A method for controlling the warpage of strip steel in a continuous evacuation strong water mist cooling system

By constructing a discrete model of the strip steel and optimizing the nozzle opening, the problem of uneven strip steel warp distribution was solved, achieving uniform control of warp and improving product quality and production efficiency.

CN115874040BActive Publication Date: 2024-11-26BAOSTEEL ZHANJIANG IRON & STEEL CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202211090126.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-09-07
Publication Date
2024-11-26
Estimated Expiration
2042-09-07

Smart Images

  • Figure CN115874040B_ABST
    Figure CN115874040B_ABST
Patent Text Reader

Abstract

The present invention discloses a strip warping control method for a continuous annealing strong water mist cooling system, the steps of which include constructing a discrete model of the strip under the action of a single spray beam, collecting equipment process parameters and on-site feedback data of the water mist cooling section, calculating the number of effective nozzles corresponding to the strip, calculating the absolute difference in warping of each unit of the strip, calculating the distribution value of the opening adjustment amount of the α and β sides of the strip, the nozzle opening values ​​on both sides of the α and β sides of each row of spray beams, re-collecting the warping value corresponding to a single unit of the strip, and judging whether the warping of the strip meets the standard. The method of the present invention aims at uniform lateral distribution of the warping of the strip, designs a nozzle opening optimization adjustment idea suitable for the water mist cooling process of the continuous annealing unit, and greatly improves the uniformity control effect of the warping of the strip in the water mist cooling section; the method of the present invention is applied to the water mist cooling equipment of the rapid cooling section of the continuous annealing unit, which can improve the quality of the finished strip products and bring economic benefits to the enterprise.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of continuous annealing, and in particular relates to a method for controlling the warpage of a strip steel in a continuous annealing strong water mist cooling system. Background Art

[0002] The strong water mist cooling process is the main method for continuous annealing of strip steel in the rapid cooling section. The strong water mist cooling process can meet the cooling rate requirements of ultra-high strength steel. The distribution of strip temperature during the cooling process not only affects the plate shape but also affects the uniformity of product performance. As one of the methods for expressing the plate shape, the warpage of the strip is an important evaluation criterion for measuring the quality of the strip. When controlling the warpage on the basis of ensuring the temperature of the strip, it is necessary to utilize the change in internal stress when the strip steel drops from high temperature to low temperature. By controlling the change in strip temperature through the opening of the nozzle, the redistribution of internal stress of the strip steel can be controlled, which can effectively reduce the warpage of the strip steel and ensure that the lateral distribution of temperature will not cause the uniformity of the performance distribution of the strip steel.

[0003] The control of the temperature and shape of the water mist cooling plate is mainly completed by the nozzle. The position of the spray beam, the number of nozzles, and the opening of the nozzles are used to control the distribution of the water flow, thereby adjusting the temperature and shape of the plate. In order to ensure the uniformity of the strip temperature, the temperature change should be considered when adjusting the strip warpage. The change in the difference in the opening on both sides of the strip should not cause the change in the total opening of the strip, otherwise the strip temperature will have the defect of lateral unevenness, which will affect the uniformity of the strip performance distribution and even cause other strip defects. Summary of the invention

[0004] The object of the present invention is to provide a method for controlling the warping of the strip in a continuous annealing strong water mist cooling system, which can accurately control the uniform distribution of the lateral warping of the annealed strip in the water mist cooling section and reduce the strip shape defects caused by the warping distribution.

[0005] In order to achieve the above technical objectives, the present invention adopts the following technical solution: a method for accurately controlling the temperature of a continuous retreat strong water mist cooling system, characterized in that it includes the following steps:

[0006] (A) Construct a discrete model of the strip under the action of a double-sided spray beam, determine the number of nozzles acting on the strip, divide the strip into corresponding units according to the location of the nozzles, and adjust the temperature of the corresponding unit strip by the nozzles on both sides of the strip, thereby adjusting the strip warpage caused by temperature, such as Figure 1 ;

[0007] (B) Collect the main equipment process parameters and on-site feedback data of the water mist cooling section, including: the number of spray beams M, the number of nozzles in each row of spray beams K, and the maximum nozzle opening U max , the opening U of each nozzle in each spray beam i,j, the distance d between adjacent nozzles, the strip width B, the warpage value λ corresponding to a single strip unit j ;

[0008] (C) Calculate the effective nozzle number N corresponding to the strip, integrate the warpage value corresponding to each unit of the strip, and obtain the absolute difference △λ of the warpage of each unit of the outlet strip under the current process j :

[0009]

[0010] (D) Taking the adjustment of the last row of spray beams as the initial adjustment state, calculate the opening adjustment amount △U′ that each pair of nozzles in the Mth row of spray beams should make under the current warpage difference M,j , where λ x is the current △λ j The maximum value of the corresponding warpage range, U x is the current △λ j The corresponding opening adjustment amount is as follows:

[0011]

[0012] (E) According to the actual situation on site, the convexity to the α side of the strip is set as the positive warping value, and the convexity to the β side of the strip is set as the negative warping value, and the distribution value of the opening adjustment amount on the α and β sides of the strip is calculated:

[0013]

[0014] (F) Calculate the opening value U′ of the nozzles on the α and β sides of the M-th row of spray beams α,M,j , U′ β,M,j :

[0015]

[0016] (G) Determine 0≤U α,M,j +△U′ α,M,j ≤△U max , 0≤U β,M,j +△U′ β,M,j ≤△U max Is it true? If it is true, go to step (K); if not, go to step (H);

[0017] (H) Calculate the opening data that is not satisfied by the Mth row of spray beams to obtain the opening adjustment amount △U′ that the nozzles on the α and β sides of the M-1th row of spray beams should make. α,M,j , △U′ β,M,j :

[0018]

[0019] (I) Calculate the opening value U′ of each nozzle in the M-1th row of spray beamsα,M-1,j , U′ β,M-1,j :

[0020]

[0021] (J) Judge 0≤U α,M-1,j +△U′ α,M-1,j ≤△U max , 0≤U β,M-1,j +△U′ β,M-1,j ≤△U max Is it true? If it is true, go to step (K). If it is not true, set M = M-1 and go to step (H);

[0022] (K) Send the nozzle opening value U′ on both sides of each row of spray beams to the PLC α,i,j , U′ β,i,j , keep the adjusted opening value for 30 seconds, and then re-collect the warpage value λ corresponding to the single unit of the strip j ;

[0023] (L) Calculate the lateral distribution objective function G(X) of the warpage of annealed strip:

[0024]

[0025] (M) Determine whether G(X)≤ε is true? Where ε is the on-site process value. If true, end. If not, proceed to step (C).

[0026] The beneficial effects of the present invention are as follows: compared with the prior art, the method of the present invention aims at uniform lateral distribution of warpage of the strip, optimizes and adjusts the nozzle opening during the cooling process, and can accurately control the uniform lateral distribution of warpage of the annealed strip in the water mist cooling section, thereby reducing the strip shape defects caused by the warpage distribution.

[0027] The specific warpage adjustment operation is: when the strip steel plate shape is warped upward, the warpage can be controlled by increasing the nozzle opening of the upper surface and reducing the nozzle opening of the lower surface; when the strip steel plate shape is warped downward, the warpage can be controlled by reducing the nozzle opening of the upper surface and increasing the nozzle opening of the lower surface. The method of the present invention is applied to the water mist cooling equipment of the fast cooling section of the continuous annealing unit, which can improve the quality of the finished strip steel products, bring economic benefits to the enterprise, and has great promotion value. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 It is a flow chart of the temperature accurate control method of the continuous retreat strong water mist cooling system of the present invention;

[0029] Figure 2 It is a discrete model of the strip steel under the action of a single spray beam in the present invention;

[0030] Figure 3for Figure 2 Schematic side view of

[0031] Figure 4 This is the temperature distribution diagram before and after control in Example 1 of the present invention;

[0032] Figure 5 This is the temperature distribution diagram before and after regulation of Example 2 of the present invention. DETAILED DESCRIPTION

[0033] In order to further illustrate the application process of the technology of the present invention, the production performance of the water mist cooling process section of a continuous annealing production line is taken as an example to explain in detail the application of the method in the field.

[0034] Example 1

[0035] like Figure 1 As shown, the present invention provides a method for accurately controlling the temperature of a continuous retreat strong water mist cooling system, and the implementation steps are as follows.

[0036] (1) In step (A), a discrete model of the strip under the action of the double-sided spray beam is constructed, such as Figure 2-3 As shown;

[0037] (2) In step (B), the main equipment process parameters and on-site feedback data of the water mist cooling section are collected, including: the number of spray beams M = 10, the number of nozzles in each row of spray beams K = 5, the maximum nozzle opening U max =100, the opening of each nozzle in each spray beam U i,j See Table 1, the distance between adjacent nozzles d = 400, the strip width B = 1600, and the warpage value λ corresponding to a single strip unit j ={-15.6,-3.2,14.9,18.6,2.8}, unit: mm;

[0038] Table 1 Opening U of each nozzle in each spray beam of Example 1 i,j

[0039]

[0040] (3) In step (C), the effective number of nozzles N corresponding to the strip is calculated, and the warpage value corresponding to each unit of the strip is integrated and calculated to obtain the absolute difference △λ of the warpage of each unit of the outlet strip under the current process. j :

[0041]

[0042] After calculation, N = 5, △λ j ={-19.1,-6.7,11.4,15.1,-0.7}, unit: mm;

[0043] (4) In step (D), the last row of spray beams is adjusted as the initial adjustment state, and the opening adjustment amount △U′ that each pair of nozzles of the Mth row of spray beams should make under the current warpage difference is calculated. M,j , where λ x is the current △λ j The maximum value of the corresponding warpage range, U x is the current △λ j The corresponding opening adjustment amount is as follows:

[0044]

[0045] After calculation, △U′ M,j ={-4.32,-1.84,1.79,2.53,-0.64};

[0046] (5) In step (E), according to the actual situation on site, the convexity to the α side of the strip is set as the positive warping value, and the convexity to the β side of the strip is set as the negative warping value, and the distribution value of the opening adjustment amount of the α and β sides of the strip is calculated:

[0047]

[0048] After calculation, △U′ α,M,j ={-2.16,-0.92,0.89,1.26,-0.32}, △U′ β,M,j ={2.16,0.92,-0.89,-1.26,0.32};

[0049] (6) In step (F), calculate the opening value U′ of the nozzles on the α and β sides of the M-th row of spray beams α,M,j , U′ β,M,j :

[0050]

[0051] After calculating U′ α,M,j ={57.84,59.08,60.89,61.26,59.68}、U′ β,M,j ={62.16,60.92,59.11,58.74,60.32};

[0052] (7) In step (G), determine 0≤U α,M,j +△U′ α,M,j ≤△U max , 0≤U β,M,j +△U′ β,M,j ≤△U max Is it established? If it is determined to be established, proceed to step (K);

[0053] (8) In step (K), the nozzle opening values ​​U′ on both sides of each row of spray beams are sent to the PLC α,i,j, U′ β,i,j , keep the adjusted opening value for 30 seconds, and then re-collect the warpage value λ corresponding to the single unit of the strip j ={-8.4,2.5,9.1,12.6,3.2}, unit: mm;

[0054] (9) In step (L), the objective function G(X) of the lateral distribution of warpage of the annealed strip is calculated:

[0055]

[0056] After calculation, G(X)=64.1;

[0057] (10) In step (M), determine whether G(X)≤ε holds. Where ε=100. If it holds, the calculation ends.

[0058] In this example, the nozzle opening of the water mist cooling section is adjusted to optimize the lateral distribution of the warpage at the strip outlet and reduce the strip defects. The situation before and after the adjustment is shown in Figure 4 .

[0059] Example 2

[0060] like Figure 1 As shown, the present invention provides a method for accurately controlling the temperature of a continuous retreat strong water mist cooling system, and the implementation steps are as follows.

[0061] (1) In step (A), a discrete model of the strip under the action of the double-sided spray beam is constructed, such as Figure 2-3 As shown;

[0062] (2) In step (B), the main equipment process parameters and on-site feedback data of the water mist cooling section are collected, including: the number of spray beams M = 10, the number of nozzles in each row of spray beams K = 5, the maximum nozzle opening U max =100, the opening of each nozzle in each spray beam U i,j See Table 2, the distance between adjacent nozzles d = 400, the strip width B = 1400, and the warpage value λ corresponding to a single strip unit j ={-14.2,-2.8,18.4,4.1,-12.6}, unit: mm;

[0063] Table 2 Opening U of each nozzle in each spray beam of Example 2 i,j

[0064]

[0065] (3) In step (C), the effective number of nozzles N corresponding to the strip is calculated, and the warpage value corresponding to each unit of the strip is integrated and calculated to obtain the absolute difference △λ of the warpage of each unit of the outlet strip under the current process. j :

[0066]

[0067] After calculation, N = 5, △λ j ={-12.78,-1.38,19.82,5.52,-11.18}, unit: mm;

[0068] (4) In step (D), the last row of spray beams is adjusted as the initial adjustment state, and the opening adjustment amount △U′ that each pair of nozzles of the Mth row of spray beams should make under the current warpage difference is calculated. M,j , where λ x is the current △λ j The maximum value of the corresponding warpage range, U x is the current △λ j The corresponding opening adjustment amount is as follows:

[0069]

[0070] After calculation, △U′ M,j ={-3.16,-0.88,3.37,0.51,-2.84};

[0071] (5) In step (E), according to the actual situation on site, the convexity to the α side of the strip is set as the positive warping value, and the convexity to the β side of the strip is set as the negative warping value, and the distribution value of the opening adjustment amount of the α and β sides of the strip is calculated:

[0072]

[0073] After calculation, △U′ α,M,j ={-1.58,-0.44,1.68,0.25,-1.42}, △U′ β,M,j ={1.58,0.44,-1.68,-0.25,1.42};

[0074] (6) In step (F), calculate the opening value U′ of the nozzles on the α and β sides of the M-th row of spray beams α,M,j , U′ β,M,j :

[0075]

[0076] After calculating U′ α,M,j ={0,0,1.68,0.25,0}, U′ β,M,j ={1.58,0.44,0,0,1.42};

[0077] (7) In step (G), determine 0≤U α,M,j +△U′ α,M,j ≤△U max , 0≤Uβ,M,j +△U′ β,M,j ≤△U max Is it established? If it is judged not to be established, go to step (H);

[0078] (8) In step (H), the opening data that is not satisfied by the Mth row of spray beams is calculated to obtain the opening adjustment amount △U′ that the nozzles on the α and β sides of the M-1th row of spray beams should make. α,M,j , △U′ β,M,j :

[0079]

[0080] After calculation, △U′ α,M-1,j ={-1.24,-0.1,0.34,0.34,-1.08}, △U′ β,M-1,j ={0.55,0.55,-1.13,0.3,0.55};

[0081] (9) In step (I), calculate the opening value U′ of each nozzle of the M-1th row of spray beams α,M-1,j , U′ β,M-1,j :

[0082]

[0083] Calculated

[0084] U′ α,M-1,j ={38.76,39.9,40.34,40.34,38.92}、U′ β,M-1,j ={40.55,40.55,38.87,40.3,40.55};

[0085] (10) In step (J), determine whether 0≤U α,M-1,j +△U′ α,M-1,j ≤△U max , 0≤U β,M-1,j +△U′ β,M-1,j ≤△U max Is it established? If it is determined to be established, proceed to step (K);

[0086] (11) In step (K), the nozzle opening values ​​U′ on both sides of each row of spray beams are sent to the PLC α,i,j , U′ β,i,j , keep the adjusted opening value for 30 seconds, and then re-collect the warpage value λ corresponding to the single unit of the strip j ={-8.8,1.1,8.5,2.9,-9.1}, unit: mm;

[0087] (12) In step (L), the objective function G(X) of the lateral distribution of warpage of the annealed strip is calculated:

[0088]

[0089] After calculation, G(X)=59.07;

[0090] (13) In step (M), determine whether G(X)≤ε holds. Where ε=100. If it holds, the calculation ends.

[0091] The distribution of warpage before and after the regulation in this example is shown in Figure 5 .

[0092] The above contents are only used to illustrate the technical solution of the present invention. Simple modifications or equivalent substitutions of the technical solution of the present invention made by ordinary technicians in this field do not deviate from the essence and scope of the technical solution of the present invention.

Claims

1. A method for controlling the warpage of strip steel in a continuous evacuation strong water mist cooling system. It is characterized in that The steps include: (A) A discrete model of the steel strip under the action of a double-sided spray beam is constructed to determine the number of nozzles acting on the steel strip. The steel strip is divided into corresponding units according to the positions of the nozzles. The temperature of the corresponding unit strip is adjusted by the nozzles on both sides of the strip, thereby adjusting the warpage of the steel strip caused by temperature. (B) Collect the main equipment process parameters and on-site feedback data of the water mist cooling section, including: the number of spray beams M, the number of nozzles in each row of spray beams K, and the maximum nozzle opening U max , the opening U of each nozzle in each spray beam i,j , the distance d between adjacent nozzles, the strip width B, the warpage value λ corresponding to a single strip unit j ; (C) Calculate the effective nozzle number N corresponding to the strip, integrate the warpage value corresponding to each unit of the strip, and obtain the absolute difference Δλ of the warpage of each unit of the outlet strip under the current process j : (D) Taking the adjustment of the last row of spray beams as the initial adjustment state, calculate the opening adjustment amount ΔU′ that each pair of nozzles in the Mth row of spray beams should make under the current warpage difference M,j , where λ x is the current Δλ j The maximum value of the corresponding warpage range, U x is the current Δλ j The corresponding opening adjustment amount is as follows: (E) According to the actual situation on site, the convexity to the α side of the strip is set as the positive warping value, and the convexity to the β side of the strip is set as the negative warping value, and the distribution value of the opening adjustment amount on the α and β sides of the strip is calculated: (F) Calculate the opening value U′ of the nozzles on the α and β sides of the M-th row of spray beams α,M,j , U′ β,M,j : (G) Determine 0≤U α,M,j +ΔU′ α,M,j ≤ΔU max , 0≤U β,M,j +ΔU′ β,M,j ≤ΔU max Is it true? If it is true, go to step (K); if not, go to step (H); (H) Calculate the opening data that is not satisfied by the Mth row of spray beams to obtain the opening adjustment amount ΔU′ that the nozzles on the α and β sides of the M-1th row of spray beams should make. α,M,j , ΔU′ β,M,j : (I) Calculate the opening value U′ of each nozzle in the M-1th row of spray beams α,M-1,j , U′ β,M-1,j : (J) Judge 0≤U α,M-1,j +ΔU′ α,M-1,j ≤ΔU max , 0≤U β,M-1,j +ΔU′ β,M-1,j ≤ΔU max Is it true? If it is true, go to step (K). If it is not true, set M = M-1 and go to step (H); (K) Send the nozzle opening value U′ on both sides of each row of spray beams to the PLC α,i,j , U′ β,i,j , keep the adjusted opening value for 30 seconds, and then re-collect the warpage value λ corresponding to the single unit of the strip j ; (L) Calculate the lateral distribution objective function G(X) of the warpage of annealed strip: (M) Determine whether G(X)≤ε is true? Where ε is the on-site process value, ε=100. If true, end; if not, proceed to step (C).

Citation Information

Patent Citations

  • Calculation method suitable for temperature of strip steel in rapid cooling section of continuous annealing processing line

    CN111154965A

  • Temperature optimization setting method for preventing and treating C warping of strip steel of hot-dip aluminum and zinc plating unit

    CN113444872A

  • Tension optimization setting method for hot-dip aluminum-zinc plating unit based on strip steel C warping treatment

    CN113449389A

  • Transverse adjustment method for spraying process of water mist cooling section of continuous annealing unit by taking control plate shape as target

    CN113637837A

  • Method and system suitable for optimizing fan cooling process of galvanizing unit

    CN113652622A