Preparation method and equipment for quartz purification from secondary tungsten tailings
By combining strong magnetic separation, acid leaching and flotation processes, high-purity silica is separated by solvent resistance, the problem of the inability to purify fine particle-caterings in secondary tungsten tailings is solved, and the efficient purification of quartz and Effective utilization of resources reduces environmental pollution and production costs.
Patent Information
- Application Number
- CN202111178480.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2021-09-30
- Filing Date
- 2021-10-10
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2041-10-10
AI Technical Summary
The fine-grained coniferous bodies in secondary tungsten tailings cannot purify quartz, resulting in waste of resources and environmental pollution. The existing technology is difficult to effectively treat fluorine-containing solid waste, which increases production costs.
Using a combination of strong magnetic separation, acid leaching and flotation processes, the continuous chemical reaction of the acid dissolving silicon is interrupted by using a solvent resistor (such as boric acid) to separate high-purity silica, and reduce the gas-liquid solid three-state through the recycling process. Waste.
It has achieved efficient purification of quartz in secondary tungsten tailings, reducing production costs, reducing environmental pollution, improving resource utilization, and saving processes and equipment.
Smart Images

Figure CN115888975B_ABST
Abstract
Description
[0001] The priority basis of the present invention includes: an invention application with an application date of September 30, 2021, application number 2021111612834, and patent name "A method and equipment for preparing quartz purified from secondary tungsten tailings". Technical Field
[0002] The invention relates to the technical field of quartz purification from fluorine-containing solid waste, and in particular to a preparation method and equipment for quartz purification from secondary tungsten tailings. Background Art
[0003] Secondary tailings are the discarded tailings after the original ore is processed and purified to obtain valuable minerals, and then the tailings are processed again to recover useful minerals. The characteristics of secondary tailings are as follows: the tailings particles are fine or even fine particles, most of the valuable non-metallic minerals are too fine or even fine particles, and the minerals are mostly intergrown, without monomer dissociation, and can no longer be separated into monomers by physical separation methods. They have no reuse value and are discarded and piled in the tailings pond. They are piled in the open air for a long time, causing safety hazards to the surrounding areas and personnel. Some secondary tailings (such as non-ferrous metal mines, non-metallic mines containing fluorite and asbestos, etc.) contain some toxic and harmful elements and minerals, which will pollute the surrounding environment and water sources and cause harm to personnel.
[0004] At present, the domestic treatment method for secondary tailings is mainly used in the construction and building materials industries, such as construction sand, construction bricks, cement, ceramics, etc. However, due to the low added value, the sales price is low, and most tailings ponds are located in remote areas, resulting in high transportation costs, which increases the production cost of secondary tailings treatment and leads to no profit or even negative profit, thus limiting the large-scale reuse of such tailings in the construction and building materials industries, and it is even impossible to fully utilize them.
[0005] Secondary tungsten tailings are the secondary tailings after the primary tailings of quartz vein-type tungsten ore are processed and purified to recover useful minerals (such as non-ferrous metal minerals or fluorite). They are a type of fluorine-containing solid waste. The mineral characteristics of this type of secondary tungsten tailings are basically as follows: 1. The main mineral in the tailings is quartz, followed by calcite, mica (mainly muscovite, biotite, sericite, etc., and the mica in different mining areas is mainly a certain type of mica, and other micas are basically non-existent or exist in small quantities), fluorite, dolomite (such as dolomite, ankerite, etc.), and a small amount of other minerals (mainly feldspar). Most of the quartz, calcite, dolomite, mica, and fluorite have been dissociated and exist in monomer form. However, there are still a small number of fine-particle-level minerals that have not been separated into monomers and are still intertwined, and cannot be separated into monomers by physical separation methods. 2. After secondary purification, the total content of non-ferrous metal minerals in secondary tailings is very small, and most of them are fine-particle-level and have not been separated into monomers and are still intertwined with quartz, fluorite, calcite, etc., which have been determined to have no recycling value in the existing technology. The mineral composition and multi-element content (wt%) and particle size range (mm) of this type of secondary tungsten tailings are specifically shown in the corresponding Figure 3 Table 1. Summary of the invention
[0006] The main purpose of the present invention is to provide a preparation method and equipment for purifying quartz from secondary tungsten tailings. The main progress is to overcome the difficulty of purifying quartz due to the presence of fine particle-level intergrowths in fluorine-containing solid waste and effectively recover intermediate products to reduce the pollution of the environment by gas-liquid-solid three-state waste.
[0007] The second main purpose of the present invention is to provide a quartz equipment for purifying fluorine-containing solid waste, so as to solve the problem that fine-grained (≧0.038mm) fluorine-containing solid waste cannot be purified into silicon dioxide and the intermediate product pollution after solid waste treatment.
[0008] One aspect of the main purpose of the present invention is achieved through the following technical solutions:
[0009] A preparation method for quartz purified from secondary tungsten tailings is proposed, comprising:
[0010] Performing a strong magnetic separation process on the secondary tungsten tailings to separate the iron-containing substances in the secondary tungsten tailings to obtain separated non-weakly magnetic minerals and weakly magnetic minerals;
[0011] The non-weakly magnetic mineral is subjected to an acid leaching step II and a solid-liquid separation step V to dissolve calcium-containing substances and magnesium-containing substances in the non-weakly magnetic mineral to obtain a quartz / fluorite / mica mixed ore, wherein the quartz / fluorite / mica mixed ore contains a conjoined body of quartz / fluorite / calcite without monomer dissociation;
[0012] The quartz / fluorite / mica mixed ore is subjected to a flotation I step to separate the fluorite concentrate to obtain a quartz / mica mixed ore, wherein the quartz / mica mixed ore contains a conjoined body of quartz / fluorite / calcite without monomer dissociation;
[0013] The quartz / mica mixed ore is subjected to flotation II process to separate the mica concentrate and obtain a quartz rough concentrate, wherein the quartz rough concentrate contains a conjoined body of quartz / fluorite / calcite without monomer dissociation;
[0014] The quartz rough concentrate is subjected to an acid leaching step III and a solid-liquid separation step VI, wherein a strong acid and a dissolving agent are used in the acid leaching step III, wherein the strong acid dissolves the fluorine-containing substances in the quartz rough concentrate but does not dissolve the silicon dioxide, thereby dissociating the intergrown monomers, and the dissolving agent can interrupt the continuous chemical reaction of the acid dissolving silicon, so that the silicon dioxide of the intergrown before the monomer dissociation is retained in the quartz rough concentrate, thereby obtaining a quartz concentrate;
[0015] The fluorine-containing liquid dissolved in the solid-liquid separation step VI is subjected to a first recovery process to obtain chemical products to eliminate gas-liquid-solid three-state waste.
[0016] By adopting the above technical solution, it is known that hydrofluoric acid, which is an intermediate product generated in the acid reaction, can also react continuously with silicon dioxide, aluminum oxide, and silicon dioxide in the aluminosilicate-containing material to generate fluorosilicic acid;
[0017] Chemical reaction equation: 6HF+SiO 2 (S) = H 2 SiF 6 + 2H 2 O; This is the intermediate reaction that the present invention hopes to avoid generating;
[0018] Therefore, in the acid leaching III process, the secondary tungsten tailings is specifically a solid waste including fluorine-containing substances (it can also be wet pyrometallurgical slag, smoke and flue gas sediment, wastewater and waste acid sediment, fluorine-containing minerals and tailings, etc.), and the fluorine-containing substances are specifically fluoride, fluoride salt, fluorite, fluoroapatite, etc., and the fluorine-containing solid waste also contains a certain amount or a large amount of silicon dioxide, aluminum oxide, aluminum silicate, calcium magnesium compounds and other substances, among which fluorite, fluoroapatite, fluoride, and fluoride salt will react chemically with strong acid to generate hydrofluoric acid (HF). Therefore, when the solid waste contains fluorine-containing substances (such as fluorite, fluoroapatite, fluoride, and fluoride salt), it is impossible to use a strong acid decomposition method or a strong acid selective acid leaching method to separate the fluorine-containing substances from silicon dioxide, aluminum oxide, aluminum silicate, and calcium magnesium compounds, because fluoride ions will react with silicon dioxide in silicon dioxide, aluminum oxide, aluminum silicate, and calcium magnesium compounds to generate corresponding fluorine compounds. Moreover, the strong acid solution obtained after the treatment by the strong acid decomposition method and the strong acid selective acid leaching method contains fluorosilicic acid and fluorosilicate, which increases the difficulty of treatment and recovery or even makes it impossible to treat and recycle, increases the production cost, and even makes it impossible to produce in serious cases. In the present invention, a dissolution inhibitor (specifically boric acid, or borates can also be used, but the recovery is more complicated) is added to the strong acid, so that the fluorine-containing substance in the solid waste of fluorine-containing substances reacts with the strong acid to generate hydrofluoric acid and preferentially reacts with the dissolution inhibitor (specifically boric acid (H 3 BO 3 ) or borate) to produce fluoroboric acid (HBF 4 ), blocking the chain acid reaction of silicon dissolution. Moreover, the dissolution inhibitor (specifically boric acid or borate) can be reused after recovery. Under the conditions of specific temperature, hydrofluoric acid concentration, boric acid, reaction time, solid-liquid ratio and stirring range, fluoroboric acid does not chemically react with silicon dioxide. However, oxides of calcium, magnesium, aluminum, potassium, iron, etc. in substances such as alumina, aluminosilicates, and calcium-magnesium compounds will chemically react with fluoroboric acid and be dissolved into fluoroboric acid, while silicon dioxide in substances such as alumina, aluminosilicates, and calcium-magnesium compounds will not be dissolved by fluoroboric acid and exist as a solid, so that silicon dioxide is separated from other substances, and high value-added silicon dioxide powder and chemical products containing calcium, magnesium, aluminum, potassium, iron, etc. that meet the requirements of demanding industries are obtained;
[0019] The main chemical reaction equation of acid leaching III process:
[0020] 2HCl + CaF 2 (s) = 2HF + CaCl 2 (aq) , where CaF 2 It is calcium fluoride that belongs to the composition of fluorite before the dissociation of the conjoined monomers;
[0021] 2HCl + CaCO 3 (s) = CO 2 (g) ↑ + CaCl2 (aq) + H 2 O, of which CaCO 3 It is calcium carbonate that belongs to the calcite composition before the intergrowth monomers are dissociated; therefore, the intergrowth is dissociated by monomers in the acid leaching III process;
[0022] The chemical reaction equation for silicon dissolution in the acid leaching III process is:
[0023] 4HF + H 3 BO 3 + SiO 2 (s) = HBF 3 OH + HF + 2H 2 O + SiO 2 (s) ;
[0024] HBF 3 OH + HF + SiO 2 (s) = HBF 4(aq) + H 2 O + SiO 2 (s) , where SiO 2 Including silicon dioxide that belongs to quartz composition after the dissociation of conjoined monomers;
[0025] The purified quartz has a higher yield and no gas, liquid, and solid three-state waste.
[0026] In a preferred example, the present invention can be further configured as follows: the first recovery process of the fluorine-containing liquid includes:
[0027] A precipitation step IV of adding aqueous ammonia and a solid-liquid separation step VII to separate the calcium fluoride product and the first recovered liquid;
[0028] The first recovered liquid is subjected to an alkali decomposition step of adding calcium hydroxide and a distillation step IV to obtain a second recovered liquid, wherein the gas separated by the alkali decomposition step and the distillation step is subjected to an absorption step I to obtain a high-purity ammonia product;
[0029] The second recovered liquid is subjected to a precipitation step V of adding sulfuric acid and a solid-liquid separation step VIII to separate a calcium sulfate product and a third recovered liquid;
[0030] The third recovered liquid is subjected to a distillation step V to separate the boric acid product and the distilled fourth recovered liquid, and the fourth recovered liquid is subjected to an absorption step II to obtain a high-purity hydrochloric acid product.
[0031] By adopting the above-mentioned preferred technical features, the separation and recovery of various chemicals can be achieved mainly by utilizing the precipitation IV step of adding ammonia water, the alkali decomposition step of adding calcium hydroxide, and the precipitation V step of adding sulfuric acid.
[0032] In a preferred example, the present invention can be further configured as follows: the strong acid used in the acid leaching III process is hydrochloric acid, the dissolution inhibitor used is boric acid, and the fluoroboric acid generated by the intermediate reaction does not chemically react with silicon dioxide, but chemically reacts with oxides containing calcium, magnesium, aluminum, potassium, and iron in alumina, aluminosilicate, and calcium-magnesium compounds to dissolve them into the fluoroboric acid.
[0033] By adopting the above-mentioned preferred technical features, using hydrochloric acid as a strong acid and boric acid as a silicon-inhibiting solvent, the quartz / fluorite / calcite intergrowth can dissolve the fluorite and calcite components while retaining the quartz component as a solid, so that the intergrowth can be well dissociated into monomers, and the quartz concentrate has a higher yield and purity.
[0034] The present invention can be further configured as follows in a preferred example: the operating conditions of the acid leaching III process include: temperature less than 50-90°C, reaction time less than 20-70min, solid-liquid ratio 1kg: (1-3)L; preferably, temperature 40-70°C, reaction time 30-60min, solid-liquid ratio 1kg: (1-1.4)L, hydrofluoric acid concentration range of 6-11%, solvent inhibitor concentration range of 7.5-12.5%, hydrochloric acid concentration range of 3-5mol / L.
[0035] By adopting the above-mentioned preferred technical features, the solid-liquid ratio of the acid leaching process III is 1kg: (1-3)L. When the calcium fluoride content is fixed, as the amount of liquid in the solid-liquid ratio increases, the improvement of the acid leaching effect is not large, but the production cost will be increased and it is not cost-effective; when the concentrations of hydrochloric acid and boric acid remain unchanged, hydrochloric acid reacts with calcium fluoride to generate hydrofluoric acid, and hydrofluoric acid reacts with boric acid to generate fluoroboric acid, so the amount of liquid in the solid-liquid ratio within the range is proportional to the content of calcium fluoride in the tailings; the temperature (50°C-90°C) and time (30min-60min) of the acid leaching process III are also the same. When the concentration of hydrofluoric acid increases, the concentration of boric acid also increases, and the concentrations of the two acids are proportional to the content of calcium fluoride in the leached solid; the stirring speed has no excessive influence, as long as the solid does not sink to the bottom and does not splash.
[0036] The present invention can be further configured in a preferred example as follows: the preparation method further comprises:
[0037] The weakly magnetic mineral is subjected to an acid leaching step I and a solid-liquid separation step I, using hydrochloric acid to obtain biotite concentrate and a non-fluorine-containing liquid;
[0038] Performing a second recovery process on the non-fluorine-containing liquid to obtain separated iron hydroxide products, sodium chloride products, calcium sulfate products, magnesium sulfate products and high-purity hydrochloric acid products;
[0039] Preferably, the second recovery process of the non-fluorine-containing liquid includes: an oxidation / precipitation I step, a solid-liquid separation II step corresponding to the preparation of the iron hydroxide product, a precipitation II step, a solid-liquid separation III step, a neutralization step, an evaporation I step corresponding to the preparation of the sodium chloride product, an acid dissolution step, a precipitation III step, a solid-liquid separation IV step corresponding to the preparation of the calcium sulfate product, and a distillation / evaporation II step corresponding to the preparation of the magnesium sulfate product.
[0040] In a preferred example, the present invention can be further configured as follows: the first recovery process of the fluorine-containing liquid and the second recovery process of the non-fluorine-containing liquid overlap in the absorption II process, so as to simultaneously recover the high-purity hydrochloric acid product; preferably, the tailings conjoined body dissociation process and the second recovery process of the non-fluorine-containing liquid overlap in the precipitation III process, so as to simultaneously recover the calcium sulfate I product through the solid-liquid separation IV process S49, recover the magnesium sulfate product through the distillation / evaporation II process, and recover the high-purity hydrochloric acid product through the absorption II process.
[0041] By adopting the above-mentioned preferred technical features, the first recovery process of the fluorine-containing liquid and the second recovery process of the non-fluorine-containing liquid, as well as the tailings intergrowth dissociation process and the second recovery process of the non-fluorine-containing liquid can be integrated by overlapping processes, so as to save process steps and reduce the construction of production equipment.
[0042] Another aspect of the main purpose of the present invention is achieved by the following technical solutions:
[0043] A secondary tungsten tailings purified quartz device is proposed, which is used to implement a preparation method of secondary tungsten tailings purified quartz according to the possible technical combination as described above.
[0044] The second main purpose of the present invention is achieved through the following technical solutions:
[0045] A quartz device for purifying fluorine-containing solid waste is proposed, comprising:
[0046] The strong magnetic separation unit separates the iron-containing substances in the solid waste to obtain non-magnetic solid waste;
[0047] The acid leaching unit II and the solid-liquid separation unit V are used to dissolve the calcium-containing substances and the magnesium-containing substances in the non-magnetic solid waste to obtain a first mixed solid waste, wherein the first mixed solid waste contains a conjoined body of silicon dioxide / calcium fluoride / calcium carbonate without monomer dissociation;
[0048] A conjoined body dissociation module is used to dissociate the conjoined bodies at the fine particle level in the first mixed solid waste; the conjoined body dissociation module comprises:
[0049] A flotation I unit, used for separating calcium fluoride from the first mixed solid waste to obtain a second mixed solid waste, wherein the second mixed solid waste contains the conjoined bodies;
[0050] A flotation II unit is used to separate mica from the second mixed solid waste to obtain a third mixed solid waste, wherein the third mixed solid waste contains the conjoined bodies; and
[0051] an acid leaching III unit and a solid-liquid separation VI unit, wherein the acid leaching III unit uses a strong acid and a dissolving agent to dissolve the fluorine-containing substances and the calcium-containing substances in the conjoined bodies of the third mixed solid waste but not the silicon dioxide, so that the conjoined bodies are dissociated into monomers, and the dissolving agent interrupts the continuous chemical reaction of the acid-dissolved silicon, so that the silicon dioxide of the conjoined bodies before the monomers are dissociated is retained in the third mixed solid waste, so as to obtain silicon dioxide; and,
[0052] A recovery equipment module is used to recover the fluorine-containing liquid dissolved by the acid leaching unit III and separated by the solid-liquid separation unit VI to obtain chemical products, so as to eliminate gas-liquid-solid three-state waste;
[0053] Among them, the fluorine-containing solid waste is specifically selected from any one of wet pyrometallurgical smelting slag, smoke and flue gas sediment, treated wastewater and waste acid precipitates, fluorine-containing minerals and secondary tungsten tailings; preferably, the process conditions of the acid leaching III unit include: temperature 40-70°C, reaction time 30-60min, solid-liquid ratio 1kg: (1-1.4)L, hydrofluoric acid concentration range of 6-11%, solvent inhibitor concentration range of 7.5-12.5%, and hydrochloric acid concentration range of 3-5mol / L.
[0054] In summary, the present invention includes at least one of the following technical effects that contribute to the prior art:
[0055] 1. The secondary tailings processed by the present invention are mainly for quartz vein type tungsten ores, which are secondary tailings after secondary processing and purification of useful minerals. Most of the valuable non-metallic minerals in this type of secondary tailings are too finely embedded or even at the level of fine particles, and are mostly conjoined bodies without monomer dissociation. They can no longer be separated into monomers by physical mineral separation methods. They have no reuse value and are piled up in the open air for a long time, causing safety hazards to the surrounding areas and personnel, polluting the surrounding environment and water sources, and causing harm to personnel. However, through the production process adopted by the present invention, this type of secondary tailings can be fully utilized and turned into treasure, without causing the production cost of the secondary tailings to be increased, which will reduce the company's production profit or even make no profit. Instead, it can generate profits by treating the secondary tailings alone. No tailings are generated, and no three wastes are generated, which are harmless to the surrounding environment and human body.
[0056] 2. The first recovery process of fluorine-containing liquid and the second recovery process of non-fluorine-containing liquid overlap in the absorption II process, so as to simultaneously recover high-purity hydrochloric acid products, thereby saving processes and production equipment. The tailings intergrowth dissociation process and the second recovery process of non-fluorine-containing liquid overlap in the precipitation III process, so as to simultaneously recover calcium sulfate I products through the solid-liquid separation IV (filtration) / rinsing process, recover magnesium sulfate products through the distillation / evaporation II process, and recover high-purity hydrochloric acid products through the absorption II process, thereby saving processes and production equipment;
[0057] 3. The purity of hydrochloric acid used in each process must be industrial grade, and the purity of the recovered hydrochloric acid can reach analytical grade. BRIEF DESCRIPTION OF THE DRAWINGS
[0058] Figure 1 A production process flow chart showing a method for preparing quartz purified from secondary tungsten tailings according to some preferred embodiments of the present invention is shown;
[0059] Figure 2 A schematic diagram of a module of a quartz device for purifying fluorine-containing solid waste according to some preferred embodiments of the present invention is shown;
[0060] Figure 3 Corresponding to Table 1, the mineral composition and multi-element content range (wt%) and particle size range (mm) of the secondary tungsten tailings are listed; Figure 4 The mineral compositions, multi-element contents and particle sizes of the secondary tungsten tailings used in the examples listed in Table 2 correspond to each other;
[0061] Figure 5 Corresponding Table 3 lists the mineral recovery rate and yield of 100 kg of secondary tungsten tailings obtained according to the process flow of the present invention;
[0062] Figure 6 Corresponding to Table 4, 500 kg of quartz was mixed evenly and then samples were taken for mineral phase and element analysis, and the contents of various mineral phases and elements were listed;
[0063] Figure 7 Corresponding Table 5 lists the quartz dissolution rate (%) with and without adding a dissolving inhibitor when the hydrofluoric acid concentration (mass ratio) is changed under the same production process parameters;
[0064] Figure 8 Corresponding Table 6 lists the quartz dissolution rate (%) with and without adding a dissolving inhibitor when the acid leaching temperature is changed under the same production process parameters;
[0065] Fig. 9 Corresponding Table 7 lists the quartz dissolution rate (%) with and without adding a dissolving inhibitor when the acid leaching reaction time is changed under the same production process parameters;
[0066] Fig.10 Corresponding Table 8 lists the quartz dissolution rate (%) with and without adding a dissolution inhibitor when the boric acid (dissolution inhibitor) concentration condition is changed under the same production process parameters;
[0067] Fig.11 Corresponding Table 9 lists the quartz dissolution rate (%) with and without adding a dissolving agent when the solid-liquid ratio is changed under the same production process parameters;
[0068] Fig.12 Table 10 shows the time required for calcium fluoride to be completely dissolved by the acid leaching agent (different volumes, concentrations and temperatures);
[0069] Fig.13 Corresponding Table 11 lists the solubility of boric acid at different temperatures;
[0070] Fig.14 Corresponding Table 12 lists the quartz dissolution rate (%) under the condition of changing a certain production process parameter;
[0071] Fig.15 Corresponding Table 13 lists the quartz dissolution rate test results of two different quartz samples with different silicon dioxide contents (99.99% and 99.74% respectively) under the same conditions (temperature 90°C, reaction time 80min, solid-liquid ratio 1.0:3.0) with different fluoroboric acid concentrations;
[0072] Fig.16 Corresponding Table 14 lists the dissolution rates of mica and feldspar when the concentration of fluoroboric acid is changed under the same production process parameters.
[0073] Figure symbols: S11, strong magnetic separation process; S12, acid leaching II process; S13, solid-liquid separation V (filtration) / rinsing process; S14, acid leaching I process; S15, solid-liquid separation I (filtration) / rinsing process; S2, tailings intergrowth dissociation process; S21, flotation I process; S22, flotation II process; S23, acid leaching III process; S24, solid-liquid separation VI (filtration) / rinsing process; S3, first recovery process of fluorine-containing liquid; S31, precipitation IV process; S32, solid-liquid separation VII (filtration) / rinsing process; S33, alkali decomposition process; S34, distillation IV process; S35, absorption I process; S36, precipitation V process; S37, solid-liquid separation VIII (filtration) / rinsing process; S38, distillation V process; S39, absorption II process; S41, oxidation / precipitation I process; S42, solid-liquid separation II (filtration) / rinsing process; S43, precipitation II process; S44, solid-liquid separation III (filtration) / rinsing process; S45, neutralization process; S46, evaporation I process; S47, acid dissolution process; S48, precipitation III process; S49, solid-liquid separation IV (filtration) / rinsing process; S50, distillation / evaporation II process; 11, strong magnetic separation unit; 12, acid leaching II unit; 13, solid-liquid separation V unit; 14, acid leaching I unit;
[0074] 20. Conjoined body dissociation module; 21. Flotation I unit; 22. Flotation II unit;
[0075] 23. Acid leaching III unit; 24. Solid-liquid separation VI unit;
[0076] 30. A first recovery equipment module for fluorine-containing liquid; 31. A precipitation IV unit;
[0077] 32. Solid-liquid separation VII unit; 33. Alkali decomposition unit; 34. Distillation IV unit;
[0078] 35. Absorption I unit; 36. Precipitation V unit; 37. Solid-liquid separation VIII unit;
[0079] 38. Distillation V unit; 39. Absorption II unit. DETAILED DESCRIPTION
[0080] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments for understanding the inventive concept of the present invention, and cannot represent all the embodiments, nor are they interpreted as the only embodiments. Based on the embodiments in the present invention, all other embodiments obtained by ordinary technicians in this field on the premise of understanding the inventive concept of the present invention are within the scope of protection of the present invention.
[0081] Figure 1 A production process flow chart of a method for preparing quartz purified from secondary tungsten tailings according to some preferred embodiments of the present invention is shown. The accompanying drawings only show the common parts of multiple embodiments, and the parts with differences or distinctions are described in text or presented in comparison with the drawings. Therefore, based on the industrial characteristics and technical essence, technicians familiar with the field should be able to correctly and reasonably understand and judge whether the individual technical features described below or any combination of them can characterize the same embodiment, or whether multiple technical features with mutually exclusive technical essences can only characterize different variant embodiments respectively.
[0082] In a specific embodiment, the secondary tungsten tailings minerals used include: ① The total content of non-ferrous metal minerals in the secondary tailings after secondary purification is 0.034%, and most of them are fine particles and are still intergrown with quartz, fluorite, calcite, etc. without monomer dissociation, and have no recovery value. In the secondary tungsten tailings; ② The main minerals in the tailings are quartz, followed by calcite, biotite, fluorite, dolomite, iron dolomite, and mica. A small amount of other minerals (mainly feldspar). Most of the quartz and (calcite, dolomite, iron dolomite, biotite, mica, fluorite) have been dissociated from each other and exist in the form of monomers, but there are still a small number of (0.019-0.005mm) fine-grained minerals and minerals that have no monomer dissociation and are still intergrown, and can no longer be separated into monomers by physical separation methods. ③ The average yield of particles below -0.15mm is 98%, the average yield of particles below -0.038mm is 73%, and the average yield of particles below -0.019mm is 43.61%. Particles below -0.019mm are fine-particle tailings and contain a certain amount of mineral processing reagents. The calcite, ankerite, and biotite in the secondary tungsten tailings are mostly below -0.038mm. Fluorite and quartz are mostly above +0.038mm. The mineral composition, multi-element content, and particle size range of the secondary tungsten tailings are shown in the corresponding Figure 4 Table 2.
[0083] Reference Figure 1 , is a preparation method for purifying quartz from secondary tungsten tailings disclosed in an embodiment of the present invention, comprising:
[0084] Step S11: performing a strong magnetic separation process on the secondary tungsten tailings to separate the iron-containing substances in the secondary tungsten tailings to obtain separated non-weakly magnetic minerals and weakly magnetic minerals;
[0085] Steps S12 and S13: performing an acid leaching process II and a solid-liquid separation process V on the non-weakly magnetic mineral to dissolve calcium-containing substances and magnesium-containing substances in the non-weakly magnetic mineral to obtain a quartz / fluorite / mica mixed ore, wherein the quartz / fluorite / mica mixed ore contains a conjoined body of quartz / fluorite / calcite without monomer dissociation; the solid-liquid separation process V is specifically a solid-liquid separation V (filtration) / elution process S13;
[0086] See also Figure 1 The dotted box on the upper right side is followed by the tailings intergrowth dissociation process S2, including:
[0087] Step S21: performing a flotation I process on the quartz / fluorite / mica mixed ore to separate the fluorite concentrate and obtain a quartz / mica mixed ore, wherein the quartz / mica mixed ore contains a conjoined body of quartz / fluorite / calcite without monomer dissociation;
[0088] Step S22: performing flotation II process on the quartz / mica mixed ore to separate the mica concentrate and obtain a quartz rough concentrate, wherein the quartz rough concentrate contains a conjoined body of quartz / fluorite / calcite without monomer dissociation;
[0089] Steps S23 and S24: the quartz rough concentrate is subjected to an acid leaching process III and a solid-liquid separation process VI. A strong acid and a dissolving agent are used in the acid leaching process III. The strong acid dissolves the fluorine-containing substances in the quartz rough concentrate but does not dissolve the silicon dioxide, so that the intergrown monomers are dissociated. The dissolving agent can interrupt the continuous chemical reaction of the acid-dissolved silicon, so that the silicon dioxide of the intergrown before the monomer dissociation is retained in the quartz rough concentrate to obtain the quartz concentrate. The solid-liquid separation process VI is specifically a solid-liquid separation process VI (filtration) / elution process S24;
[0090] See also Figure 1 The dotted box on the lower right side is step S3: performing a first recovery process on the fluorine-containing liquid dissolved in the solid-liquid separation step VI to obtain chemical products to eliminate gas-liquid-solid three-state waste.
[0091] The implementation principle of this embodiment is: the tailings intergrowth dissociation process S2 is implemented after the strong magnetic separation process S11, the acid leaching II process S12 to the solid-liquid separation V (filtration) / rinsing process S13 and before the first recovery process S3 of the fluorine-containing liquid. The input of the tailings intergrowth dissociation process S2 is a quartz / fluorite / mica mixed ore with intergrowths mainly below the fine particle size (containing 0.038mm) (>70 wt%); the output after the solid-liquid separation VI (filtration) / rinsing process S24 is the separated quartz concentrate and the fluorine-containing liquid. The first recovery process S3 of the fluorine-containing liquid can purify quartz with high purity and high yield, and there is no gas-liquid-solid three-state waste.
[0092] about Figure 1 S11, the input of the strong magnetic separation process S11 is secondary tungsten tailings, the magnetic field strength is 1.3~1.5T, and the magnetic separation slurry concentration is 20~30% by mass. In the specific example, 100Kg of secondary tungsten tailings are mixed evenly and then the calculated volume of water is added to control the concentration of the magnetic separation slurry within the range of 20~30% (mass ratio), including the endpoint value. After entering the strong magnetic separation production process under stirring, the separated weak magnetic minerals and non-weak magnetic minerals are obtained respectively. Weak magnetic minerals (including biotite and iron dolomite) enter the production process of acid leaching I process S14. Non-weak magnetic minerals (including fluorite, quartz, calcite, dolomite, mica, and other minerals (mainly feldspar)) enter the production process of acid leaching II process S12.
[0093] The non-weakly magnetic minerals are purified based on the description of the following process, including the first recovery process S3 of the fluorine-containing liquid, corresponding to S31 to S39 in the figure.
[0094] about Figure 1 In S12, the non-weakly magnetic minerals are subjected to acid leaching II step S12, and the acid leaching solution II used is specifically 1 mol / L hydrochloric acid (preparation; commercially available concentrated hydrochloric acid solution: water = 1:11). Since the acid leaching II step S12 is implemented after the secondary tungsten tailings enter the strong magnetic separation step S11, the separated non-weakly magnetic minerals are selected for treatment, which does not include iron substances but includes fluorine substances. The non-weakly magnetic minerals put into the acid leaching II step S12 generally contain fluorite, quartz, calcite, dolomite, mica, and other minerals (mainly feldspar). Under stirring, the acid leaching solution II is first added to the solution at a flow rate of 50L / min. After no large amount of bubbles are generated, the acid leaching solution II is added at a flow rate of 10L / min until the pH of the solution reaches ≈ 1.0. Among them, the S12 acid leaching solution II and the CaCO in calcite and dolomite 3 MgCO 3 Chemical reactions generate calcium chloride and magnesium chloride that are easily soluble in water, which dissolve into the acid leaching solution II; while fluorite is slightly soluble in dilute hydrochloric acid, and quartz and mica minerals are insoluble in dilute hydrochloric acid, and exist in the acid leaching solution II in solid form. After stirring for another 10 minutes, the mixture enters the solid-liquid separation V (filtration) / rinsing step S13 for production.
[0095] about Figure 1S13, solid-liquid separation V (filtration) / rinsing process S13 includes: firstly performing solid-liquid separation V (filtration) operation and then rinsing with clean water until the pH of the rinsing water V after rinsing the filter residue V is ≈ 5; wherein the obtained filtrate V is the acid leaching solution II, and the filtrate contains calcium and chloride ions; the obtained filter residue V contains mixed minerals of fluorite, quartz, and mica, that is, a quartz / fluorite / mica mixed ore containing quartz / fluorite / calcite without monomer dissociation intergrowth. The filtrate V and the rinsing water V preferably enter the precipitation III process S48 in the second recovery process together to enter the precipitation operation production. The filter residue V enters the tailings intergrowth dissociation process S2 for quartz purification operation.
[0096] The chemical reaction equation of the acid leaching II step S12 is as follows:
[0097] CaCO 3 + 2HCl = CaCl 2 + H 2 O + CO 2 ↑;
[0098] MgCO 3 + 2HCl = MgCl 2 + H 2 O + CO 2 ↑;
[0099] Therefore, the function of the acid leaching II step S12 is to separate the calcium and magnesium substances on the surface of the non-weakly magnetic mineral and the internal part of the mineral particles, so as to facilitate the subsequent tailings intergrowth dissociation operation. In the example, the tailings intergrowth dissociation process S2 includes: flotation I step S21, flotation II step S22, acid leaching III step S23, solid-liquid separation VI (filtration) / rinsing step S24.
[0100] Regarding the intergrowth of quartz / fluorite / calcite without monomer dissociation, the first mixed solid waste obtained after the non-magnetic solid waste in the example is subjected to the acid leaching II process S12 operation is mainly silica / calcium fluoride / mica / other minerals (mainly feldspar). Because the content of other minerals in the secondary tungsten tailings is only 1-5%, some of them are dissolved by the acid leaching solution during the acid leaching II operation, so the present invention omits recording other minerals. Calcite and dolomite are basically all dissolved by the acid leaching solution and enter the acid leaching solution in the form of calcium / magnesium ions. There are only trace amounts of calcite and dolomite in the first mixed solid waste, while silica / calcium fluoride / mica / other minerals are not dissolved by the acid leaching solution and exist in the acid leaching solution in solid form and are separated. Some of the four minerals of silica / calcium fluoride / mica / other minerals (mainly feldspar) in the first mixed solid waste are not dissociated, that is, intergrowth. After the first mixed solid waste is processed in the acid leaching step III S23, calcium fluoride is basically completely dissolved by the acid leaching solution and enters the acid leaching solution in the form of (calcium, fluoride) ions, and can be separated from the solid silicon dioxide / mica / other minerals (mainly feldspar) in the acid leaching solution. After the acid leaching step III S23, most of the other minerals (mainly feldspar) are dissolved by the acid leaching solution (because the content is less than 1-5%, the record is omitted), a small amount of mica is dissolved by the acid leaching solution, and quartz (silicon dioxide) is not dissolved by the acid leaching solution.
[0101] about Figure 1 S21, the quartz / fluorite / mica mixed ore (i.e., the filter residue V of S13) is subjected to flotation I process S21, and the specific process parameters include: the flotation pulp concentration is 30-40% (mass ratio); the flotation collector is modified oleic acid (oleic acid triethanolamine soap); the flotation depressant is acidified water glass, water glass and sodium carbonate; the flotation times are 5-7 times. When the filter residue V (containing fluorite, quartz, and mica) enters the flotation I process S21 production, the flotation foam obtained after the flotation operation of S21 is the fluorite concentrate, and the calcium fluoride content is ≥97%, which meets the requirements of the required industry. The minerals at the bottom of the S21 flotation tank are mixed minerals containing quartz and mica, that is, quartz / mica mixed ore, and the quartz / mica mixed ore contains quartz / fluorite / calcite without monomer dissociation.
[0102] about Figure 1 S22, the quartz / mica mixed ore is subjected to flotation II step S22, and the process parameters specifically include: the flotation pulp concentration is 30-40% (mass ratio); the pH value of the flotation pulp is controlled at pH3-pH4; the flotation collector is dodecylamine; the flotation collector dosage is controlled at 50-100 g / t (t is the solid mass ton of the flotation pulp concentration); the flotation depressant is sodium hexametaphosphate [Na(PO 3 ) 6]; The amount of flotation depressant is controlled at 4-6 kg / t (t is the solid mass tons of the flotation pulp concentration); The number of flotation times is 2-3 times. S22 specifically includes: putting the quartz / mica mixed ore into the flotation II process S22 for production, and the flotation foam produced by the flotation operation in the flotation II process S22 is a mica concentrate, and the mica content is ≧94%, which meets the requirements of the required industry. The mineral at the bottom of the flotation tank is a quartz rough concentrate, which contains a small amount of fluorite, a very small amount of mica, and other minerals, that is, a quartz rough concentrate containing quartz / fluorite / calcite intergrowths. The quartz rough concentrate obtained by S22 enters the acid leaching solution III process S23 for production.
[0103] about Figure 1 S23, the acid leaching solution III used in the acid leaching step S23 is specifically hydrochloric acid concentration (4mol / L): boric acid = 100:5 (volume mass ratio). The input of the acid leaching step S23 is quartz rough concentrate. The solid-liquid ratio of the purification production process is specifically quartz rough concentrate: purification liquid = 1: (1-2) (mass volume ratio). The specific operating conditions of the acid leaching step S23 include: temperature less than 50°C, hydrofluoric acid concentration less than 20% (mass ratio), boric acid less than 10% (mass ratio), reaction time less than 30min, solid-liquid ratio 50kg: 50L (1:1), stirring speed 90 rpm. S23 specifically includes: the quartz rough concentrate enters the acid leaching solution III process S23 for production operation, and under stirring, the calculated volume of the acid leaching solution III is added at a flow rate of 25L / min, heated to 50°C, and then boric acid solid is added (the mass of the required boric acid solid is added at a ratio of purified liquid: boric acid solid = 100:5) to make the boric acid concentration in the acid leaching solution III about 10% (mass ratio). Because the solubility of boric acid is low at room temperature and the solubility does not reach 10%, this addition method is adopted; then the quartz rough concentrate is placed in In the acid leaching solution III (boric acid concentration is about 10%), the acid leaching solution III is heated to 50°C and maintained at 50°C. After stirring for 10-30 minutes, the acid leaching solution III reacts with the fluorite in the quartz rough concentrate to generate calcium chloride and hydrofluoric acid. The hydrofluoric acid reacts with the boric acid to generate fluoroboric acid so that the hydrofluoric acid does not react with the quartz. Boric acid is preferably used as a dissolution inhibitor. Without considering the lowest recovery cost, the silicon dissolution inhibitor can be selected from borates to prevent hydrofluoric acid from reacting with quartz to generate fluorosilicic acid and avoid quartz being dissolved by hydrofluoric acid, thereby reducing the mass of quartz solids. Most of the quartz in S23 exists in the acid leaching solution III in solid form. The acid leaching solution III containing solids enters the solid-liquid separation VI (filtration) step S24 for production.
[0104] about Figure 1S24, the acid leaching solution III obtained in S23 enters the solid-liquid separation VI (filtration) / rinsing process S24 for production, first performs solid-liquid separation (filtration) operation and then rinses with clean water until the pH of the rinsing water VI after rinsing the filter residue VI is 6-7. The filtrate VI obtained in S24 includes the acid leaching solution III and the acid leaching solution III containing calcium, chloride ions, fluoroboric acid, boric acid, and the filtrate VI and the rinsing water VI as fluorine-containing liquid, and enters the first recovery process S3 of the fluorine-containing liquid. The filter residue VI obtained in S24 is a high-purity quartz concentrate product with a silicon dioxide content of ≧99.60%, which meets the requirements of the required industry.
[0105] The chemical reaction equation of the acid leaching III step S23 is as follows:
[0106] 2HCl + CaF 2 = 2HF + CaCl 2 ;
[0107] 4HF + H 3 BO 3 = HBF 4 + 3H 2 0;
[0108] Therefore, the role of the acid leaching step III S23 is to dissolve the fluorine-containing substances and calcium-containing substances in the quartz rough concentrate but not dissolve the silicon dioxide, so that the fine particle-level intergrowth monomers are dissociated, and the solvent inhibitor interrupts the continuous chemical reaction of the acid-dissolved silicon, so that the silicon dioxide of the intergrowth before the monomer dissociation is retained in the quartz rough concentrate, so as to improve the yield and purity of the quartz concentrate.
[0109] The following is a specific example description of the first recovery process S3 of the fluorine-containing liquid of the present invention.
[0110] about Figure 1 S31, the precipitant IV used in the precipitation IV step S31 is specifically commercially available concentrated ammonia water. Take the filtrate VI (containing calcium, chloride ions, fluoroboric acid, boric acid) of S24 as the fluorine-containing liquid and enter the precipitation IV step S31 for production. It includes: under stirring, first add the precipitant IV at a flow rate of 50L / min until the pH in the filtrate VI is ≈ 5, and then add the precipitant IV at a flow rate of 10L / min until the pH of the filtrate VI is ≈ 8.0, the precipitant IV reacts with fluoroboric acid to form ammonium fluoroborate, and ammonium fluoroborate is completely hydrolyzed at pH ≈ 8.0 to form ammonium fluoride, hydrofluoric acid, and boric acid. Ammonium fluoride reacts with hydrofluoric acid and calcium ions to form a calcium fluoride precipitate. After standing for 10 minutes, enter the solid-liquid separation VII (filtration) / rinsing step S32 for production. The concentrated ammonia water used in the precipitant IV of S31 is specifically industrial grade.
[0111] about Figure 1In S32, the product obtained from the precipitation IV step S31 is subjected to solid-liquid separation VII (filtration) / rinsing step S32, which includes: firstly performing solid-liquid separation (filtration) and then rinsing with clean water until the pH of the rinsing water VII after rinsing the filter residue VII is 6-7. After S32 production, the filtrate VII contains boric acid and ammonium chloride, which together with the rinsing water VII is used as the first recovery liquid and enters the alkaline decomposition step S33 for production. The filter residue VII obtained after S32 production is a calcium fluoride product (mainly fine particle grade), and the calcium fluoride content is ≥97%, which meets the requirements of the required industry.
[0112] The chemical reaction equation of the precipitation IV step S31 is as follows:
[0113] NH 4 OH + HCl = NH 4 Cl + H 2 O;
[0114] NH 4 OH + HBF 4 = NH 4 BF 4 + H 2 O;
[0115] NH 4 BF 4 + 3H 2 O = NH 4 F + 3HF + H 3 BO 3 ;
[0116] 2NH 4 F + CaCl 2 =CaF 2 ↓ + 2NH 4 Cl;
[0117] 2HF + CaCl 2 =CaF 2 ↓ + 2HCl;
[0118] Therefore, the purpose of the precipitation IV step S31 is to remove the fluorine ions in the fluorine-containing liquid and solidify it into a calcium fluoride product. Most of the fluorine ions are dissociated from the fine-particle-level quartz / fluorite / calcite intergrowth monomers, and the fluorine substances in the non-fine-particle-level intergrowths are separated in advance in the flotation I step S21 to become fluorite concentrate.
[0119] about Figure 1 The alkali decomposition agent used in the alkali decomposition step S33 is specifically 50% (mass ratio) of calcium hydroxide [Ca(OH) 2The filtrate VII (containing boric acid and ammonium chloride) obtained in S32 and the rinse water VII are used as the first recovery liquid and enter the alkali decomposition step S33 for production. S33 specifically includes: under stirring, adding the calculated volume of the alkali decomposition agent V required to be added at a flow rate of 25L / min, the calculation method is to respectively measure the NH 4 The content of CI and the content of calcium hydroxide in the alkali decomposer V are then 4 The chemical reaction equation and calculation formula of CI and calcium hydroxide are used to calculate NH 4 The volume of alkali decomposition agent V required to be added when CI and calcium hydroxide react completely; after stirring for another ten minutes, enter the distillation step IV S34 for production operation. Heat at 60-80℃ until there is no NH 3 The gas is produced until the calcium hydroxide and ammonium chloride react chemically with the gas (NH 3 ) enters absorption I process S35 for production, and then obtains a high-purity ammonia product solution with analytical grade purity, and the purity reaches the requirements of analytical purity grade reagent products in the chemical industry. In the common knowledge in this field, the purity level of reagents in the chemical industry is divided into five purity levels from high to low: reference grade, superior grade, analytical grade, chemical grade, and industrial grade. The higher the purity, the higher the product price. Products with purity levels of reference grade, superior grade, and analytical grade are generally used for testing, scientific research, and experiments. The chemical reagents and product purities used in industrial production are generally of industrial grade. The purity of the ammonia water used in the example of the present invention is industrial grade, and the purity of the recovered ammonia water can be higher than the industrial grade.
[0120] The chemical reaction equation of the alkali decomposition step S33 is as follows:
[0121] Ca(OH) 2 + 2NH 4 Cl = CaCl 2 + 2NH 3 ↑ + 2H 2 O;
[0122] Therefore, the role of the alkali decomposition step S33 is to recover the ammonia water used in the precipitation IV step S31, and in the preferred example, a higher purity can be achieved.
[0123] about Figure 1The solution distillation temperature of the distillation IV process S34, distillation V process S38, evaporation I process S46 and distillation / evaporation II process S50 is about 60-80°C, and the solution evaporation temperature is about 100°C. The solution temperature in the production operation of other processes can be room temperature. The addition flow rate of various solutions (acid leaching solution / precipitant / neutralizer / alkali decomposition agent) is controlled at 10-50L / min. In the distillation / evaporation process or other processes requiring stirring as described above, the stirring speed can be controlled at 90 rpm.
[0124] about Figure 1 The precipitant used in the precipitation step S36 may be 9 mol / L sulfuric acid (H 2 SO 4 The precipitant V used in the precipitation step S36 is specifically 9 mol / L sulfuric acid (prepared; commercially available sulfuric acid solution: water = 1:1). 3 ) The alkali decomposition liquid produced includes the solution after the filtrate VII reacts completely with calcium hydroxide, and the solution contains CaCl 2 , boric acid, as the second recovered liquid, enters the precipitation V step S36 for production operation. The precipitation V step S36 specifically includes: under stirring, adding the calculated volume of the precipitant V required to be added at a flow rate of 25L / min, the calculation method is to respectively determine the content of Ca ions in the alkaline decomposition liquid and the content of sulfuric acid in the precipitant V, and then calculate the volume of the precipitant V required to be added when the reaction of Ca ions and sulfuric acid is complete according to the chemical reaction equation of Ca ions and sulfuric acid and the calculation formula; let it stand for 10 minutes, and then enter the solid-liquid separation VIII (filtration) / elution step S37 for production. Figure 1 S37 is to first perform solid-liquid separation (filtration) and then rinse with clean water until the pH of the leaching water VIII after leaching the filter residue VIII is 6-7. The filter residue VIII obtained in S37 is a calcium sulfate II product with a calcium sulfate content of ≥97%, which meets the requirements of the required industry. S37 obtains filtrate VIII, which contains hydrochloric acid and boric acid and is used as the third recovery liquid together with the leaching water VIII, and enters the distillation / evaporation V step S38 for production.
[0125] The chemical reaction equation of the precipitation V step S36 is as follows:
[0126] H 2 SO 4 + CaCl 2 = CaSO 4 ↓ + 2HCl;
[0127] Therefore, the main function of the precipitation step S36 is to recover the alkaline decomposition agent (calcium hydroxide) used in the alkaline decomposition step S33, and the hydrochloric acid used in the previous process can also be recovered. The calcium substance separated and decomposed from the intergrowth in the non-weakly magnetic mineral after the acid leaching step S23 is fluorite (calcium fluoride), and the calcium fluoride chemical product generated in the precipitation step IV S31 has been recovered. The calcium substance of the non-intergrowth in the non-weakly magnetic mineral is recovered in the flotation step I S21.
[0128] about Figure 1 S38, the third recovery liquid obtained in S37 is processed, including filtrate VIII (the filtrate VIII contains hydrochloric acid and boric acid) and rinsing water VIII, and the production operation is carried out in the distillation / evaporation V step S38. The distillation operation temperature at the beginning of the distillation / evaporation V operation is 60-80°C. The gas produced at this time is mainly HCl gas. The HCl gas enters the absorption II step S39 and produces a high-purity hydrochloric acid product solution with a purity of analytical grade. Therefore, the hydrochloric acid purity used in the present invention is industrial grade, and the recovered hydrochloric acid purity can be at the analytical grade. When the HCl in the filtrate VIII is completely distilled at 60-80°C, the evaporation temperature is increased to 100°C until the water evaporates to obtain a solid boric acid product with a boric acid content of ≧97%, which meets the requirements of the required industry and can be returned to the acid leaching III step S23 for recycling.
[0129] The weakly magnetic minerals are purified based on the description of the following process, including a second recovery process of the non-fluorine-containing liquid, corresponding to S41 to S50 in the figure.
[0130] about Figure 1 S14, the weak magnetic mineral is subjected to acid leaching I step S14, and the acid leaching solution I used is specifically 1 mol / L hydrochloric acid (preparation; commercial concentrated hydrochloric acid solution: water = 1:11). The weak magnetic minerals (containing biotite and ankerite) obtained after the secondary tailings are processed in the strong magnetic separation production step S11; enter the acid leaching I production step S14, and under stirring, first add the acid leaching solution I at a flow rate of 50L / min until there are no large amounts of bubbles in the solution, and then add the acid leaching solution I at a flow rate of 10L / min until the pH of the solution reaches 1.0. The acid leaching solution I and the (CaCO 3 MgCO 3 , Fe 2 (CO 3 ) 3 ) chemically reacts to generate calcium chloride, magnesium chloride and ferric chloride, which then enter the acid leaching liquid I. Biotite is insoluble in dilute hydrochloric acid and exists in the acid leaching liquid I in solid form.
[0131] about Figure 1In S15, the acid leaching liquid I of S14 is stirred for another 10 minutes and then enters the solid-liquid separation I (filtration) / rinsing production process S15. The solid-liquid separation (filtration) operation is first performed and then rinsed with clean water until the pH of the rinsing water I after rinsing the filter residue I is 6-7. The filtrate I obtained in S15 is the acid leaching liquid I (the filtrate contains calcium, magnesium, iron ions, and HCl) and enters the second recovery production process (S41-S50) together with the rinsing water I as a non-fluorine-containing liquid. Among them, the filter residue I obtained after the solid-liquid separation I (filtration) / rinsing production process S15 is a biotite concentrate product. The biotite content in the example is 94%, ≧90wt%, that is, more than 90% of the total weight of the product is biotite, and the quality meets the requirements of the required industry.
[0132] The chemical reaction equation of the acid leaching I step S14 is as follows:
[0133] CaCO 3 + 2HCl = CaCl 2 + CO 2 ↑ + H 2 O;
[0134] MgCO 3 + 2HCl = MgCl 2 + CO 2 ↑ + H 2 O;
[0135] Fe 2 (CO 3 ) 3 + 6HCl = 2FeCl 3 + 3CO 2 ↑ + 3H 2 O;
[0136] Therefore, the role of the acid leaching step S14 is to dissolve and separate the Fe of weakly magnetic minerals such as biotite and ankerite. +2 , Fe +3 , Ca +2 Mg +2 Metal ions, and the solid obtained in S15 is a biotite concentrate product, without any solid waste; the discharged gas is carbon dioxide, which is an original component in the atmosphere, and there is no gaseous waste. Since weakly magnetic minerals usually do not contain non-magnetic fluorite (calcium fluoride), there will be no continuous chemical reaction of silicon dissolution. After the strong magnetic separation process S11, the yield of biotite concentrate products is relatively high. The main difference between mica and quartz is that the crystal state is different and the silicon content of mica is lower. The content of metal ions such as aluminum, potassium, and calcium is higher than that of quartz. Biotite also contains iron metal ions before becoming a concentrate product. Biotite molecular formula: K(Mg.Fe)3AlSi 3 O10 (F.OH) 2 . Mica molecular formula; K{A n [BSi 3 O 10 ](OH) 2}, A and B in mica can be one or more of aluminum, calcium, sodium, lithium, magnesium, iron, etc. Because the composition of A and B in mica is uncertain, it can only be represented by n. They all belong to aluminosilicate minerals. Quartz molecular formula: SiO 2 It is a silicon oxide mineral, not an aluminum silicate mineral. The mica ore contains a certain amount of impurities such as quartz, feldspar, carbonate, etc. The quartz ore contains a certain amount of impurities such as mica, feldspar, carbonate, etc.
[0137] about Figure 1 In S41, the filtrate I and the rinse water I (the filtrate contains calcium, magnesium, iron ions, and HCl) derived from step S15 are used as non-fluorine-containing liquids to enter the production operation of the oxidation / precipitation I step S41. Under the stirring of S41, the added oxidant is specifically a hydrogen peroxide solution (the amount added; the volume of the filtrate I and the rinse water I: the volume of the commercially available hydrogen peroxide (30%) solution = 100:5). After stirring for 10 minutes in S41, the added hydrogen peroxide can oxidize the positive divalent iron ions to positive trivalent iron ions. First, add the precipitant I at a flow rate of 50L / min until the pH value of the acid leaching solution I derived from S14 reaches pH 5.0, and then add the precipitant I at a flow rate of 10L / min until the pH of the filtrate I reaches pH 7.0. At this time, the iron ions are completely hydrolyzed to obtain iron hydroxide precipitates and exist in the filtrate I in a solid form, and then stand for ten minutes. The oxidant used in the oxidation / precipitation I step S41 is specifically a commercially available hydrogen peroxide (30%) solution, and the precipitant I used in the oxidation / precipitation I step S41 is specifically 5 mol / L sodium hydroxide (NaOH) (preparation; commercially available sodium hydroxide solid: water = 20:100).
[0138] about Figure 1 S42, and then the pH7.0 filtrate I of S41 enters the solid-liquid separation II (filtration) / rinsing production process S42 to first perform solid-liquid separation (filtration) and then rinse with clean water until the pH of the rinsing water II after rinsing the filter residue II is 6-7. The filtrate II obtained from S42 (the filtrate contains calcium, magnesium ions, and sodium chloride) and the rinsing water II enter the precipitation II process S43 for production. The filter residue II obtained from S42 is an iron hydroxide product. The iron hydroxide content in the example is 98%, ≧90wt%, that is, more than 90% of the total weight of the product is iron hydroxide, and the quality meets the requirements of the required industry, and can be further used to produce iron red pigment or metallic iron powder.
[0139] The chemical reaction equation of the oxidation / precipitation I step S41 is as follows:
[0140] H 2 O 2 + 2Fe 2+ + 2H + = 2Fe 3+ + 2H 2 O;
[0141] NaOH + HCl = NaCl + H 2 O;
[0142] Fe 3+ + 3OH - = Fe(OH) 3 ↓;
[0143] Therefore, the function of the oxidation / precipitation step S41 is to oxidize the iron ions and neutralize the hydrochloric acid to precipitate to obtain the iron hydroxide product, and separate the iron ions from the calcium, magnesium and sodium ions, wherein the sodium ions are provided by the precipitant I.
[0144] about Figure 1 In S43, the filtrate II and rinse water II of S42 are put into the precipitation II step S43 for production operation. Under stirring, the precipitant II is first added at a flow rate of 50L / min until the pH value of the filtrate II of S42 is ≈11, and then the precipitant II is added at a flow rate of 10L / min until the pH of the filtrate II is ≈12.5. At this time, the calcium and magnesium ions will be completely hydrolyzed at pH = 12.5 to form a precipitation mixture (calcium hydroxide, magnesium hydroxide) and exist in the filtrate II in solid form. The precipitant II used in the precipitation II step S43 is also specifically 5mol / L sodium hydroxide.
[0145] about Figure 1 S44, the filtrate II obtained in S43 enters the solid-liquid separation III (filtration) / rinsing step S44 for production, firstly performs solid-liquid separation (filtration) operation and then rinses with clean water until the pH of the rinsing water III after rinsing the filter residue III is 6-7. The filter residue III obtained in S44 contains a precipitated mixture of calcium hydroxide and magnesium hydroxide, which enters the acid dissolution step S47 for production operation. The filtrate III obtained in S44 contains sodium chloride and sodium hydroxide, which enters the neutralization step S45 for production together with the rinsing water III of S44.
[0146] The chemical reaction equation of the precipitation II step S43 is as follows:
[0147] Ca 2+ + 2OH - = Ca(OH) 2 ↓;
[0148] Mg 2+ + 2OH- = Mg(OH) 2 ↓;
[0149] Therefore, the function of the precipitation II step S43 is to precipitate calcium and magnesium ions to achieve the separation effect from sodium ions.
[0150] about Figure 1 In S45, the filtrate III and the rinse water III derived from S44 are put into the neutralization process S45 for production operation. Under stirring, the neutralizer is first added at a flow rate of 50L / min until the pH value of the filtrate III is ≈9, and then the neutralizer is added at a flow rate of 10L / min until the pH value of the solution is ≈7.0. Then the evaporation process I S46 is entered to evaporate the water to obtain the sodium chloride product, and the sodium chloride content is ≧97%, and the quality meets the requirements of the required industry. The neutralizer used in the neutralization process S45 is specifically 1mol / L hydrochloric acid (prepared; commercial concentrated hydrochloric acid solution: water = 1:11).
[0151] The chemical reaction equation of the neutralization step S45 is as follows:
[0152] NaOH + HCl = NaCl + H 2 O;
[0153] Therefore, the function of the neutralization step S45 is to neutralize the sodium ions separated from the calcium and magnesium ions with acid and alkali and evaporate and purify them to obtain a sodium chloride product without gas, liquid or solid waste.
[0154] about Figure 1 In S47, the filter residue III of S44, such as the precipitated mixture of calcium hydroxide and magnesium hydroxide, enters the acid dissolution process S47 for production operation. Under stirring, the acid dissolving agent is first added at a flow rate of 50L / min until the pH value of the filtrate III is ≈5, and then the acid dissolving agent is added at a flow rate of 10L / min until the pH value of the acid solution is ≈7.0. The acid dissolving agent reacts chemically with the precipitated mixture of calcium hydroxide and magnesium hydroxide to generate calcium chloride and magnesium chloride that are easily soluble in water and enter the acid solution. The acid solution enters the precipitation III process S48 for production. The acid dissolving agent used in the acid dissolution process S47 is specifically 1mol / L hydrochloric acid (prepared; commercial concentrated hydrochloric acid solution: water = 1:11).
[0155] The chemical reaction equation of the acid dissolution step S47 is as follows:
[0156] Ca(OH) 2 + 2HCl = CaCl 2 + 2H 2 O;
[0157] Mg(OH) 2 + 2HCl = MgCl2 +2H 2 O;
[0158] Therefore, the function of the acid dissolution step S47 is to dissolve the precipitate containing calcium and magnesium ions to facilitate subsequent separation.
[0159] about Figure 1 S48, the acid solution of S47 enters the precipitation III step S48 for production operation. Under stirring, add the calculated volume of precipitant III to be added at a flow rate of 25L / min. The calculation method is to respectively determine the content of Ca and Mg ions in the acid solution and the content of sulfuric acid in the precipitant III. Then, according to the chemical reaction equation of Ca, Mg ions and sulfuric acid and the calculation formula. Calculate the volume of precipitant III required to be added when Ca, Mg and sulfuric acid react completely. The precipitant III used in the precipitation III step S48 is completely different from the precipitant II used in the precipitation II step S44. The precipitant III is exemplified as sulfuric acid. The precipitant III used in the precipitation III step S48 is specifically 9mol / L sulfuric acid (prepared; commercially available sulfuric acid solution: water = 1:1). Precipitant III (sulfuric acid) reacts chemically with the acid solution containing calcium chloride and magnesium chloride to generate calcium sulfate, magnesium sulfate, and hydrochloric acid. Calcium sulfate is insoluble in water and exists in the acid solution in solid form, while magnesium sulfate is easily soluble in water and enters the acid solution.
[0160] The chemical reaction equation of the precipitation III step S48 is as follows:
[0161] CaCl 2 + H 2 SO 4 = CaSO 4 ↓ + HCl;
[0162] MgCl 2 + H 2 SO 4 =MgSO 4(aq) + HCl;
[0163] Therefore, the function of the precipitation III step S48 is to separate and precipitate the calcium sulfate product obtained in S49 from the solution of sodium and magnesium ions by acid displacement.
[0164] about Figure 1 S49, the acid solution containing dissolved magnesium sulfate and precipitated calcium sulfate obtained in S48 enters the solid-liquid separation IV (filtration) / rinsing step S49 for production, firstly performs solid-liquid separation (filtration) operation and then rinses with clean water until the pH value of the rinsing water IV after rinsing the filter residue IV is 6-7, and the obtained filter residue IV is the calcium sulfate I product with a calcium sulfate content of ≧97%, and the quality meets the requirements of the required industry.
[0165] about Figure 1 S50, the filtrate IV obtained in S49 (containing magnesium sulfate) and the rinse water IV are put into the distillation / evaporation II process S50 for production operation. Specifically, it includes: firstly distillation operation at 60-80℃, the gas produced by distillation is HCl, which enters the absorption II process S39 for production, and after absorption, a high-purity hydrochloric acid solution is obtained, and its purity meets the requirements of analytical grade reagent products in the chemical industry. When all the HCl in the filtrate IV of S49 is distilled at 60-80℃, the evaporation temperature is increased to 100℃ until the water is evaporated to obtain a magnesium sulfate product, and the magnesium sulfate content is ≧97%, which meets the requirements of the required industry. Among them, the purity level of reagents in the chemical industry is divided into five purity levels: benchmark grade, superior grade, analytical grade, chemical grade, and industrial grade. The higher the purity, the higher the price. Purity levels of reference grade, superior grade, and analytical grade are generally used for testing, scientific research, and experiments; the chemical reagents and product purity used in the industrial production of this application are generally industrial grade. Specifically, the hydrochloric acid purity used in the examples of the present invention is industrial grade, and the purity of the recovered hydrochloric acid can reach analytical grade. Therefore, cheaper industrial grade hydrochloric acid products can be purchased, and more expensive analytical grade high-purity hydrochloric acid products can be sold. Other reagents added in the process can also have the same effect, such as analytical grade high-purity ammonia products.
[0166] Therefore, the first recovery process S3 of the fluorine-containing liquid in the example of the present invention overlaps with the second recovery process of the non-fluorine-containing liquid in the absorption II step S39, so as to simultaneously recover the high-purity hydrochloric acid product, thereby saving processes and production equipment. In addition, the tailings intergrowth dissociation process S2 in the example of the present invention overlaps with the second recovery process of the non-fluorine-containing liquid in the precipitation III step S48, so as to simultaneously recover the calcium sulfate I product through the solid-liquid separation IV (filtration) / rinsing step S49, recover the magnesium sulfate product through the distillation / evaporation II step S50, and recover the high-purity hydrochloric acid product through the absorption II step S39, thereby saving processes and production equipment.
[0167] Using the process flow of the present invention as described above, 100 kg of secondary tungsten tailings are taken, and the final mineral recovery rate and yield are as follows: Figure 5 As shown in Table 3.
[0168] The calculation of mineral yield and recovery rate is divided into two types: theoretical and practical. The yield described in the present invention refers to the actual yield, that is, the mass of a certain product (such as quartz) obtained is divided by the mass percentage of the secondary tailings. The recovery rate described in the present invention refers to the actual recovery rate, that is, the mass of a certain product (such as quartz) obtained is multiplied by the purity content of silicon dioxide as the numerator, and the mass of the secondary tailings is multiplied by the percentage of pure quartz (100% silicon dioxide) in the secondary tailings (60.5%) as the denominator, and the recovery rate is obtained by dividing. In the calculation of the actual recovery rate, the content of silicon dioxide is obtained by first taking two mineral samples of the quartz concentrate product and the secondary tungsten tailings and then testing them. Therefore, it is very important to take the above two mineral samples and whether the test is representative (authenticity). If there is no representativeness, it will affect the authenticity of the recovery rate. However, in fact, no matter how carefully and seriously you take more samples and test them, the test results cannot reach 100% authenticity.
[0169] Therefore, the yield is calculated by dividing the individual mass of individual products by the input mass of secondary tungsten tailings. The total non-chemical yield of secondary tungsten tailings excluding chemical products is 76.65 wt% (≧70 wt%), and the chemical products obtained by recovering the acid solution after acid dissolution of calcite, ankerite and dolomite have a total chemical yield of 106.64 wt%. This is because the hydroxyl, sulfate, calcium / sodium / chloride ions of each process additive will be added to the individual products and have an impact. Therefore, the total yield of secondary tungsten tailings including chemical products will reach more than 100 wt%.
[0170] Content is also called percentage content, which refers to the ratio of the mass of a certain element or compound (such as silicon dioxide in quartz concentrate products) in a certain mineral (such as secondary tailings) or a certain product (such as quartz concentrate) to the total mass of a certain mineral (such as secondary tailings) or a certain product (such as quartz concentrate). For example, the content of silicon dioxide in quartz concentrate products is 99.60%, which means that in the quartz product, silicon dioxide accounts for 99.60%, and there are 0.4% other substances. Mineral recovery rate refers to the ratio of the mass of a certain element or compound (such as silicon dioxide in quartz concentrate products) in a certain product (such as quartz concentrate) to the mass of pure quartz (100% silicon dioxide) in secondary tailings (60.5%). The quality (content) of an element or compound in the product is inversely proportional to the mineral recovery rate, that is, the higher the quality (content), the lower the mineral recovery rate. When ensuring that the quality (content) meets the quality index requirements, the higher the mineral recovery rate, the better. In other words, the more complete the recovery, the higher the gold content of the production process flow and production process parameters and technology. The mineral recovery rate is the actual recovery rate of the corresponding element. For example, the corresponding element of high-purity quartz concentrate is silicon dioxide. 59.43 kg of high-purity quartz concentrate can be recovered from 100 kg of secondary tungsten tailings. The purity of silicon dioxide in high-purity quartz concentrate is 99.6 wt%, that is, the maximum mass of pure quartz (silicon dioxide content is 100wt%) that can be recovered is 59.43 × 99.6%Kg=59.19Kg, that is, 59.19Kg of pure quartz (silicon dioxide content is 100wt%) is actually recovered. The actual recovery rate is (59.19Kg÷60.5Kg)×100%=97.84%. The proportion (similar to the percentage content) of pure quartz (100wt% silicon dioxide content) in 100kg of secondary tungsten tailings is 60.5wt% (that is, 60.5wt% means that the mass of pure quartz (100wt% silicon dioxide content) in 100kg of secondary tungsten tailings is 60.5Kg). After production and processing, 59.43Kg of high-purity quartz concentrate (99.60wt% silicon dioxide content) is obtained (recovered).
[0171] The (actual) yield and (actual) recovery of high purity quartz concentrate are as follows;
[0172] (Actual) yield: (mass of high-purity quartz concentrate (59.43Kg) ÷ mass of secondary tungsten tailings (Kg)) = (59.43Kg ÷ 100Kg) = 59.43%.
[0173] The (actual) recovery rate is: [(silicon dioxide content of high-purity quartz concentrate (99.60%)) multiplied by (mass of high-purity quartz concentrate (59.43Kg)] divided by [the proportion of pure quartz (silicon dioxide percentage is 100wt%) in secondary tungsten tailings (60.5wt%) multiplied by (mass of secondary tungsten tailings (100Kg))] = (99.60wt% × 59.43Kg) ÷ (60.5wt% × 100Kg) = 97.84%.
[0174] The corresponding elements of biotite concentrate and muscovite concentrate are also silicon dioxide, and the corresponding element of fluorite concentrate is calcium fluoride. The present invention can achieve a mineral recovery rate (%) of more than 85% in high-purity quartz concentrate, biotite concentrate and muscovite concentrate, mainly because the quartz / fluorite / calcite intergrowth that cannot be physically dissociated in fine-grained minerals (≦0.019mm) in the prior art is decomposed and separated.
[0175] The example of the present invention also provides a secondary tungsten tailings purified quartz device, which is used to execute the preparation method of the secondary tungsten tailings purified quartz as described above.
[0176] See also Figure 2 The present invention also provides a quartz device for purifying fluorine-containing solid waste, which can be combined with or referred to the process description of the above example, and the device includes:
[0177] A strong magnetic separation unit 11 is used to separate the iron-containing substances from the fluorine-containing solid waste to obtain non-magnetic fluorine-containing solid waste; the fluorine-containing solid waste is mainly below the fine particle level;
[0178] The acid leaching unit II 12 and the solid-liquid separation unit V 13 are used to dissolve the calcium-containing substances and magnesium-containing substances in the non-magnetic fluorine-containing solid waste to obtain the first fluorine-containing mixed solid waste, wherein the first fluorine-containing mixed solid waste contains a conjoined body of silicon dioxide / calcium fluoride / calcium carbonate without monomer dissociation; in the example, calcite and dolomite are very few and almost non-existent, and contain a little mica / other minerals (feldspar);
[0179] The conjoined body dissociation module 20 is used to dissociate the conjoined bodies at the fine particle level in the first fluorine-containing mixed solid waste; the conjoined body dissociation module 20 comprises:
[0180] The flotation unit I 21 is used to separate calcium fluoride from the first fluorine-containing mixed solid waste to obtain a second mixed solid waste, wherein the second mixed solid waste contains the intertwined bodies; therefore, the non-intertwined body fluorine-containing substances in the fluorine-containing solid waste are first separated and purified, and the interference of the non-intertwined body fluorine-containing substances on the dissociation of the intertwined bodies is eliminated in advance;
[0181] The flotation II unit 22 is used to separate mica from the second mixed solid waste and obtain a third mixed solid waste, wherein the third mixed solid waste contains the intergrowth; and then separate and purify the silicon-containing substances and calcium-containing substances of the non-intergrowth in the fluorine-containing solid waste, and eliminate the interference of the silicon-containing substances and calcium-containing substances of the non-intergrowth or / and other mineral impurities on the dissociation of the intergrowth; and,
[0182] Acid leaching III unit 23 and solid-liquid separation VI unit 24, the acid leaching III unit 23 uses a strong acid and a dissolving agent to dissolve the fluorine-containing substances and calcium-containing substances in the intergrowth of the third mixed solid waste but not dissolve the silicon dioxide, so that the intergrowth monomers are dissociated, the dissolving agent interrupts the continuous chemical reaction of the acid-dissolved silicon, so that the silicon dioxide of the intergrowth before the monomer dissociation is retained in the third mixed solid waste to obtain silicon dioxide, the silicon dioxide is taken from the intergrowth and non-intergrowth in the fluorine-containing solid waste; in the example, calcite and dolomite are very little or almost gone, and contain a little mica / other minerals (feldspar); and,
[0183] The first recovery equipment module 30 for fluorine-containing liquid recovers the fluorine-containing liquid dissolved by the acid leaching III unit 23 and separated by the solid-liquid separation VI unit 24 to obtain chemical products to eliminate gas-liquid-solid three-state waste; the first recovery equipment module 30 specifically includes a precipitation IV unit 31, a solid-liquid separation VII unit 32, an alkali decomposition unit 33, a distillation IV unit 34, an absorption I unit 35, a precipitation V unit 36, a solid-liquid separation VIII unit 37, a distillation V unit 38, and an absorption II unit 39 corresponding to the above process numbers. The chemical products specifically include separated and purified calcium fluoride products, high-purity ammonia products, CaSO 4 products, boric acid products and high purity hydrochloric acid products.
[0184] The fluorine-containing solid waste is specifically selected from any one of wet pyrometallurgical smelting slag, smoke and flue gas sediment, waste water and waste acid precipitate, fluorine-containing minerals and secondary tungsten tailings.
[0185] Regarding the acid leaching II unit 12, the aforementioned calcium carbonate in the silicon dioxide / calcium fluoride / calcium carbonate intergrowth without monomer dissociation is a broad definition, specifically mica and a very small amount of other minerals, and only a trace amount of calcium carbonate is also included. The calcium carbonate in the silicon dioxide / calcium fluoride / calcium carbonate intergrowth without monomer dissociation can specifically include calcite (chemical name is calcium carbonate, molecular formula: CaCO 3 ), or may include dolomite (molecular formula: CaCO 3 MgCO 3 ). The chemical name of fluorite is calcium fluoride, and its molecular formula is: CaF 2The purpose of the acid leaching II operation of the acid leaching II unit 12 is to dissolve calcite (calcium carbonate) and dolomite (calcium carbonate and magnesium carbonate) as much as possible and enter the acid leaching agent in the form of calcium / magnesium ions to achieve the purpose of separation from the intergrowth (silicon dioxide / calcium fluoride / mica / other minerals).
[0186] Regarding the acid leaching III unit 23, when the third mixed solid waste contains mica / feldspar, it will also be dissolved.
[0187] In addition, the present invention further studies the silicon dissolving agent as follows:
[0188] Hydrofluoric acid can react chemically with quartz and silicon dioxide in aluminum silicate minerals (such as mica, feldspar, etc.) to produce fluorosilicic acid.
[0189] Related chemical reaction equations;
[0190] 6HF+SiO 2 =H 2 SiF 6 +2H 2 O
[0191] 4HF+SiO 2 =SiF 4 +2H 2 O
[0192] 3SiF 4 +3H 2 O=2H 2 SiF 6 +2H 2 SiO 3
[0193] SiF 4 +3H 2 O=H 2 SiO 3 +4HF
[0194] H 2 SiF 6 =SiF 4 +2HF
[0195] H 2 SiO 3 =SiO 2 ·H 2 O↓
[0196] Some minerals and tailings contain fluorine-containing minerals (such as fluorite, fluorapatite, etc.), and fluorine-containing solid wastes (such as hydrometallurgical slag, smoke and flue gas sediments, wastewater and waste acid sediments, etc.) also contain fluorine-containing substances. And it also contains a certain amount or even a large amount of substances such as silicon dioxide. Fluorite, fluorapatite, and fluorine-containing substances will react chemically with strong acids to produce hydrofluoric acid (HF). Therefore, when there are fluorine-containing substances (such as fluorite, fluorapatite, fluoride salts) in some (minerals, tailings, solid wastes), it is impossible to use strong acid decomposition methods or strong acid selective acid leaching methods to separate fluorine-containing minerals (or fluorine-containing substances) from quartz (or silicon dioxide). Moreover, the solution obtained after treatment with strong acid decomposition methods and strong acid selective acid leaching methods contains fluorosilicic acid and fluorosilicates. It increases the difficulty of treatment and recycling, and even makes it impossible to treat and recycle. It increases production costs and even makes it impossible to produce in serious cases. This patent adds a dissolution inhibitor (boric acid) to a strong acid, so that the hydrofluoric acid generated by the reaction of fluorine-containing minerals and fluorine-containing substances in (minerals, tailings, solid waste) with the strong acid preferentially reacts with the dissolution inhibitor [boric acid (H3BO3)] to generate [fluoroboric acid (HBF 4 )]. Moreover, the dissolvent (boric acid) can be reused after recovery. Under the conditions of (hydrofluoric acid concentration of 6-10%, acid leaching temperature of 40-70℃, acid leaching time of 20-40min, dissolvent concentration range of 7.5-12.5%, solid-liquid ratio range of 1.0:1.0-1.0:1.4%), fluoroboric acid does not react chemically with quartz (silicon dioxide) and is not dissolved. However, aluminosilicate (mica, feldspar) minerals will react chemically and a small amount will be dissolved.
[0197] Chemical reaction equation:
[0198] 4HF+H 3 BO 3 =HBF 3 OH+HF+2H 2 O
[0199] HBF 3 OH+HF=HBF 4 +H 2 O
[0200] The concentration of hydrofluoric acid is 20% in volume ratio. The preparation method is: commercial concentrated hydrofluoric acid (40% mass ratio): water = 1:4. When the concentration of hydrofluoric acid is 20% (volume ratio), the converted mass ratio is 8%.
[0201] Acid leaching principle:
[0202] The hydrochloric acid (HCl) and calcium fluoride (CaF 2 ) reacts to form hydrofluoric acid (HF). 3 BO3 ) to generate fluoroboric acid (HBF 4 ). The coordination (complexation) ability of fluorine with boron is stronger than that of fluorine with silicon. When fluorine, boron and silicon are present in the reaction system, fluorine first reacts with boron to form fluoroboric acid instead of reacting with silicon to form hydrofluoric acid.
[0203] When there is no boric acid in the acid leaching agent, the hydrofluoric acid generated by the reaction of hydrochloric acid in the acid leaching agent with calcium fluoride reacts with silicon dioxide to form silicon tetrafluoride (SiF 4 ), silicon tetrafluoride reacts with water vapor (H 2 O) and hot water (H 2 O) to generate fluorosilicic acid (H 2 SiF 6 ) and metasilicic acid (H 2 SiO 3 ) and metasilicic acid and hydrofluoric acid. Fluorosilicic acid decomposes into silicon tetrafluoride and hydrofluoric acid at a certain temperature (the higher the temperature, the faster the reaction speed), and hydrofluoric acid reacts with silicon dioxide to form silicon tetrafluoride, which reacts with water vapor and hot water to form fluosilicic acid and metasilicic acid as well as metasilicic acid and hydrofluoric acid. Hydrofluoric acid and silicon tetrafluoride are volatile, but because acid leaching is carried out in a closed acid leaching device, hydrofluoric acid and silicon tetrafluoride evaporate to the inner wall of the closed acid leaching device and adhere to the inner wall, and react with water vapor attached to the inner wall to obtain fluosilicic acid and hydrofluoric acid liquid, which flows back to the acid leaching agent under the action of gravity and reacts with silicon dioxide again.
[0204] Example:
[0205] After 500kg of quartz is mixed evenly, samples are taken for mineral phase and element analysis. The mineral phase and element content are shown in the corresponding Figure 6 Table 4. As can be seen from Table 4, the yield of muscovite in the quartz mineral used in the embodiment is 1%, and the yield of quartz is 99%. 500kg quartz mineral (SiO 2: 99.74%), under the production process parameters of [hydrofluoric acid concentration 8% (mass ratio), boric acid concentration 10% (mass ratio), temperature 50°C, reaction time 30min, solid-liquid ratio 1:1, stirring speed 90 rpm], 1.1 kg of quartz was dissolved after acid leaching, with a dissolution rate of 0.22%. Quartz mineral (SiO 2 :99.74%), the yield of muscovite in the quartz is 1%, that is, the muscovite is 5Kg, so what is actually dissolved by fluoroboric acid is muscovite, not quartz, and quartz is not dissolved by fluoroboric acid.
[0206] Process parameter range selection:
[0207] The silica content of the quartz mineral sample used in the test is 99.74%, and the mineral composition of the quartz mineral sample is 99% quartz and 1% muscovite. The price of pure quartz samples with a silica content of 99.99% is relatively expensive, so the quartz sample used in the test is a quartz sample with a silica content of 99.74% instead of a pure quartz sample. In the quartz sample with a silica content of 99.74%, the muscovite yield accounts for 1% and the quartz yield accounts for 99%.
[0208] Hydrofluoric acid concentration (fluoroboric acid) selection:
[0209] Under the production process parameters (boric acid concentration 10% (mass ratio), temperature 50℃, reaction time 30min, solid-liquid ratio 1:1, stirring speed 90 rpm), when the hydrofluoric acid concentration (mass ratio) is changed, the dissolution rate of quartz with and without the addition of a dissolving agent is shown in the corresponding Figure 7 Table 5. The silicon dioxide content of the quartz mineral sample used in the test is 99.74%.
[0210] According to the data in Table 5, it can be judged that;
[0211] ① When the dissolution inhibitor (10%) is added, the dissolution rate of quartz is very low (0.09%-0.39%) when the hydrofluoric acid concentration is 0.8%-11.2%, and it starts to rise significantly when it is greater than 11.2%. The concentration of hydrofluoric acid in the acid leaching agent is proportional to the calcium fluoride content in the solid in the acid leaching pulp. In the present invention, according to the data in Table 5 and the subsequent table, the concentration range of hydrofluoric acid in the acid leaching agent can be selected to be 6-11%. The optimal concentration range is 8%, and when the concentration of hydrofluoric acid is 8.0%, the concentration of fluoroboric acid is equivalent to 2.0%.
[0212] When the mass of boric acid (dissolution inhibitor) in 1L of acid leaching solution is 100g, and 100g of boric acid reacts completely with 1L of hydrofluoric acid solution, the concentration of 1L of hydrofluoric acid solution required is 11.25%.
[0213] ② Without adding a dissolution inhibitor, when the hydrofluoric acid concentration is less than 0.8%, the dissolution rate of quartz is as low as 1.71%, but it is still much higher than 0.39% [dissolution inhibitor (10%), hydrofluoric acid concentration 11.2%. When it is greater than 0.8%, it begins to rise significantly.
[0214] The reason is as follows: the coordination (complexation) ability of fluorine with boron is stronger than that of fluorine with silicon. When fluorine, boron and silicon are present in the reaction system, fluorine first reacts with boron to form fluoroboric acid instead of reacting with silicon to form hydrofluoric acid.
[0215] About acid leaching temperature selection:
[0216] S23 under the production process parameters of hydrofluoric acid concentration 8% (mass ratio), boric acid concentration 10% (mass ratio), reaction time 30min, solid-liquid ratio 1:1, stirring speed 90 rpm, when the acid leaching temperature conditions are changed, the dissolution rate of quartz with and without adding the inhibitor is shown in the corresponding Figure 8 Table 6.
[0217] According to the data in Table 6, it can be judged that:
[0218] ① When the dissolution inhibitor (10%) is added, the dissolution rate of quartz is very low (0.05%-0.345%) when the acid leaching temperature is 10-70°C, and it begins to rise significantly when the temperature is greater than 60°C. In this patent, according to the data in Table 6, Table 10 and Table 11, the acid leaching temperature can be selected to be 40-70°C, and the optimal range is 50°C;
[0219] ② Without adding a solvent inhibitor, when the acid leaching temperature is 10°C, the dissolution rate of quartz has reached 5.61%, which is much higher than 0.33% [adding a solvent inhibitor (10%), and the acid leaching temperature is 60°C];
[0220] The reason is as follows: the coordination (complexation) ability of fluorine with boron is stronger than that of fluorine with silicon. When fluorine, boron and silicon are present in the reaction system, fluorine first reacts with boron to form fluoroboric acid instead of reacting with silicon to form hydrofluoric acid.
[0221] Acid leaching reaction time selection:
[0222] Under the production process parameters (hydrofluoric acid concentration 8% (mass ratio), boric acid concentration 10% (mass ratio), temperature 50℃, solid-liquid ratio 1:1, stirring speed 90 rpm), when the acid leaching reaction time conditions are changed, the dissolution rate of quartz with and without the addition of a solvent inhibitor is shown in the corresponding Fig. 9 Table 7.
[0223] According to the data in Table 7, it can be judged that:
[0224] ① When the solvent inhibitor (10%) is added, the dissolution rate of quartz is very low (0.38%) when the acid leaching time is 5-80 minutes, and it begins to rise significantly when the temperature is greater than 70°C. In this patent, the acid leaching temperature can be selected from 20-70 minutes according to the data in Table 7 and Table 10, and the optimal range is 30 minutes;
[0225] ② Without adding a solvent inhibitor, the dissolution rate of quartz reached 9.59% when the acid leaching time was 5 minutes, which was much higher than 0.39% [adding a solvent inhibitor (10%) and the acid leaching temperature was 80 minutes];
[0226] The reason is as follows: the coordination (complexation) ability of fluorine with boron is stronger than that of fluorine with silicon. When fluorine, boron and silicon are present in the reaction system, fluorine first reacts with boron to form fluoroboric acid instead of reacting with silicon to form hydrofluoric acid.
[0227] Boric acid (solvent inhibitor) concentration selection:
[0228] Under the production process parameters (hydrofluoric acid concentration 8% (mass ratio), time 30min, temperature 50℃, solid-liquid ratio 1:1, stirring speed 90 rpm), when the concentration of boric acid (dissolving agent) is changed, the dissolution rate of quartz with and without adding dissolving agent % is shown below: Fig.10 Table 8.
[0229] According to the data in Table 8, it can be judged that:
[0230] ① When the dissolution inhibitor concentration is 7.5-12.5%, the dissolution rate of quartz is very low (0.26-0.185%). When the dissolution inhibitor concentration is greater than 12.5%, the dissolution rate of quartz (0.18%) remains unchanged. When the dissolution inhibitor concentration is less than 7.5%, the dissolution rate of quartz increases. In the present invention, the dissolution inhibitor concentration range can be selected to be 7.5-12.5% according to the data in Tables 8, 10 and 11. The optimal range is 10%;
[0231] (In 1L of acid leaching solution, the amount of boric acid (inhibiting agent) is 100g (10%). When 100g of boric acid reacts completely with 1L of hydrofluoric acid solution, the concentration of the required 1L of hydrofluoric acid solution is 11.25%).
[0232] ② Without adding a solvent inhibitor, the dissolution rate of quartz reaches 23.53%, which is much higher than 4.73% [with the addition of a solvent inhibitor (2.5%)];
[0233] The reason is as follows: the coordination (complexation) ability of fluorine with boron is stronger than that of fluorine with silicon. When fluorine, boron and silicon are present in the reaction system, fluorine first reacts with boron to form fluoroboric acid instead of reacting with silicon to form hydrofluoric acid.
[0234] Selection of acid leaching solid-liquid ratio conditions:
[0235] Under the production process parameters (hydrofluoric acid concentration 8% (mass ratio), time 30min, temperature 50℃, boric acid (10%), solid-liquid ratio 1:1, stirring speed 90 rpm), when the solid-liquid ratio conditions are changed, the dissolution rate of quartz with and without the addition of a dissolving agent is shown in the corresponding Fig.11 Table 9.
[0236] According to the data in Table 9, it can be judged that;
[0237] ① When the solid-liquid ratio (mass ratio) is 1:0.8-1:3.0, the dissolution rate of quartz is very low (0.183-0.285%), but when the solid-liquid ratio (mass ratio) is 1:0.8, it is not conducive to stirring and increases the difficulty of stirring. When the solid-liquid ratio (mass ratio) is large, the single batch processing volume is reduced, and the processing production cost will also increase. In this patent, according to the data in Table 2, the solid-liquid ratio range can be selected as 1.0:1.0-1.0:1.4%;
[0238] ② Without adding a dissolution inhibitor, when the solid-liquid ratio (mass ratio) is 1:0.8, the dissolution rate of quartz has reached 19.24%, which is much greater than 0.285% [solid-liquid ratio 1:3.0];
[0239] The reason is as follows: the coordination (complexation) ability of fluorine with boron is stronger than that of fluorine with silicon. When fluorine, boron and silicon are present in the reaction system, fluorine first reacts with boron to form fluoroboric acid instead of reacting with silicon to form hydrofluoric acid.
[0240] The time required for calcium fluoride to be completely dissolved by the acid leaching agent (different volumes, concentrations and temperatures):
[0241] Under the same production process parameters (hydrochloric acid concentration (4-6mol / L), temperature 30-80℃, boric acid (10%), solid-liquid ratio (mass ratio) 1.0:1.0, stirring speed 90 rpm), when the calcium fluoride quality conditions are changed, the time (min) required for calcium fluoride to be completely dissolved by the acid leaching agent is shown in the corresponding Fig.12 Table 10. When the solid-liquid ratio (mass ratio) is 1.0:1.0, the mass of calcium fluoride added is 10g, 20g, and 30g, respectively, and the corresponding calcium fluoride content in the solid of the acid leaching pulp is 1%, 2%, and 3%, respectively.
[0242] The solubility of boric acid at different temperatures is shown in the corresponding Fig.13 According to the data in Table 11, we can know that:
[0243] At 50℃, the solubility of boric acid in 1L aqueous solution is 115.4g, that is, the solubility of boric acid in 1L aqueous solution is 11.54g / %, and the boric acid added in 1L acid leaching agent is 100g (concentration 10%). When the temperature of 1L acid leaching agent is lower than about 42℃-43℃, the boric acid will not be completely dissolved. Therefore, when the boric acid in 1L acid leaching agent is 100g (concentration 10%), the temperature of the acid leaching agent should be greater than 40℃ during the acid leaching operation. However, the higher the temperature, the higher the production cost. According to the data in the table, the optimal temperature of the acid leaching agent can be selected as 50℃.
[0244] According to the data in Table 11, it can be judged that:
[0245] ① When the concentration of the acid leaching agent is [HCl (4 mol / L, 6 mol / L)] and the temperature is 50°C, the greater the solid-liquid ratio (mass ratio), the shorter the time required for the calcium fluoride to be completely dissolved, and the more calcium fluoride can be dissolved. However, when the solid-liquid ratio (mass ratio) is larger, the single batch processing volume decreases, which increases the processing production cost. Therefore, the selection criterion for the solid-liquid ratio is to select according to the content of calcium fluoride in the solids in the acid leaching slurry when other conditions remain unchanged. In this patent, according to the data in Tables 9 and 10, the solid-liquid ratio range can be selected as 1:1.0-1.0:1.4;
[0246] ② When the temperature is 50°C and the solid-liquid ratio remains unchanged, the higher the concentration of the acid leaching agent, the shorter the time required for the calcium fluoride to be completely dissolved, and the more calcium fluoride can be dissolved. However, the higher the concentration of the acid leaching agent (when the concentration of hydrochloric acid is greater than 5 mol / L, the volatility increases sharply), the stronger the volatility, which has an impact on the environment and human body. It is highly corrosive to the equipment, and the performance and corrosion protection requirements of the equipment are higher. Increase the investment in production equipment and production costs. In the present invention, according to the data in Table 5 and Table 10, the concentration range of hydrochloric acid in the acid leaching agent can be selected to be 3-5 mol / L, and the optimal concentration range is 4 mol / L;
[0247] ③ When the concentration of the acid leaching agent is [HCl (4 mol / L], the solid-liquid ratio (mass ratio) is 1.0: 1.0, and the temperature is 50 ° C. When the temperature is less than 50 ° C, the lower the temperature, the longer the time required for the calcium fluoride to be completely dissolved, and the smaller the mass of the calcium fluoride that can be dissolved. When the temperature is greater than 60 ° C, the higher the temperature, the longer the time required for the calcium fluoride to be completely dissolved, and the smaller the mass of the calcium fluoride that can be dissolved. This is because hydrochloric acid, hydrofluoric acid, and fluoroboric acid are volatile. The higher the temperature, the more volatile they are, which reduces the concentration of hydrochloric acid, hydrofluoric acid, and fluoroboric acid in the acid leaching agent. The higher the temperature, the faster the speed at which the concentration of hydrochloric acid, hydrofluoric acid, and fluoroboric acid in the acid leaching agent decreases. And the higher the temperature, the greater the production cost. In the present invention. According to the data in the table, the acid leaching temperature can be selected to be in the range of 40-60 ° C. The optimal temperature is 50 ° C.
[0248] Fluoroboric acid dissolves quartz:
[0249] Under the conditions of quartz purity 99.74%, temperature 10-70℃, reaction time 10-70min, solid-liquid ratio 1.0:0.8-1.0:2.0, stirring speed 90 rpm, fluoroboric acid concentration 0.5-4.0%, when one of the conditions is changed, the dissolution rate of quartz is shown in the corresponding Fig.14Table 12. When the concentration of boric acid in the acid leaching agent is greater than the concentration required for the complete reaction of boric acid and hydrofluoric acid, the concentration of fluoroboric acid is 25% of the concentration of fluorosilicic acid. That is, when the concentration of hydrofluoric acid is 8% and reacts completely with boric acid of sufficient concentration, the concentration of fluoroboric acid generated is 2%.
[0250] Chemical reaction equations;
[0251] 4HF+H 3 BO 3 =HBF 4 +3H 2 O.
[0252] According to the data in Table 12, it can be judged that:
[0253] ① When the concentration of fluoroboric acid is 1-6%, the dissolution rate of quartz mineral is very low (0.442%) when the reaction time (maximum time is 80min), temperature (maximum temperature is 80℃), and solid-liquid ratio (maximum ratio is 1.0:3.0) are changed respectively. When the concentration of fluoroboric acid is greater than 6%, quartz begins to be slowly dissolved by fluoroboric acid (dissolution rate is 0.890%).
[0254] ② The quartz (SiO 2 The content is 99.74%). When the concentration of fluoroboric acid is 6%, a small amount of it dissolves (the dissolution rate is 0.495%). However, according to Table 13 (corresponding to Fig.15 ) and Table 14 (corresponding Fig.16 ) can be judged from the data in the experiment; the dissolved mineral is mica (the quartz content of the quartz mineral used in the experiment is 99%, the muscovite content is 1%, and the molecular formula of muscovite is KAl 2 (AlSi 3 O 10 )(OH) 2 , SiO in muscovite 2 Content is 45%) instead of quartz, so quartz (SiO 2 ) is not dissolved by fluoroboric acid under the conditions of (temperature 50°C, fluoroboric acid concentration 6%, reaction time 30 min, solid-liquid ratio (1.0:1.0), fluoroboric acid concentration less than 6%);
[0255] The reason is as follows: the coordination (complexation) ability of fluorine with boron is stronger than that of fluorine with silicon. When fluorine, boron and silicon are present in the reaction system, fluorine first reacts with boron to form fluoroboric acid instead of reacting with silicon to form hydrofluoric acid.
[0256] Experimental verification that fluoroboric acid does not dissolve quartz:
[0257] The silicon dioxide content of two different quartz samples of 500g each was 99.99% and 99.74% respectively. Under the same conditions (temperature 90℃, reaction time 80min, solid-liquid ratio 1.0:3.0), the concentration of fluoroboric acid was changed. The dissolution rate test of quartz was carried out at the same time. See the corresponding Fig.15 Table 13.
[0258] From the data in Table 13, we can judge that:
[0259] ① The quartz with a silicon dioxide content of 99.99% used in the test was not dissolved by fluoroboric acid under the conditions of (temperature 90°C, reaction time 80min, solid-liquid ratio 1.0:3.0mL, fluoroboric acid concentration 6%). When the fluoroboric acid concentration was greater than 6%, the quartz began to be slowly dissolved by fluoroboric acid;
[0260] ② The quartz with a silicon dioxide content of 99.74% used in the test was slowly dissolved by fluoboric acid under the conditions of (temperature 90°C, reaction time 80min, solid-liquid ratio 1.0:3.0mL, fluoboric acid concentration 6%), and the dissolution rate was very low (0.180%-0.591%). When the fluoboric acid concentration was greater than 6%, the dissolution rate began to increase.
[0261] Experimental verification of fluoroboric acid dissolving mica and feldspar:
[0262] 500g of mica (purity greater than 99%) and feldspar (purity greater than 99%) were added under the conditions of (temperature 90℃, reaction time 80min, solid-liquid ratio 1.0:3.0), and the concentration of fluoroboric acid was changed. The dissolution rates of mica and feldspar were shown in the corresponding Fig.16 Table 14.
[0263] It can be judged from the data in Table 14 that a small amount of mica and feldspar used in the test were dissolved by fluoboric acid under the conditions of temperature 90°C, fluoboric acid concentration 1%, reaction time 80 min, and solid-liquid ratio (1.0:3.0), and the dissolution rates were (1.18%, 1.10%). When the fluoboric acid concentration was greater than 2%, the speed at which mica and feldspar were dissolved by fluoboric acid accelerated, and the dissolution rate began to increase.
[0264] From Table 13 (corresponding Fig.15 ) and Table 14 (corresponding Fig.16 ) can be used to determine:
[0265] ① Quartz with a silicon dioxide content of 99.99% is not dissolved by fluoroboric acid under the conditions of (temperature 90°C, reaction time 80 min, solid-liquid ratio 1.0:3.0 mL, fluoroboric acid concentration 6%);
[0266] ② Quartz with a silicon dioxide content of 99.74% was slowly dissolved by fluoroboric acid under the conditions of (temperature 90°C, reaction time 80min, solid-liquid ratio 1.0:3.0mL, fluoroboric acid concentration 6%), and the dissolution rate was very low (0.591%), but the mineral dissolved was mica instead of quartz. This is because quartz (SiO 2 The content is 99.74%), which contains about 1% muscovite, [muscovite molecular formula; K[Al 2 (AlSi 3 O 10 ](OH) 2 , SiO 2 Content is 45%];
[0267] ③Selection of process parameter range:
[0268] The concentration of hydrofluoric acid in the acid leaching agent used in S23 ranges from 6-11%. The optimal range is 8%. The equivalent concentration of fluosilicic acid is 2%;
[0269] Acid leaching temperature is 40-70℃, the optimum value is 50℃;
[0270] Acid leaching temperature is 20-70min, the optimum value is 30min;
[0271] The optimal concentration range of the inhibitor is 7.5-12.5%, and the middle value of the optimal range is 10%;
[0272] The solid-liquid ratio ranges from 1.0:1.0 to 1.0:1.4, with the optimum value being 1.0:1.0;
[0273] The concentration range of hydrochloric acid in the acid leaching agent is 3-5 mol / L, and the middle value of the optimal range is 4 mol / L.
[0274] The embodiments of this specific implementation method are all preferred embodiments for facilitating the understanding or implementation of the technical solutions of the present invention, and are not intended to limit the protection scope of the present invention. All equivalent changes made based on the structure, shape, and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing quartz purified from secondary tungsten tailings, characterized in that: include: S11, performing a strong magnetic separation process on the secondary tungsten tailings to separate the iron-containing substances in the secondary tungsten tailings to obtain separated non-weakly magnetic minerals and weakly magnetic minerals; the secondary tungsten tailings are the secondary tailings after the primary tailings of the quartz vein type tungsten ore are processed and purified to recover the useful minerals, and are a kind of fluorine-containing solid waste, most of which are fine particles, and a small part of the fine particles are still intergrown without monomer dissociation between the minerals; S12 and S13, subjecting the non-weakly magnetic mineral to an acid leaching step II and a solid-liquid separation step V, dissolving the calcium-containing substances and magnesium-containing substances in the non-weakly magnetic mineral to obtain a quartz / fluorite / mica mixed ore, wherein the quartz / fluorite / mica mixed ore contains quartz / fluorite / calcite intergrowths without monomer dissociation; the intergrowths are fine-grained minerals that cannot be physically separated, and the particle size of the intergrowths is 0.019-0.005 mm; S2, the tailings intergrowth dissociation process, is implemented after the strong magnetic separation process S11, the acid leaching process II S12 and the solid-liquid separation process V S13, and includes: S21, flotation process I is performed on the quartz / fluorite / mica mixed ore, the flotation foam obtained after the flotation operation is fluorite concentrate, the calcium fluoride content is ≥97%, the flotation tank bottom mineral is quartz / mica mixed ore, and the quartz / mica mixed ore contains the intergrowth; in flotation process I S21, the flotation pulp concentration is 30-40% by mass, the flotation collector is modified oleic acid, specifically oleic acid triethanolamine soap, and the flotation depressant is acidified water glass, water glass and sodium carbonate; S22, flotation II process is performed on the quartz / mica mixed ore, the flotation foam obtained after the flotation operation is mica concentrate, the mica content is ≥94%, the flotation tank bottom mineral is quartz rough concentrate, and the quartz rough concentrate contains the intergrowth; in flotation II process S22, the flotation pulp concentration is 30-40% by mass, the pH value of the flotation pulp is controlled at pH3-pH4, dodecylamine is selected as the flotation collector, and sodium hexametaphosphate [(NaPO3)6] is selected as the flotation depressant; S23 and S24, performing an acid leaching step III and a solid-liquid separation step VI on the quartz rough concentrate, wherein a strong acid and a dissolving agent are used in the acid leaching step III S23, wherein the strong acid dissolves the fluorine-containing substances and calcium-containing substances in the quartz rough concentrate but does not dissolve the silicon dioxide, thereby dissociating the intergrown monomers, and the dissolving agent interrupts the continuous chemical reaction of the acid-dissolved silicon, thereby retaining the silicon dioxide of the intergrown before the monomer dissociation in the quartz rough concentrate, thereby obtaining a quartz concentrate; S3, a first recovery process of fluorine-containing liquid, implemented after the tailings intergrowth dissociation process S2, including: performing a first recovery process on the fluorine-containing liquid dissolved in the solid-liquid separation VI process S24, and obtaining a chemical product to eliminate gas-liquid-solid three-state waste; Among them, the strong acid used in the acid leaching step III S23 is hydrochloric acid, and the dissolution inhibitor used is boric acid. The fluoroboric acid generated by the intermediate reaction does not chemically react with silicon dioxide, but chemically reacts with oxides containing calcium, magnesium, aluminum, potassium, and iron in alumina, aluminosilicate, and calcium-magnesium compounds to dissolve them into the fluoroboric acid.
2. The method for preparing quartz purified from secondary tungsten tailings according to claim 1, characterized in that: The first recovery process S3 of the fluorine-containing liquid comprises: S31 and S32, precipitation step IV with adding ammonia water and solid-liquid separation step VII to separate the calcium fluoride product and the first recovered liquid; S33 and S34, performing an alkali decomposition process of adding calcium hydroxide and a distillation IV process on the first recovered liquid to obtain a second recovered liquid, wherein the gas separated by the alkali decomposition process S33 and the distillation IV process S34 is subjected to an absorption I process S35 to obtain a high-purity ammonia product; S36 and S37, performing a precipitation step V of adding sulfuric acid and a solid-liquid separation step VIII on the second recovered liquid to separate the calcium sulfate product and the third recovered liquid; S38, the third recovered liquid is subjected to a distillation step V to separate the boric acid product and the distilled fourth recovered liquid, and the fourth recovered liquid is subjected to an absorption step II S39 to obtain a high-purity hydrochloric acid product.
3. The method for preparing quartz purified from secondary tungsten tailings according to claim 1, characterized in that: The operating conditions of the acid leaching step III S23 include: temperature of 50-90° C., reaction time of 20-70 min, and solid-liquid ratio of 1 kg:1-3 L.
4. The method for preparing quartz purified from secondary tungsten tailings according to claim 1, characterized in that: The operating conditions of the acid leaching step III S23 include: temperature 40-70° C., reaction time 30-60 min, solid-liquid ratio 1 kg:1-1.4 L, hydrofluoric acid concentration range 6-11%, dissolution inhibitor concentration range 7.5-12.5%, hydrochloric acid concentration range 3-5 mol / L.
5. The method for preparing quartz purified from secondary tungsten tailings according to claim 2, characterized in that: After the strong magnetic separation step S11, the following steps are also included: S14 and S15, performing an acid leaching step I and a solid-liquid separation step I on the weakly magnetic mineral, using hydrochloric acid to obtain biotite concentrate and non-fluorine-containing liquid; The non-fluorine-containing liquid is subjected to a second recovery process to obtain separated ferric hydroxide products, sodium chloride products, calcium sulfate products, magnesium sulfate products and high-purity hydrochloric acid products.
6. The method for preparing quartz purified from secondary tungsten tailings according to claim 5, characterized in that: The second recovery process of the non-fluorine-containing liquid includes: an oxidation / precipitation I step S41, a solid-liquid separation II step S42 corresponding to the preparation of the iron hydroxide product, a precipitation II step S43, a solid-liquid separation III step S44, a neutralization step S45, an evaporation I step S46 corresponding to the preparation of the sodium chloride product, an acid dissolution step S47, a precipitation III step S48, a solid-liquid separation IV step S49 corresponding to the preparation of the calcium sulfate product, and a distillation / evaporation II step S50 corresponding to the preparation of the magnesium sulfate product.
7. The method for preparing quartz purified from secondary tungsten tailings according to claim 6, characterized in that: The first recovery process S3 of the fluorine-containing liquid and the second recovery process of the non-fluorine-containing liquid are overlapped in the absorption II step S39 to simultaneously recover high-purity hydrochloric acid products.
8. The method for preparing quartz purified from secondary tungsten tailings according to claim 7, characterized in that: The tailings intergrowth dissociation process S2 and the second recovery process of the non-fluorine-containing liquid overlap in the precipitation III step S48, so that the calcium sulfate I product is recovered through the solid-liquid separation IV step S49, the magnesium sulfate product is recovered through the distillation / evaporation II step S50, and the high-purity hydrochloric acid product is recovered through the absorption II step S39.
9. A secondary tungsten tailings purification quartz equipment, characterized in that: For executing the preparation method of quartz purified from secondary tungsten tailings according to any one of claims 1 to 8, the quartz purification equipment for fluorine-containing solid waste includes: The strong magnetic separation unit separates the iron-containing substances in the solid waste to obtain non-magnetic solid waste; The acid leaching unit II and the solid-liquid separation unit V are used to dissolve the calcium-containing substances and the magnesium-containing substances in the non-magnetic solid waste to obtain a first mixed solid waste, wherein the first mixed solid waste contains a conjoined body of silicon dioxide / calcium fluoride / calcium carbonate without monomer dissociation; A conjoined body dissociation module is used to dissociate the conjoined bodies at the fine particle level in the first mixed solid waste; the conjoined body dissociation module comprises: A flotation I unit, used for separating calcium fluoride from the first mixed solid waste to obtain a second mixed solid waste, wherein the second mixed solid waste contains the conjoined bodies; A flotation II unit is used to separate mica from the second mixed solid waste to obtain a third mixed solid waste, wherein the third mixed solid waste contains the conjoined bodies; and Acid leaching III unit and solid-liquid separation VI unit, wherein the acid leaching III unit uses a strong acid and a dissolving agent to dissolve the fluorine-containing substances and calcium-containing substances in the intergrowth of the third mixed solid waste but not dissolve the silicon dioxide, so that the intergrowth monomers are dissociated, and the dissolving agent interrupts the continuous chemical reaction of the acid-dissolved silicon, so that the silicon dioxide of the intergrowth before the monomer dissociation is retained in the third mixed solid waste, so as to obtain silicon dioxide; The recovery equipment module recovers the fluorine-containing liquid dissolved by the acid leaching unit III and separated by the solid-liquid separation unit VI to obtain chemical products, thereby eliminating gas-liquid-solid three-state waste.
10. The secondary tungsten tailings purification quartz equipment according to claim 9, characterized in that: The fluorine-containing solid waste is specifically selected from any one of wet pyrometallurgical smelting slag, smoke and flue gas sediment, treated wastewater and waste acid precipitates, fluorine-containing minerals and secondary tungsten tailings; the process conditions of the acid leaching III unit include: temperature 40-70°C, reaction time 30-60min, solid-liquid ratio of 1kg:1-1.4L, hydrofluoric acid concentration range of 6-11%, solvent inhibitor concentration range of 7.5-12.5%, and hydrochloric acid concentration range of 3-5mol / L.