A bio-based water-based polyetheramine polymer and its preparation method and application
A bio-based polyetheramine polymer with a double cross-linked network structure addresses the poor adsorption of cottonseed protein flocculants, enhancing water treatment efficiency through improved charge neutralization and floc formation.
Patent Information
- Application Number
- CN202211455536.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-11-21
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2042-11-21
AI Technical Summary
Bio-based flocculants, such as cottonseed protein, suffer from poor net capture adsorption performance due to strong hydrogen bonding and insolubility, limiting their application in water treatment.
A bio-based water-based polyetheramine polymer is synthesized using cottonseed protein and condensed tannins, with modifications to reduce steric hindrance and enhance reactivity, forming a double cross-linked network structure for improved adsorption and flocculation.
The polymer exhibits enhanced adsorption capacity and flocculation performance, facilitating wider application in water treatment by neutralizing charges and promoting floc formation, with higher efficiency in pollutant removal.
Smart Images

Figure CN115850695B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of flocculants, and in particular to a bio-based water-based polyetheramine macromolecular polymer and a preparation method and application thereof. Background Art
[0002] At present, as people's demand for environmental protection is getting higher and higher, more and more environmentally friendly materials are being developed and applied to water treatment. Among them, bio-based flocculants are a kind of natural organic polymer flocculants, which can be divided into three categories according to their chemical composition, namely protein, cellulose, polysaccharide and other carbohydrate flocculants. Bio-based flocculants with plant protein or chitosan as the main raw materials are natural environmentally friendly flocculants, which can be modified and compounded, and then used for sewage treatment. Compared with traditional chemical flocculants, natural organic flocculants have the advantages of safety, stability, renewability, no "secondary pollution", and biodegradability. However, due to the strong hydrogen bonding within and between molecules, the molecular structure is in a compact crystalline state, insoluble in water and most organic solvents, which greatly limits its application.
[0003] Cottonseed protein is a high-protein product made from cottonseeds after being delinted and shelled, soaked in oil at low temperature, drained, and then removed from toxic substances (cottonpol). At present, the cottonseed protein production process requires detoxification treatment. The wet meal that has been detoxified by solvents is mostly dried by heating evaporation process to prepare finished protein. Patent application No. 200510124534.6 introduces a cottonseed protein production method: cottonseed protein extraction is completed in an extractor using a mixed solvent of 6# solvent and methanol in a ratio of 1:1.5; the wet meal is first extruded by an extruder and then dried by a disc dryer to obtain cottonseed finished protein. The production process is simple, with less loss, less energy consumption, and low cost. It can obtain high-quality cottonseed protein with a protein free cottonpol content of less than 400ppm and a protein solubility of more than 55%, and is easy to realize continuous industrial production; however, the cottonseed protein in the prior art still has the disadvantage of poor net capture adsorption performance, which limits its application range. Summary of the invention
[0004] In order to overcome the shortcomings of the prior art, the present invention provides a bio-based water-based polyetheramine high molecular polymer and a preparation method and application thereof. The polymer not only retains the inherent excellent properties of tannin and cottonseed protein such as non-toxicity, biocompatibility, and degradability, but each structural unit of the molecular chain has a positive charge, and the charge distribution is uniform, which can more effectively neutralize the excess negative charge carried by micro-flocculation, promote the formation and growth of flocs, and improve the structure of flocs, thereby improving the adsorption capacity for pollutants and the flocculation and sedimentation performance, and has a wider range of applications.
[0005] The first aspect of the present invention provides a bio-based water-based polyetheramine polymer, which is prepared from the following raw materials in parts by weight: 80-10 parts by weight of epichlorohydrin, 0.36-0.6 parts by weight of ethylene glycol, 0.7-1.4 parts by weight of boron trifluoride tetrahydrofuran complex, 30-45 parts by weight of tetrahydrofuran, 260-320 parts by weight of polyethylene polyamine, 50-80 parts by weight of cottonseed protein intermediate, and 150-300 parts by weight of methanol.
[0006] In the present invention, as a preferred embodiment, the bio-based water-based polyetheramine polymer is prepared from the following raw materials in parts by weight: 90 parts by weight of epichlorohydrin, 0.36-0.6 parts by weight of ethylene glycol, 0.7-1.4 parts by weight of boron trifluoride tetrahydrofuran complex, 30-45 parts by weight of tetrahydrofuran, 260-320 parts by weight of polyethylene polyamine, 50-80 parts by weight of cottonseed protein intermediate, and 150-300 parts by weight of methanol.
[0007] In the present invention, as a preferred embodiment, the bio-based water-based polyetheramine polymer is prepared from the following raw materials in parts by weight: 90 parts by weight of epichlorohydrin, 0.6 parts by weight of ethylene glycol, 1.4 parts by weight of boron trifluoride tetrahydrofuran complex, 45 parts by weight of tetrahydrofuran, 280 parts by weight of polyethylene polyamine, 70 parts by weight of cottonseed protein intermediate, and 300 parts by weight of methanol.
[0008] In the present invention, as a preferred embodiment, the cottonseed protein intermediate is prepared from the following raw materials in parts by weight: 8-15 parts by weight of cottonseed protein, 2-4 parts by weight of 1,2,3-propanetriol triglycidyl ether, 5-10 parts by weight of depolymerized condensed tannin, and 45-55 parts by weight of water.
[0009] In the present invention, as a preferred embodiment, the depolymerized condensed tannin is prepared from the following raw materials in parts by weight: 5-10 parts by weight of urea, 2-4 parts by weight of 2-mercaptoethanol, 2-4 parts by weight of NaOH, 30-50 parts by weight of condensed tannin, and 90 parts by weight of water.
[0010] The second aspect of the present invention also provides a method for preparing a bio-based water-based polyetheramine polymer, comprising the following steps: adding a formula amount of tetrahydrofuran solvent to a flask equipped with a thermometer, a stirrer, a water separator and a reflux condenser, then adding a formula amount of ethylene glycol and a formula amount of boron trifluoride tetrahydrofuran complex, reducing the temperature to below 10°C, slowly dripping a formula amount of epichlorohydrin diluted with tetrahydrofuran, the dripping time is 6-8h, reacting for 12h after the dripping is completed to obtain polyepichlorohydrin, then adding a formula amount of cottonseed protein intermediate, polyethylene polyamine and methanol, first stirring and reacting at 50°C for 2-3h, then heating to 90°C, reacting for 3-5h, and cooling at room temperature to obtain the target product.
[0011] In the present invention, as a preferred embodiment, the preparation method of the cottonseed protein intermediate includes the step of modifying the cottonseed protein with condensed tannin: mixing a formulated amount of cottonseed protein, depolymerized condensed tannin, 1,2,3-propanetriol triglycidyl ether and water, and stirring at room temperature for 6-8 hours to obtain the cottonseed protein intermediate.
[0012] In the present invention, as a preferred embodiment, it also includes a depolymerization step of condensed tannins: into a flask equipped with a thermometer, a stirrer, and a water separator, urea, 2-mercaptoethanol, NaOH, condensed tannins and water in a formulated amount are added in sequence, stirred, and a water bath is heated to 65° C. to react for 2-4 hours, and the solution is continued to be stirred at room temperature for 15 hours to obtain the depolymerized condensed tannins.
[0013] In the present invention, as a preferred embodiment, it also includes a pretreatment step: grinding the cottonseed meal after oil extraction into powder with a crusher, passing through a 200-mesh screen, washing with water for multiple times, preparing a cottonseed meal solution with a concentration of 40%, and placing it in a water bath at 80-85°C for preheating for 30 minutes. During the treatment process, the cottonseed meal solution is continuously stirred. After the preheating is completed, the cottonseed meal solution is cooled to room temperature and centrifuged; the cottonseed meal powder after centrifugation is placed in an oven and dried at 60°C to constant weight; the dried cottonseed meal powder is ground again and passed through a 200-mesh screen to obtain the cottonseed protein.
[0014] The third aspect of the present invention also provides an application of a bio-based water-based polyetheramine polymer as a flocculant.
[0015] Compared with the prior art, the beneficial effect of the present invention is that the bio-based water-based polyetheramine high molecular polymer of the present invention can be used as a flocculant. On the one hand, it retains the inherent excellent properties of condensed tannins and cottonseed proteins, such as non-toxicity, biocompatibility, degradability, and macromolecular adsorption. At the same time, due to the large relative molecular weight of tannins, there is a certain amount of steric hindrance, and the reactivity with other molecules is poor. The tannins are treated with green and environmentally friendly urea and 2-mercaptoethanol to reduce the steric hindrance of the condensed tannins and increase their reactivity. On the other hand, polyepichlorohydrin with a large relative molecular weight is synthesized as a cross-linking agent, which not only undergoes a cross-linking condensation reaction with polyethylene polyamines, but also utilizes the catechol groups on the condensed tannins to react with the NH2 groups on the cottonseed protein chains and polyethylene polyamines to form a double cross-linked network structure to enhance the net-catching and sweeping effect. In this way, the polymer molecular chain is longer and the degree of branching is higher, forming a more developed network structure, which has a stronger bridging effect and electrical neutralization effect on oil droplets, is easier to contact emulsified oil droplets, and replaces some original natural surfactants on the oil-water surface, extruding to promote the aggregation of oil droplets and promote floating or sinking. Furthermore, the cottonseed protein intermediate of the present invention utilizes green and environmentally friendly urea and 2-mercaptoethanol to treat condensed tannins, thereby reducing the steric hindrance of the condensed tannins and increasing their reaction activity, and the depolymerized condensed tannin solution is evenly dispersed in the cottonseed protein to increase the network structure, thereby enhancing the net capture adsorption performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] Figure 1 This is a schematic diagram showing the effect of different addition amounts of the bio-based waterborne polyetheramine polymer on the light transmittance of the kaolin solution in Example 3;
[0017] Figure 2 This is a comparison chart of the oil removal effect of the bio-based water-based polyetheramine polymer of Example 3 and a market comparison sample on polymer-containing wastewater;
[0018] Figure 3 This is a comparison chart of the flocculation effect of the bio-based water-based polyetheramine polymer of Examples 1-4 on kaolin suspension. DETAILED DESCRIPTION
[0019] The invention is further described below in conjunction with the accompanying drawings and specific implementation methods. It should be noted that, under the premise of no conflict, the various embodiments or technical features described below can be arbitrarily combined to form a new embodiment. Unless otherwise specified, the materials and equipment used in this embodiment can be purchased from the market.
[0020] A bio-based water-based polyetheramine high molecular polymer is prepared from the following raw materials in parts by weight: 80-10 parts by weight of epichlorohydrin, 0.36-0.6 parts by weight of ethylene glycol, 0.7-1.4 parts by weight of boron trifluoride tetrahydrofuran complex, 30-45 parts by weight of tetrahydrofuran, 260-320 parts by weight of polyethylene polyamine, 50-80 parts by weight of cottonseed protein intermediate, and 150-300 parts by weight of methanol.
[0021] As a preferred embodiment, the bio-based water-based polyetheramine polymer is prepared from the following raw materials in parts by weight: 90 parts by weight of epichlorohydrin, 0.36-0.6 parts by weight of ethylene glycol, 0.7-1.4 parts by weight of boron trifluoride tetrahydrofuran complex, 30-45 parts by weight of tetrahydrofuran, 260-320 parts by weight of polyethylene polyamine, 50-80 parts by weight of cottonseed protein intermediate, and 150-300 parts by weight of methanol.
[0022] As a preferred embodiment, the bio-based water-based polyetheramine polymer is prepared from the following raw materials in parts by weight: 90 parts by weight of epichlorohydrin, 0.6 parts by weight of ethylene glycol, 1.4 parts by weight of boron trifluoride tetrahydrofuran complex, 45 parts by weight of tetrahydrofuran, 280 parts by weight of polyethylene polyamine, 70 parts by weight of cottonseed protein intermediate, and 300 parts by weight of methanol.
[0023] As a preferred embodiment, the cottonseed protein intermediate is prepared from the following raw materials in parts by weight: 8-15 parts by weight of cottonseed protein, 2-4 parts by weight of 1,2,3-propanetriol triglycidyl ether, 5-10 parts by weight of depolymerized condensed tannin, and 45-55 parts by weight of water.
[0024] As a preferred embodiment, the depolymerized condensed tannin is prepared from the following raw materials in parts by weight: 5-10 parts by weight of urea, 2-4 parts by weight of 2-mercaptoethanol, 2-4 parts by weight of NaOH, 30-50 parts by weight of condensed tannin, and 90 parts by weight of water.
[0025] The second aspect of the present invention also provides a method for preparing a bio-based water-based polyetheramine polymer, comprising the following steps: adding a formula amount of tetrahydrofuran solvent to a flask equipped with a thermometer, a stirrer, a water separator and a reflux condenser, then adding a formula amount of ethylene glycol and a formula amount of boron trifluoride tetrahydrofuran complex, reducing the temperature to below 10°C, slowly dripping a formula amount of epichlorohydrin diluted with tetrahydrofuran, the dripping time is 6-8h, reacting for 12h after the dripping is completed to obtain polyepichlorohydrin, then adding a formula amount of cottonseed protein intermediate, polyethylene polyamine and methanol, first stirring and reacting at 50°C for 2-3h, then heating to 90°C, reacting for 3-5h, and cooling at room temperature to obtain the target product.
[0026] As a preferred embodiment, the preparation method of the cottonseed protein intermediate includes the step of modifying the cottonseed protein with condensed tannin: mixing a formulated amount of cottonseed protein, depolymerized condensed tannin, 1,2,3-propanetriol triglycidyl ether and water, and stirring at room temperature for 6-8 hours to obtain the cottonseed protein intermediate.
[0027] As a preferred embodiment, the method further includes a depolymerization step of condensed tannins: adding formulated amounts of urea, 2-mercaptoethanol, NaOH, condensed tannins and water to a flask equipped with a thermometer, a stirrer and a water separator, stirring, heating the water bath to 65° C. to react for 2-4 hours, and continuing to stir the solution at room temperature for 15 hours to obtain the depolymerized condensed tannins.
[0028] As a preferred embodiment, the method further comprises a pretreatment step: grinding the cottonseed meal after oil extraction into powder with a pulverizer, passing the powder through a 200-mesh screen, washing the powder with water for multiple times, preparing a cottonseed meal solution with a concentration of 40%, placing the powder in a water bath at 80-85° C. for preheating for 30 minutes, stirring the cottonseed meal solution continuously during the treatment process, cooling the cottonseed meal solution to room temperature after the preheating, and centrifuging; placing the cottonseed meal powder after centrifugation in an oven, and drying the powder at 60° C. to a constant weight; and grinding the dried cottonseed meal powder again through a 200-mesh screen to obtain the cottonseed protein.
[0029] The third aspect of the present invention also provides an application of a bio-based water-based polyetheramine polymer as a flocculant.
[0030] The embodiments described below with reference to the accompanying drawings are exemplary and are only used to explain the present application, but should not be understood as limiting the present application.
[0031] Embodiment 1:
[0032] This embodiment provides a method for preparing a bio-based water-based polyetheramine polymer, comprising:
[0033] 1) Pretreatment of cottonseed meal: Grind the cottonseed meal after oil extraction into powder with a pulverizer, pass through a 200-mesh screen, wash three times with water, prepare a 40% cottonseed meal solution, put it in a water bath at 80-85°C for preheating for 30 minutes, stir the cottonseed meal solution continuously during the treatment process, and after preheating, cool the cottonseed meal solution to room temperature and centrifuge. Place the centrifuged cottonseed meal powder in an oven and dry it to constant weight at 60°C. Grind the dried cottonseed meal powder again and pass through a 200-mesh screen as the intermediate product base material.
[0034] 2) Depolymerization of condensed tannins: Into a flask equipped with a thermometer, a stirrer and a water separator, 5 parts by weight of urea, 3 parts by weight of 2-mercaptoethanol, 2 parts by weight of NaOH, 30 parts by weight of condensed tannins and 90 parts by weight of water were added in sequence, and stirred. The temperature of the water bath was raised to 65° C. for reaction for 4 hours, and the solution was continued to be stirred at room temperature for 15 hours to obtain depolymerized condensed tannins.
[0035] 3) Condensed tannin modified cottonseed protein: 8 parts by weight of pretreated cottonseed protein, 5 parts by weight of depolymerized condensed tannin, 3 parts by weight of 1,2,3-propanetriol triglycidyl ether, and 50 parts by weight of water were weighed, and stirred at room temperature for 6-8 hours to obtain a cottonseed protein intermediate.
[0036] 4) In a flask equipped with a thermometer, a stirrer, a water separator and a reflux condenser, 45 parts by weight of tetrahydrofuran solvent are first added, followed by 0.36 parts by weight of ethylene glycol and 0.7 parts by weight of boron trifluoride tetrahydrofuran complex, the temperature is reduced to below 10°C, 90 parts by weight of epichlorohydrin diluted with 45 parts by weight of tetrahydrofuran is slowly added dropwise, the addition time is 6 hours, after the addition is completed, the reaction is carried out for 12 hours to obtain polyepichlorohydrin, and then 50 parts by weight of cottonseed protein intermediate, 280 parts by weight of polyethylene polyamine, and 150 parts by weight of methanol are added, the reaction is first stirred at 50°C for 3 hours, then heated to 90°C, reacted for 3 hours, cooled at room temperature to obtain the target product, and diluted with water according to the required solid content.
[0037] Example 2
[0038] This embodiment provides a method for preparing a bio-based water-based polyetheramine polymer, comprising:
[0039] 1) Pretreatment of cottonseed meal: Grind the cottonseed meal after oil extraction into powder with a pulverizer, pass through a 200-mesh screen, wash three times with water, prepare a 40% cottonseed meal solution, put it in a water bath at 80-85°C for preheating for 30 minutes, stir the cottonseed meal solution continuously during the treatment process, and after preheating, cool the cottonseed meal solution to room temperature and centrifuge. Place the centrifuged cottonseed meal powder in an oven and dry it to constant weight at 60°C. Grind the dried cottonseed meal powder again and pass through a 200-mesh screen as the intermediate product base material.
[0040] 2) Depolymerization of condensed tannins: Into a flask equipped with a thermometer, a stirrer and a water separator, 10 parts by weight of urea, 3 parts by weight of 2-mercaptoethanol, 4 parts by weight of NaOH, 50 parts by weight of condensed tannins and 90 parts by weight of water were added in sequence, and the mixture was stirred. The temperature of the water bath was raised to 65° C. and the reaction was carried out for 4 hours. The solution was continued to be stirred at room temperature for 15 hours to obtain depolymerized condensed tannins.
[0041] 3) Condensed tannin modified cottonseed protein: 15 parts by weight of pretreated cottonseed protein, 10 parts by weight of depolymerized condensed tannin, 3 parts by weight of 1,2,3-propanetriol triglycidyl ether, and 50 parts by weight of water were weighed and stirred at room temperature for 8 hours to obtain a cottonseed protein intermediate.
[0042] 4) In a flask equipped with a thermometer, a stirrer, a water separator and a reflux condenser, 40 parts by weight of tetrahydrofuran solvent are first added, and then 0.5 parts by weight of ethylene glycol and 1.2 parts by weight of boron trifluoride tetrahydrofuran complex are added, the temperature is reduced to below 10°C, 90 parts by weight of epichlorohydrin diluted with 40 parts by weight of tetrahydrofuran are slowly added dropwise, the addition time is 6 hours, and the reaction is completed for 12 hours to obtain polyepichlorohydrin, and then 80 parts by weight of cottonseed protein intermediate, 320 parts by weight of polyethylene polyamine, and 280 parts by weight of methanol are added, and the reaction is stirred at 50°C for 3 hours, and then heated to 90°C, reacted for 5 hours, and cooled at room temperature to obtain the target product, and diluted with water according to the required solid content.
[0043] Example 3
[0044] This embodiment provides a method for preparing a bio-based water-based polyetheramine polymer, comprising:
[0045] 1) Pretreatment of cottonseed meal: Grind the cottonseed meal after oil extraction into powder with a pulverizer, pass through a 200-mesh screen, wash three times with water, prepare a 40% cottonseed meal solution, put it in a water bath at 80-85°C for preheating for 30 minutes, stir the cottonseed meal solution continuously during the treatment process, and after preheating, cool the cottonseed meal solution to room temperature and centrifuge. Place the centrifuged cottonseed meal powder in an oven and dry it to constant weight at 60°C. Grind the dried cottonseed meal powder again and pass through a 200-mesh screen as the intermediate product base material.
[0046] 2) Depolymerization of condensed tannins: Into a flask equipped with a thermometer, a stirrer and a water separator, 8 parts by weight of urea, 3 parts by weight of 2-mercaptoethanol, 4 parts by weight of NaOH, 40 parts by weight of condensed tannins and 90 parts by weight of water were added in sequence, and stirred. The temperature of the water bath was raised to 65° C. for reaction for 3 h, and the solution was continued to be stirred at room temperature for 15 h to obtain depolymerized condensed tannins.
[0047] 3) Condensed tannin modified cottonseed protein: 10 parts by weight of pretreated cottonseed protein, 8 parts by weight of depolymerized condensed tannin, 3 parts by weight of 1,2,3-propanetriol triglycidyl ether, and 50 parts by weight of water were weighed and stirred at room temperature for 8 hours to obtain a cottonseed protein intermediate.
[0048] 4) In a flask equipped with a thermometer, a stirrer, a water separator and a reflux condenser, 45 parts by weight of tetrahydrofuran solvent are first added, followed by 0.6 parts by weight of ethylene glycol and 1.4 parts by weight of boron trifluoride tetrahydrofuran complex, the temperature is reduced to below 10°C, 45 parts by weight of epichlorohydrin diluted with tetrahydrofuran is slowly added dropwise for 7 hours, and the reaction is continued for 12 hours after the addition is completed to obtain polyepichlorohydrin, and then 70 parts by weight of cottonseed protein intermediate, 280 parts by weight of polyethylene polyamine and 300 parts by weight of methanol are added, the reaction is first stirred at 50°C for 3 hours, then heated to 90°C for 5 hours, cooled at room temperature to obtain the target product, and diluted with water according to the required solid content.
[0049] Example 4
[0050] This embodiment provides a method for preparing a bio-based water-based polyetheramine polymer, comprising:
[0051] 1) Pretreatment of cottonseed meal: Grind the cottonseed meal after oil extraction into powder with a pulverizer, pass through a 200-mesh screen, wash three times with water, prepare a 40% cottonseed meal solution and put it into a water bath at 80-85°C for preheating for 30 minutes. During the treatment, the cottonseed meal solution is continuously stirred. After the preheating is completed, the cottonseed meal solution is cooled to room temperature and centrifuged. The centrifuged cottonseed meal powder is placed in an oven and dried at 60°C to constant weight. The dried cottonseed meal powder is ground again and passed through a 200-mesh screen as the intermediate product base material.
[0052] 2) Depolymerization of condensed tannins: Into a flask equipped with a thermometer, a stirrer and a water separator, 6 parts by weight of urea, 3 parts by weight of 2-mercaptoethanol, 3 parts by weight of NaOH, 45 parts by weight of condensed tannins and 90 parts by weight of water were added in sequence, and stirred. The temperature of the water bath was raised to 65° C. for reaction for 2 h, and the solution was continued to be stirred at room temperature for 15 h to obtain depolymerized condensed tannins.
[0053] 3) Condensed tannin modified cottonseed protein: Weigh 12 parts by weight of pretreated cottonseed protein, 8 parts by weight of depolymerized condensed tannin, 3 parts by weight of 1,2,3-propanetriol triglycidyl ether, and 50 parts by weight of water, and stir at room temperature for 8 hours to obtain a cottonseed protein intermediate.
[0054] 4) In a flask equipped with a thermometer, a stirrer, a water separator and a reflux condenser, 30 parts by weight of tetrahydrofuran solvent are first added, followed by 0.4 parts by weight of ethylene glycol and 1.0 parts by weight of boron trifluoride tetrahydrofuran complex, the temperature is reduced to below 10°C, 30 parts by weight of epichlorohydrin diluted with tetrahydrofuran is slowly added dropwise for 8 hours, and the reaction is completed for 12 hours to obtain polyepichlorohydrin, followed by 60 parts by weight of cottonseed protein intermediate, 260 parts by weight of polyethylene polyamine and 200 parts by weight of methanol, the reaction is first stirred at 50°C for 2 hours, then heated to 90°C for 3 hours, cooled at room temperature to obtain the target product, and diluted with water according to the required solid content.
[0055] In summary, the bio-based water-based polyetheramine high molecular polymer prepared by using the cottonseed protein intermediate of the present invention as a raw material can be used as a flocculant. On the one hand, it retains the inherent excellent properties of condensed tannins and cottonseed proteins, such as non-toxicity, biocompatibility, degradability, and macromolecular adsorption. At the same time, due to the large relative molecular weight of tannins, there is a certain amount of steric hindrance, and the reactivity with other molecules is poor. The tannins are treated with green and environmentally friendly urea and 2-mercaptoethanol to reduce the steric hindrance of the condensed tannins and increase their reactivity. On the other hand, polyepichlorohydrin with a large relative molecular weight is synthesized as a cross-linking agent, which not only undergoes a cross-linking condensation reaction with polyethylene polyamines, but also utilizes the catechol groups on the condensed tannins to react with the NH2 groups on the cottonseed protein chains and polyethylene polyamines to form a double cross-linked network structure to enhance the net-catching and sweeping effect. In this way, the polymer molecular chain is longer and the degree of branching is higher, forming a more developed network structure, which has a stronger bridging effect and electrical neutralization effect on oil droplets, is easier to contact emulsified oil droplets, and replaces some original natural surfactants on the oil-water surface, extruding to promote the aggregation of oil droplets and promote floating or sinking.
[0056] Performance Testing:
[0057] 1. Prepare the high molecular polymer of Example 3 into a dilution with a solid content of 20%. Slowly add a certain amount of flocculant mother solution to the 1g / L kaolin suspension under the continuous stirring of the cantilever stirrer, and start timing. First, stir the solution at a high speed of 200r / min for a certain period of time, then reduce the speed to 100r / min and stir for 5 minutes. After the stirring is completed, turn off the stirrer, let the solution stand for 5 minutes, and use a rubber-tipped dropper to absorb a certain amount of clear liquid 1 cm below the liquid surface. Use an ultraviolet UV-4802 spectrophotometer to measure the light transmittance (T%) of the solution at a wavelength of 550nm. The effect of polymer dosage on the flocculation effect was investigated, and the results are shown in Figure 1 shown.
[0058] Depend on Figure 1It can be seen that before the addition amount of the high molecular polymer in Example 3 is 20 mg / L, the transmittance (T%) is positively correlated with the addition amount. When the amount added is small, the positive charge generated by the self-made polymer molecules is not enough to neutralize the negative charge carried by the kaolin particles, and the charge neutralization effect is weak. Most of the particles rely on the net sweeping and adsorption bridging mechanism to form flocs and be removed. However, with the continuous addition of self-made polymer molecules, the surface of the particles will be wrapped by them, resulting in increased steric hindrance and "colloid protection". The self-made polymer molecules cannot play their due role, and the particles cannot be removed in large quantities, so the solution transmittance T% will be greatly reduced. Based on the above description, for the kaolin solution, the optimal addition amount of the polymer is 20 mg / L.
[0059] 2. To compare the difference between the self-made polymer and the commercially available comparative sample in the deoiling effect on the polymer-containing wastewater, the final treatment effect was compared with the deoiling rate of the polymer-containing wastewater after adding the high molecular polymer of Example 3 at a temperature of 60°C and other conditions remained unchanged. Figure 2 shown.
[0060] Depend on Figure 2 It can be seen that after treating the polymer-containing wastewater with the addition of the polymer of Example 3, the oil removal rate first increases and then decreases with the increase of the addition amount, and the optimal addition amount is 15 mg / L, and the removal rate reaches 86.2%. In contrast, the market comparison sample can only be further improved when the addition amount is increased, and the maximum removal rate can only reach 58.1%, and the addition amount is 25 mg / L, which is more than half of the polymer of Example 3. It can be determined that under low dosage, the polymer of Example 3 can achieve better results than the market comparison sample due to its high branching degree, molecular chain length and other aspects of the developed double network structure and high molecular weight optimization, and has better economic efficiency.
[0061] 3. Under certain conditions (room temperature), take equal portions of 100 mL of kaolin suspension (1 g / L), take 0.5 mg, 1.0 mg, 1.5 mg, 2.0 mg, 2.5 mg, and 3.0 mg of each homemade polymer (such as Example 1, Example 2, Example 3, and Example 4) in a beaker to treat the kaolin suspension, pH 7-8, stir quickly at 200 rad·min-1 for 1 min, then stir slowly at 100 rad·min-1 for 5 min, stop stirring, let it settle for a while, and measure the residual turbidity of the sample. The effects of different contents of different homemade polymers in kaolin suspension on flocculation performance were investigated, and the index for evaluating flocculation performance was the flocculation rate. The calculation formula for the flocculation rate is as follows:
[0062]
[0063] Where:
[0064] E% is the flocculation rate;
[0065] N0 is the turbidity of kaolin suspension before adding the reagent;
[0066] N1 is the turbidity of the high-temperature suspension after adding the agent.
[0067] Depend on Figure 3 It can be seen that with the increase of dosage, the flocculation effect of the four homemade polymers on kaolin suspension also increases; when the optimal dosage is 15 mg / L, the flocculation rate of the homemade polymer in Example 3 reaches 95.3%, which is higher than other homemade polymers of the same amount, and also higher than the highest flocculation rate of other homemade polymers at different dosages. Because in the homemade polymer structure, not only the excellent properties such as macromolecular adsorption inherent in condensed tannins and cottonseed protein are retained, but also the double cross-linked network structure formed by the functional groups on its molecular structure and polyamines, the grafted positive charge is also more, the homemade polymer has a strong ability to neutralize electricity with the colloid particles, which is more conducive to the capture of bridged suspended particles.
[0068] The above-mentioned embodiments are only preferred embodiments of the present invention and cannot be used to limit the scope of protection of the present invention. Any non-substantial changes and substitutions made by technicians in this field on the basis of the present invention shall fall within the scope of protection required by the present invention.
Claims
1. A bio-based water-based polyetheramine polymer, characterized in that: The invention is prepared from the following raw materials in parts by weight: 90 parts by weight of epichlorohydrin, 0.36-0.6 parts by weight of ethylene glycol, 0.7-1.4 parts by weight of boron trifluoride tetrahydrofuran complex, 30-45 parts by weight of tetrahydrofuran, 260-320 parts by weight of polyethylene polyamine, 50-80 parts by weight of cottonseed protein intermediate, and 150-300 parts by weight of methanol; The cottonseed protein intermediate is prepared from the following raw materials in parts by weight: 8-15 parts by weight of cottonseed protein, 2-4 parts by weight of 1,2,3-propanetriol triglycidyl ether, 5-10 parts by weight of depolymerized condensed tannin, and 45-55 parts by weight of water. The preparation method of the cottonseed protein intermediate includes the steps of modifying the cottonseed protein with condensed tannin: mixing a formula amount of cottonseed protein, depolymerized condensed tannin, 1,2,3-propanetriol triglycidyl ether and water, and stirring at room temperature for 6-8 hours to obtain the cottonseed protein intermediate; The depolymerized condensed tannin is prepared from the following raw materials in parts by weight: 5-10 parts by weight of urea, 2-4 parts by weight of 2-mercaptoethanol, 2-4 parts by weight of NaOH, 30-50 parts by weight of condensed tannin, and 90 parts by weight of water; the depolymerization steps of the condensed tannin are as follows: into a flask equipped with a thermometer, a stirrer, and a water separator, urea, 2-mercaptoethanol, NaOH, condensed tannin and water in a prescribed amount are added in sequence, stirred, the water bath is heated to 65° C. to react for 2-4 hours, and the solution is continuously stirred at room temperature for 15 hours to obtain the depolymerized condensed tannin.
2. The bio-based waterborne polyetheramine polymer according to claim 1, characterized in that: The bio-based water-based polyetheramine polymer is prepared from the following raw materials in parts by weight: 90 parts by weight of epichlorohydrin, 0.6 parts by weight of ethylene glycol, 1.4 parts by weight of boron trifluoride tetrahydrofuran complex, 45 parts by weight of tetrahydrofuran, 280 parts by weight of polyethylene polyamine, 70 parts by weight of cottonseed protein intermediate, and 300 parts by weight of methanol.
3. A method for preparing the bio-based waterborne polyetheramine polymer according to any one of claims 1 to 2, characterized in that: The following steps are involved: Add a formulated amount of tetrahydrofuran solvent to a flask equipped with a thermometer, a stirrer, a water separator and a reflux condenser, then add a formulated amount of ethylene glycol and a formulated amount of boron trifluoride tetrahydrofuran complex, reduce the temperature to below 10°C, slowly drop a formulated amount of epichlorohydrin diluted with tetrahydrofuran, the dropwise addition time is 6-8 hours, react for 12 hours after the dropwise addition is completed to obtain polyepichlorohydrin, then add a formulated amount of cottonseed protein intermediate, polyethylene polyamine and methanol, first stir and react at 50°C for 2-3 hours, then heat to 90°C, react for 3-5 hours, and cool to room temperature to obtain the target product.
4. The method for preparing the bio-based waterborne polyetheramine polymer according to claim 3, characterized in that: The method also includes a pretreatment step: grinding the cottonseed meal after oil extraction into powder with a crusher, passing through a 200-mesh screen, washing with water for multiple times, preparing a cottonseed meal solution with a concentration of 40%, placing it in a water bath at 80-85°C for preheating for 30 minutes, stirring the cottonseed meal solution continuously during the treatment process, cooling the cottonseed meal solution to room temperature after the preheating is completed, and centrifuging; placing the cottonseed meal powder after centrifugation in an oven, and drying it at 60°C to constant weight; and grinding the dried cottonseed meal powder again and passing it through a 200-mesh screen to obtain the cottonseed protein.
5. An application of the bio-based waterborne polyetheramine polymer as claimed in any one of claims 1 to 2, characterized in that: It acts as a flocculant.