and a long wall part in the short-diameter direction, and a shaft line relative to the nozzle hole is provided in the end area of ​​the short-diameter part. Inclined inclined portions to expand contact area and ability to stretch molten glass.

Benefits of technology

By increasing the stretching ability of the short wall portion, the surface area deformation of the molten glass is suppressed, and a high flat rate special-shaped cross-sectional glass fiber is successfully produced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115803293B_ABST
    Figure CN115803293B_ABST
Patent Text Reader

Abstract

A nozzle (8) for irregular cross-section glass fibers is provided with a flat nozzle hole (6), wherein the nozzle hole (6) has an inlet (6a) and an outlet (6b) for molten glass (2), and a wall portion surrounding the nozzle hole (6) has a pair of short wall portions (12) opposed in the long diameter direction of the nozzle hole (6) and a pair of long wall portions (11) opposed in the short diameter direction. The nozzle (8) for irregular cross-section glass fibers is used to manufacture irregular cross-section glass fibers (2f) using the molten glass (2) flowing out of the nozzle hole (6), and for each of the pair of short wall portions (12), an inclined portion (12aa) inclined relative to the axis (6x) of the nozzle hole (6) is provided in an end region (T) of the end of the short wall portion (12) located on the outlet (6b) side.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a nozzle for producing irregular cross-section glass fibers having a flat cross-sectional shape using molten glass, and a method for producing the irregular cross-section glass fibers using the nozzle. Background Art

[0002] As one type of glass fiber, a flat cross-sectional profiled glass fiber is known (see Patent Document 1). The profiled cross-sectional glass fiber can achieve a high reinforcing effect when compounded with a resin, and is therefore used in various fields such as as a fiber for fiber reinforced plastics (FRP).

[0003] When manufacturing a special-shaped cross-section glass fiber, for example, molten glass is supplied to an extruder from a feeder for circulating the molten glass, and the molten glass is drawn out from a plurality of nozzles provided in the extruder and cooled. The shape of the nozzle hole provided in the nozzle is generally a flat hole shape (elliptical, oblong, etc.).

[0004] Prior art literature

[0005] Patent Literature

[0006] Patent Document 1: International Publication No. 2017 / 221471 Summary of the invention

[0007] Technical problem that the invention aims to solve

[0008] When producing a deformed cross-section glass fiber, there is the following problem to be solved: That is, the molten glass flowing out of the nozzle hole is deformed so that the surface area becomes small due to surface tension, and thus it is difficult to form a deformed cross-section glass fiber with a high flatness.

[0009] The present invention has been made in view of the above circumstances and has the technical problem of enabling the production of a deformed cross-section glass fiber having a high flatness ratio when producing a deformed cross-section glass fiber.

[0010] Technical solutions to the problem

[0011] The present invention for solving the above-mentioned problems is a nozzle for glass fibers with special cross-sections, characterized in that a flat nozzle hole is provided, the nozzle hole has an inlet and an outlet for molten glass, a wall portion surrounding the nozzle hole has a pair of short wall portions opposing each other in the long diameter direction of the nozzle hole and a pair of long wall portions opposing each other in the short diameter direction, the nozzle for glass fibers with special cross-sections is used to manufacture glass fibers with special cross-sections using molten glass flowing out of the nozzle hole, and for each of the pair of short wall portions, an end region of the end of the short wall portion located on the outlet side has an inclined portion inclined relative to the axis of the nozzle hole.

[0012] In the present nozzle, the end region has an inclined portion that is inclined relative to the axis of the nozzle hole, so that the contact area between the end region and the molten glass is expanded compared to the conventional case where the end region does not have an inclined portion. As a result, the ability of the end region of the short wall portion to stretch the molten glass (the ability to stretch along the long diameter direction of the nozzle hole) is improved, and with this, the deformation of the molten glass that is reduced in surface area due to surface tension can be suppressed. As a result, the manufactured irregular cross-section glass fiber can be formed to have a high flatness.

[0013] In the above configuration, the inclined portion preferably has an inclined surface that is inclined so as to become more distant from the center side of the nozzle hole as it moves from the inlet side toward the outlet side.

[0014] This further improves the ability of the end region of the short wall portion to draw the molten glass, which is more advantageous in forming the special-shaped cross-section glass fiber with a high flatness.

[0015] In the above structure, the short wall portion preferably has a bottom wall surface connected to the inclined portion in the end area, and the long wall portion has a bottom wall surface at the end on the outflow side, and the sum of the length of the inclined portion in the cross section orthogonal to the short diameter direction and the length of the bottom wall surface of the short wall portion in the cross section orthogonal to the short diameter direction is longer than the length of the bottom wall surface of the long wall portion in the cross section orthogonal to the long diameter direction.

[0016] When manufacturing a special-shaped cross-section glass fiber, in addition to the inclined portion of the short wall portion, the bottom wall surface of the short wall portion and the long wall portion is also wetted by the molten glass. At this time, the inclined portion and the bottom wall surface stretch the molten glass. Furthermore, in order to improve the flatness of the manufactured special-shaped cross-section glass fiber, it is advantageous to stretch the molten glass along the long diameter direction compared to the short diameter direction of the nozzle hole. In addition, if this structure is adopted, the molten glass can be effectively stretched along the long diameter direction of the nozzle hole, which is more advantageous in forming the special-shaped cross-section glass fiber into a high flatness.

[0017] In the above structure, it is preferable that the inclined portion is composed of a single inclined surface.

[0018] This makes it difficult for the molten glass to stagnate, and it is possible to suppress devitrification.

[0019] Furthermore, the present invention for solving the above-mentioned problems is a method for manufacturing irregular cross-section glass fibers, characterized in that the manufacturing is carried out using a nozzle for irregular cross-section glass fibers, the nozzle for irregular cross-section glass fibers is provided with a flat nozzle hole, the nozzle hole has an inlet and an outlet for molten glass, the wall portion surrounding the nozzle hole has a pair of short wall portions opposing each other in the long diameter direction of the nozzle hole and a pair of long wall portions opposing each other in the short diameter direction, the nozzle for irregular cross-section glass fibers is used, the manufacturing method is used to manufacture irregular cross-section glass fibers using molten glass flowing out of the nozzle hole, for each of the pair of short wall portions, the end area of ​​the end of the short wall portion located on the outlet side has an inclined portion inclined relative to the axis of the nozzle hole.

[0020] According to this method, the same actions and effects as those already described can be obtained for the above-mentioned nozzle for irregular-section glass fibers.

[0021] Effects of the Invention

[0022] According to the present invention, when producing a special-shaped cross-section glass fiber, a fiber with a high flatness can be produced. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 This is a cross-sectional view schematically showing a method and apparatus for producing a deformed-cross-section glass fiber.

[0024] Figure 2 This is a cross-sectional view schematically showing the periphery of a nozzle for a special-shaped cross-section glass fiber.

[0025] Figure 3 This is a bottom view schematically showing the periphery of a nozzle for irregular-section glass fibers.

[0026] Figure 4 (a) is a side view of the nozzle for the special-shaped cross-section glass fiber as viewed from the long wall side, and (b) is Figure 3 (4b-4b) is a cross-sectional view of the nozzle, and (c) is a cross-sectional view of (a) at 4c-4c.

[0027] Figure 5 It is a magnified representation Figure 4 (b) is a cross-sectional view of part A.

[0028] Figure 6 This is a cross-sectional view showing the periphery of the bottom wall surface of the long wall portion in the nozzle for deformed-cross-section glass fibers.

[0029] Figure 7 It is a cross-sectional view showing a glass fiber with a special cross section.

[0030] Figure 81 is a diagram showing a modified example of a nozzle for a special-shaped cross-section glass fiber, (a) is a side view of the nozzle for a special-shaped cross-section glass fiber observed from the short wall side, (b) is Figure 3 (4b-4b cross-sectional view of the nozzle, (c) is the 4d-4d cross-sectional view of (a).

[0031] Fig. 9 It is a bottom view of a nozzle for irregular-section glass fibers according to a modification.

[0032] Explanation of symbols

[0033] 2 Molten Glass

[0034] 2f Special-section glass fiber

[0035] 6 Nozzle hole

[0036] 6a Inlet

[0037] 6b Outlet

[0038] 6x Axis

[0039] 8 Nozzles for special-shaped cross-section glass fibers

[0040] 11 Longwall

[0041] 11b Bottom wall

[0042] 12 Short wall

[0043] 12a inner wall surface

[0044] 12aa Inclined portion

[0045] 12b bottom wall surface

[0046] L1 Length

[0047] L2 Length

[0048] L3 Length

[0049] T-terminal region DETAILED DESCRIPTION

[0050] Hereinafter, a nozzle for a modified cross-section glass fiber and a method for producing a modified cross-section glass fiber according to an embodiment of the present invention will be described with reference to the drawings.

[0051] like Figure 1As shown, the special-shaped cross-section glass fiber is manufactured by a manufacturing device 1. The manufacturing device 1 includes: a feeder 3 that flows a molten glass 2 generated by a melting furnace (not shown); an extruder 4 that is arranged at a position lower than the feeder 3; and a tube 5 that connects the feeder 3 and the extruder 4. The molten glass 2 is supplied from the feeder 3 to the extruder 4 via the tube 5. Then, the molten glass 2 flows out from the nozzle hole 6 of the extruder 4. The molten glass 2 is cooled to become a special-shaped cross-section glass fiber 2f (hereinafter, referred to as glass fiber 2f).

[0052] In the present embodiment, the molten glass 2 is made of E glass, but the present invention is not limited thereto, and the molten glass 2 may be made of other glass such as D glass, S glass, AR glass, or C glass.

[0053] The feeder 3 is connected to a glass melting furnace (not shown). The feeder 3 can flow the molten glass 2 continuously produced in the glass melting furnace. Inside the feeder 3, a liquid level 2a of the molten glass 2 is formed.

[0054] The extruder 4 has a base plate 7 at the bottom. A plurality of nozzles 8 for special-shaped cross-section glass fibers (hereinafter referred to as nozzles 8) and a cooling pipe 9 arranged near these nozzles 8 are provided on the base plate 7. The plurality of nozzles 8 have the same structure as each other. The details will be described later, and the nozzle hole 6 provided in each nozzle 8 is formed flat.

[0055] The tube 5 is formed into a cylindrical shape with a tube axis extending in the up-down direction. The upper end of the tube 5 is connected to the bottom of the feeder 3, and the lower end of the tube 5 is connected to the upper end of the extruder 4. It should be noted that as long as the tube 5 can connect the feeder 3 and the extruder 4, the shape and the direction in which the tube axis extends may be different from those in the present embodiment.

[0056] The extruder 4, the tube 5, the nozzle 8 and the cooling tube 9 are partially or entirely composed of platinum or a platinum alloy (such as a platinum-rhodium alloy). In addition, in the present embodiment, the tube 5 among these components is entirely composed of platinum or a platinum alloy.

[0057] The entire flow path from the connection between the feeder 3 and the tube 5 to the nozzle hole 6 of the extruder 4 is filled with the molten glass 2. Thus, the pressure (head pressure) for causing the molten glass 2 to flow out of the nozzle hole 6 is determined by the height difference H between the nozzle hole 6 and the liquid level 2a of the molten glass 2 in the feeder 3. Here, the height difference H can be adjusted by changing the length of the tube 5, for example.

[0058] The temperature and viscosity of the molten glass 2 when forming the glass fibers 2f are set to 1100°C to 1250°C (preferably 1150°C to 1200°C), 10 2.6 dPa·s~10 3.8 dPa·s (preferably 10 2.9dPa·s~10 3.3 dPa·s). It should be noted that the "temperature and viscosity of the molten glass 2" referred to herein refers to the temperature and viscosity of the molten glass 2 at the position where it flows into the nozzle 8. The temperature and viscosity of the molten glass 2 can be adjusted, for example, by heating the extruder 4 and the tube 5 separately by any heating unit (for example, an electric heating device). In addition, the temperature and viscosity of the molten glass 2 can also be adjusted by heating the molten glass 2 and the feeder 3 in the glass melting furnace by electric heating.

[0059] The surface of the glass fiber 2f is coated with a sizing agent by an applicator (not shown). Thus, about several hundred to several thousand glass fibers 2f are spun as a strand 2s. The spun strand 2s is wound on a bobbin 10 as a winding device to form a fiber bundle 2r. The strand 2s is cut into a length of about 1 mm to 20 mm, for example, and used as chopped strands.

[0060] like Figure 2 and Figure 3 As shown, the nozzle 8 has a pair of long wall portions 11, 11 and a pair of short wall portions 12, 12. The flat nozzle hole 6 is surrounded by these wall portions. The nozzle hole 6 has an inlet 6a for the molten glass 2 to flow in and an outlet 6b for the molten glass 2 to flow out. A notch portion 13 opening toward the outlet 6b side is provided on the pair of long wall portions 11, 11. Thus, the nozzle hole 6 is connected to the external space of the nozzle 8 through the notch portion 13.

[0061] The cooling pipe 9 cools the molten glass 2 by circulating cooling water 14 therein. The outer shape of the cooling pipe 9 is formed in a plate shape, and the plate surface is parallel to the long wall portion 11. Here, the cooling pipe 9 is provided integrally with the substrate 7, but it can also be provided at a position separated from the substrate 7. In addition, the cooling pipe 9 can also be formed in a circular tube shape.

[0062] The height position of the cooling pipe 9 can be adjusted according to the cooling condition of the molten glass 2. As an example, the cooling pipe 9 can be arranged at a position above the lower end of the nozzle 8 in a manner that the plate surface does not face the molten glass 2 drawn from the nozzle 8. On the other hand, the cooling pipe 9 can also be arranged across the upper and lower sides thereof with the lower end of the nozzle 8 as a reference in a manner that the plate surface faces the nozzle 8 and the molten glass 2 drawn from the nozzle 8. In addition, in the cooling of the molten glass 2, in addition to the cooling pipe 9, cooling fins cooled by air flow, etc. can also be used. In addition, the cooling pipe 9 is not a necessary structure and can be omitted.

[0063] A plurality of nozzle rows P are arranged in parallel at intervals on the substrate 7. Each nozzle row P has a plurality of nozzles 8. The plurality of nozzles 8 belonging to the same nozzle row P are arranged so that the nozzle holes 6 formed in the nozzles 8 are located on the same straight line.

[0064] The cooling pipe 9 is arranged between two adjacent nozzle rows P and P in a manner extending in parallel with the nozzle row P. Thus, the molten glass 2 in the nozzle hole 6 is cooled by the notch portion 13 facing the cooling pipe 9. Specifically, the molten glass 2 is rapidly cooled from a temperature of more than 1000°C by the cooling pipe 9. Here, the cooling pipe 9 also has a function of improving durability by cooling the extruder 4 (substrate 7) and the nozzle 8 to suppress the degradation of these components caused by heat.

[0065] like Figure 4 As shown in (a) and (b), the notch 13 provided in the long wall portion 11 of each nozzle 8 is in the shape of an isosceles trapezoid whose upper base is shorter than the lower base. As a result, the opening width of the notch 13 gradually increases from the inlet 6a side of the nozzle hole 6 toward the outlet 6b side. The depth of the notch 13 (the length in the direction of the axis 6x of the nozzle hole 6) is 0.1 mm to 2 mm. This is because, when the depth of the notch 13 exceeds 2 mm, in the cross section of the manufactured glass fiber 2f, the two ends in the longitudinal direction are too thin, and the glass fiber 2f is easily damaged.

[0066] The shape of the notch 13 is not limited to a trapezoid, and may be other shapes. For example, it may be a triangle, a semicircle, or a rectangle. However, even when these other shapes are adopted, the notch 13 preferably has an opening width that gradually expands from the inlet 6a side of the nozzle hole 6 toward the outlet 6b side.

[0067] like Figure 4 As shown, in the present embodiment, a single nozzle hole 6 is provided in one nozzle 8. The nozzle hole 6 is formed in a long hole shape. A pair of long wall portions 11, 11 are opposed to each other in the short diameter direction of the long hole-shaped nozzle hole 6, and a pair of short wall portions 12, 12 are opposed to each other in the long diameter direction. In addition, in the present embodiment, the thickness of the short wall portion 12 (the thickness along the long diameter direction of the nozzle hole 6) is greater than the thickness of the long wall portion 11 (the thickness along the short diameter direction of the nozzle hole 6). Here, the aspect ratio (ratio of the long diameter to the short diameter) of the nozzle hole 6 is 2 to 5. The inner circumferential surface of the nozzle hole 6, including the inner wall surface 11a of the long wall portion 11 and the inner wall surface 12a of the short wall portion 12, is made of platinum or a platinum alloy. In addition, the inner wall surface 11a of the long wall portion 11 is as shown in FIG. Figure 4 (c) shows a straight line shape, and the opposing inner wall surfaces 11a are parallel.

[0068] In addition, the boundary 15 between the long wall portion 11 and the short wall portion 12 is the inner wall surface relative to the Figure 4 At the point where the inclination in the horizontal direction of the paper surface in (c) changes from 0, the portion where the inclination in the horizontal direction of the paper surface is 0 is the long wall portion 11 , and the portion where the inclination is not 0 is the short wall portion 12 .

[0069] like Figure 4 (b) and Figure 5 As shown, for each of the pair of short wall portions 12, 12, an inclined portion 12aa inclined relative to the axis 6x of the nozzle hole 6 is formed in the end region T of the end portion located on the flow outlet 6b side. Specifically, the inclined portion 12aa is inclined from the center side of the nozzle hole 6 toward the outside (from the inside to the outside in the major diameter direction) as it moves from the flow inlet 6a side toward the flow outlet 6b side. As a result, the inclined portion 12aa of one short wall portion 12 located in the pair of short wall portions 12, 12 and the inclined portion 12aa located in the other short wall portion 12 are inclined in opposite directions to each other. The two inclined portions 12aa, 12aa are respectively composed of a single inclined surface (inclined plane). The inclined portion 12aa extends throughout the short diameter direction ( Figure 4 (b) and Figure 5 The short wall portion 12 is formed along the entire length of the short wall portion 12 (in the direction perpendicular to the paper surface). The angle θ1 at which the inclined portion 12aa is inclined relative to the line perpendicular to the axis 6x is not particularly limited, and is 55° in the present embodiment. In addition, if the inclined portion 12aa is inclined relative to the axis 6x of the nozzle hole 6, the inclined portion 12aa may also be a curved surface. In addition, the surface roughness of the inclined portion 12aa may also be rougher than the surface roughness of the inner wall surface 12a. In addition, the angle θ1 at which the inclined portion 12aa is inclined relative to the line perpendicular to the axis 6x is preferably greater than 10° and less than 80°.

[0070] The short wall portion 12 has a bottom wall surface 12b connected to the inclined portion 12aa. In detail, the bottom wall surface 12b is connected to the outer side of the long diameter direction of the nozzle hole 6 relative to the inclined portion 12aa. In the present embodiment, the bottom wall surface 12b is a flat surface orthogonal to the axis 6x. Here, the length of the inclined portion 12aa is set to L1, and the length of the bottom wall surface 12b is set to L2. In addition, "the length L1 of the inclined portion 12aa and the length L2 of the bottom wall surface 12b" are respectively the lengths on the cross section orthogonal to the short diameter direction of the nozzle hole 6.

[0071] Thus, the end region T in the present embodiment becomes larger than the case where there is no inclined portion 12aa. Specifically, in the present embodiment, the approximate area of ​​the end region T is the value obtained by multiplying the sum of the length L1 of the inclined portion 12aa and the length L2 of the bottom wall surface 12b by the circumference of the short wall portion 12, while the approximate area of ​​the end region in the case where there is no inclined portion 12aa as in the past is the value obtained by multiplying the sum of the length L2 of the bottom wall surface 12b and the length L3 of the imaginary bottom wall surface by the circumference of the short wall portion 12. The relationship between L1 and L3 is L1 = L3 / cos55° = 1.74×L3. That is, the approximate area of ​​the end region T in the present embodiment becomes larger than the approximate area of ​​the end region in the past where there is no inclined portion 12aa.

[0072] like Figure 6 As shown, the long wall portion 11 has a bottom wall surface 11b. In addition, the bottom wall surface 11b at the position where the notch portion 13 is provided in the long wall portion 11 is a position corresponding to the upper base of the isosceles trapezoid or the side connecting the upper base and the lower base. In the present embodiment, the bottom wall surface 11b is a flat surface (a flat surface orthogonal to the axis 6x at a position corresponding to the upper base of the isosceles trapezoid). Here, the length of the bottom wall surface 11b is set to L4. In addition, the "length of the bottom wall surface 11b" refers to the length on the cross section orthogonal to the major diameter direction. And, compared with the length L4, the sum of the above-mentioned length L1 and the length L2 is longer. As a result, the area of ​​the end region T of the short wall portion 12 becomes larger relative to the area of ​​the bottom wall surface 11b of the long wall portion 11, and the molten glass 2 is more easily stretched along the major diameter direction than along the minor diameter direction of the nozzle hole 6.

[0073] Hereinafter, the main functions and effects of the method for producing a deformed cross-section glass fiber using the above-mentioned nozzle 8 will be described.

[0074] In the above-mentioned nozzle 8, the end region T has the inclined portion 12aa inclined with respect to the axis 6x of the nozzle hole 6, so that the contact area between the end region T and the molten glass 2 is expanded compared with the case where the inclination is not provided. As a result, the ability of the short wall portion 12 to draw the molten glass 2 is improved, and with this, deformation of the molten glass 2 such that the surface area is reduced due to surface tension can be suppressed. As a result, it is possible to manufacture Figure 7 Here, the cross-sectional shape of the glass fiber 2f is formed into a shape close to an oval.

[0075] Here, the nozzle for the irregular cross-section glass fiber and the method for producing the irregular cross-section glass fiber according to the present invention are not limited to the structures and methods described in the above-mentioned embodiments. Figure 8 As shown, the long wall portion 11 may also have an inclined portion 11aa. In addition, the angle θ2 at which the inclined portion 11aa is inclined relative to the line orthogonal to the axis 6x is preferably 10° or more and 80° or less. In addition, by setting θ1>θ2, the ability of the inner wall surface 11a of the long wall portion 11 to stretch the molten glass 2 can be suppressed from becoming too large, and the flatness of the glass fiber can be suppressed from becoming small.

[0076] Furthermore, when the long wall portion 11 is provided with the inclined portion 11aa, the inclined portion 11aa is not provided at the center side of the long wall portion 11, and the inclined portions 11aa are provided only at the two end sides of the long wall portion 11, thereby preventing the ability of the long wall portion 11 to draw the molten glass 2 from becoming too large, and preventing the flatness of the glass fiber from becoming small. Fig. 9As shown, by providing the inclined portion 11aa on the long wall portion 11 other than the upper bottom of the isosceles trapezoidal notch portion 13 and not providing the inclined portion 11aa on the upper bottom of the notch portion 13, it is possible to suppress the flatness of the glass fiber from being reduced.

[0077] In addition, in the above-mentioned embodiment, the notch 13 is provided in each of the pair of long wall portions 11, 11, but the notch 13 is not necessarily provided, and the notch 13 may be removed. In addition, the nozzle hole 6 may be in an elliptical shape, a dumbbell shape, a diamond shape, a rectangular shape, a triple perfect circle shape, etc., in addition to the long hole shape.

Claims

1. A nozzle for special-shaped cross-section glass fiber, It is characterized in that A flat nozzle hole is provided, the nozzle hole having an inlet and an outlet for molten glass, The wall portion surrounding the nozzle hole includes a pair of short wall portions facing each other in the long diameter direction of the nozzle hole and a pair of long wall portions facing each other in the short diameter direction. The nozzle for the special-shaped cross-section glass fiber is used to manufacture the special-shaped cross-section glass fiber by using the molten glass flowing out from the nozzle hole. Among the pair of the short wall portions and the pair of the long wall portions, only for each of the pair of the short wall portions, an end region of the end of the short wall portion located on the outlet side has an inclined portion inclined relative to the axis of the nozzle hole and a bottom wall surface connected to the inclined portion, The inclined portion has an inclined surface that is inclined so as to be separated from a center side of a flat cross section of the nozzle hole as it moves from the inlet side toward the outlet side.

2. The nozzle for special-shaped cross-section glass fiber according to claim 1, It is characterized in that The long wall portion has a bottom wall surface at an end portion on the outlet side. Compared with the length of the bottom wall surface of the long wall portion in the cross section perpendicular to the major diameter direction, the sum of the length of the inclined portion in the cross section perpendicular to the minor diameter direction and the length of the bottom wall surface of the short wall portion in the cross section perpendicular to the minor diameter direction is longer.

3. The nozzle for special-shaped cross-section glass fiber according to claim 1 or 2, It is characterized in that The inclined portion is composed of a single inclined surface.

4. A method for manufacturing a special-shaped cross-section glass fiber, It is characterized in that The glass fiber is manufactured using a nozzle for a special-shaped cross-section, wherein the nozzle for the special-shaped cross-section glass fiber is provided with a flat nozzle hole, the nozzle hole has an inlet and an outlet for molten glass, and a wall portion surrounding the nozzle hole has a pair of short wall portions opposed in the long diameter direction of the nozzle hole and a pair of long wall portions opposed in the short diameter direction, The manufacturing method is used to manufacture special-shaped cross-section glass fibers by using molten glass flowing out of the nozzle hole. Among the pair of the short wall portions and the pair of the long wall portions, only for each of the pair of the short wall portions, an end region of the end of the short wall portion located on the outlet side has an inclined portion inclined relative to the axis of the nozzle hole and a bottom wall surface connected to the inclined portion, The inclined portion has an inclined surface that is inclined so as to be separated from a center side of a flat cross section of the nozzle hole as it moves from the inlet side toward the outlet side.