Thermoplastic foamed particles, preparation method thereof, and foamed particle formed body
The foaming of foamed TPU particles is solved by using components such as thermoplastic polyurethane elastomer, polylactic acid, nanocellulose organogel and polytetrafluoroethylene fiber in foamed TPU particles, combined with hydrophobic modified silica and graphene, and the foamed TPU particles are solved. The problem of poor strength improves tensile resistance and cell density, and improves the mechanical properties of the foamed molded body.
Patent Information
- Application Number
- CN202310045443.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-01-30
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2043-01-30
AI Technical Summary
When the existing foamed TPU particles are heated and welded by steam, the welding strength is poor and the tensile resistance needs to be improved.
Using thermoplastic polyurethane elastomers, polylactic acid, nanocellulose organic gels and polytetrafluoroethylene fibers, the molecular weight is increased and branched and cross-linked structures are formed through chain extenders, the toughness after welding is improved, and the toughness is eliminated through hydrophobicity. Modified silica and graphene improve interfacial adhesion and cell density.
The welding strength and tensile resistance between foamed particles are significantly improved, the cell density and shape uniformity are increased, and the mechanical properties of the foamed molded body are improved.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of foaming materials, and more specifically, to a thermoplastic foamed particle, a preparation method thereof, and a foamed particle formed body. Background Art
[0002] Foam materials are favored for their low density, high specific strength, strong ability to absorb impact loads, and good thermal insulation performance. They are widely used in packaging, industry, agriculture, transportation, aviation, and daily civilian use. Commonly used foam materials include polystyrene foam, polyethylene foam, polypropylene foam, and polyurethane soft and hard foam.
[0003] Thermoplastic polyurethane (TPU) has the advantages of good physical properties, low temperature flexibility, hydrolysis resistance, aging resistance, environmental friendliness, and recyclability. The foamed products obtained by steam molding the foamed TPU particles not only retain the excellent properties of the base material, but also have excellent rebound performance and low density. Therefore, foamed TPU products have broad application prospects in the fields of footwear, automobiles, packaging and daily life.
[0004] At present, the method for preparing foaming materials is mainly to fill a large number of bubbles inside the plastic by physical or chemical methods. In a closed container, TPU resin particles are dispersed into an aqueous medium, and a foaming agent is introduced into the container, heated so that the foaming agent penetrates into the resin particles to form foamable resin particles, and then the softened foamable resin particles are released into a low-pressure environment. Furthermore, the foamed particles are filled into a mold and heated by water vapor, etc., so that the foamed particles are welded to each other to produce a TPU foamed particle molded body.
[0005] With respect to the above-mentioned related technologies, the inventors found that when the expandable resin particles are heated by passing steam, the steam causes the expandable resin particles to fuse to each other, and the welding strength between the expandable resin particles is poor, and the tensile resistance after welding needs to be improved. Summary of the invention
[0006] In order to improve the welding strength between foamed particles and improve the stretch resistance of foamed particle molded bodies, the present application provides thermoplastic foamed particles, a preparation method thereof, and a foamed particle molded body.
[0007] In a first aspect, the present application provides a thermoplastic foamed particle, which adopts the following technical solution:
[0008] A thermoplastic foamed particle comprises the following components in parts by weight: 6-9.5 parts of a thermoplastic polyurethane elastomer, 1.5-4 parts of polylactic acid, 0.6-1.4 parts of a chain extender, 1.2-3.2 parts of a nano-cellulose organic gel, and 2-4 parts of polytetrafluoroethylene fibers.
[0009] By adopting the above technical scheme, polylactic acid, nanocellulose organic gel and polytetrafluoroethylene fiber are added on the basis of thermoplastic polyurethane elastomer as a matrix. The chain extender can increase the molecular weight of the polylactic acid and thermoplastic polyurethane elastomer blend and form branched and cross-linked structures on the molecular chain segments of the blend, improve the compatibility of the two, and improve the toughness of the thermoplastic foamed particles after welding. In addition, polylactic acid can also promote the formation of open cells in the foaming process of thermoplastic polyurethane elastomer, increase melt strength, reduce the fusion of bubbles, and increase the open cell rate; the nanocellulose organic gel has good dispersibility with polylactic acid and can form a three-dimensional network structure in the blend of polylactic acid and thermoplastic polyurethane elastomer through the hydrogen bonding between hydroxyl groups, thereby limiting The polylactic acid and thermoplastic polyurethane elastomer chain segment movement is controlled, and the energy required for chain segment movement is increased, thereby improving the mechanical strength of the blended melt, increasing the melt strength, and increasing the growth resistance of the bubbles. It has a regulating effect on the growth of the pores during foaming, maintaining the shape of the pores, making the pores not easy to merge and collapse, etc. It also limits the growth of the pores, reduces the pore diameter, increases the pore density, and makes the pore diameter distribution more uniform; polytetrafluoroethylene fiber is a material with high strength and high toughness, and has the advantages of high elastic modulus, high temperature resistance, acid and alkali resistance, low density and good thermal stability. When the thermoplastic foamed particles are pressurized and welded, the polytetrafluoroethylene fibers in adjacent thermoplastic foamed particles can overlap each other, increasing the tensile strength of the welding position.
[0010] Optionally, the polytetrafluoroethylene fiber is pretreated as follows:
[0011] The silicon dioxide is hydrophobically modified to obtain hydrophobically modified silicon dioxide;
[0012] Dissolving polylactic acid to prepare a polylactic acid solution with a concentration of 13-15wt%, adding the hydrophobically modified silica to prepare a coating liquid, wherein the mass ratio of polylactic acid to hydrophobically modified silica is 1:(0.2-0.5);
[0013] The coating liquid is evenly applied on the polytetrafluoroethylene fiber, and then the polytetrafluoroethylene is placed in an ethanol solution, immersed for 5-10 minutes, washed, and dried. The mass ratio of the coating liquid to the polytetrafluoroethylene is (0.3-0.5):1.
[0014] By adopting the above technical scheme, the surface of silica contains hydroxyl groups, and after hydrophobic treatment, its hydroxyl content is reduced, the hydrophilicity is reduced, and the compatibility of silica and polylactic acid is improved. After the polylactic acid is dissolved, it is mixed with hydrophobically modified silica to form a coating liquid. After brushing on the polytetrafluoroethylene fiber, the polytetrafluoroethylene fiber is placed in an ethanol solution, and the ethanol solution is used as a coagulation bath to remove the solvent of the polylactic acid, so that the polylactic acid and the hydrophobically modified silica form a shell on the surface of the polytetrafluoroethylene fiber. When mixed with a thermoplastic polyurethane elastomer and hot-melted, the polylactic acid can be hot-melted, and the hydrophobically modified silica can also flow with it. The hydrophobically modified silica can be bonded to the thermoplastic polyurethane. Hydrogen bonds are formed. When the thermoplastic foamed particles are injected into the mold and welded, the hydrophobically modified silica is distributed at the weld and interacts with the polylactic acid and the thermoplastic polyurethane elastomer to increase the interfacial adhesion at the weld, thereby improving the tensile strength of the thermoplastic foamed particles after hot melting. The interaction between the hydrophobically modified silica nanoparticles and the interaction between the hydrophobically modified silica nanoparticles and the polylactic acid and the thermoplastic polyurethane elastomer slows down the relative movement of the molecular chains, prolongs their relaxation time, increases the elastic modulus, and improves the elasticity. In addition, the addition of the hydrophobically modified silica can serve as a heterogeneous nucleating agent to reduce the average diameter of the pores, increase the pore density, and enhance the elasticity of the foamed body.
[0015] Optionally, before the polytetrafluoroethylene fiber is coated with the coating liquid, it is subjected to the following treatment: in parts by weight, 0.4-0.6 parts of POE, 0.02-0.05 parts of ethylene-methacrylate copolymer, 0.2-0.5 parts of polyvinyl alcohol and 10 parts of water are mixed evenly to prepare a treatment liquid, the polytetrafluoroethylene fiber is added, the mixture is mixed evenly, and then filtered and dried. The mass ratio of the treatment liquid to the polytetrafluoroethylene fiber is (0.2-0.4):1.
[0016] By adopting the above technical scheme, before the polytetrafluoroethylene fiber is coated with the coating liquid, the viscosity of polyvinyl alcohol is first used to adhere POE and ethylene-glycidyl methacrylate copolymer to the surface of the polytetrafluoroethylene fiber. After the coating liquid formed by polylactic acid is coated on the surface of the polytetrafluoroethylene fiber, the shell formed by polylactic acid adheres to the surface of POE. When the thermoplastic foamed particles are subsequently prepared by hot melt, under the action of ethylene-glycidyl methacrylate copolymer as a compatibilizer, the terminal hydroxyl group or carboxyl group on the polylactic acid reacts with the epoxy group of the ethylene-glycidyl methacrylate copolymer during blending, and the generated graft polymer improves the interfacial compatibility between polylactic acid and POE, thereby further improving the strength and toughness of the polylactic acid, and further improving the mechanical strength of the thermoplastic foamed particles after welding.
[0017] Optionally, the hydrophobically modified silica is prepared by modification with hexamethyldisilazane.
[0018] By adopting the above technical scheme, hexamethyldisilazane can graft hydrophobic groups on silicon dioxide, reduce the hydroxyl content, make silicon dioxide hydrophobic, and improve the compatibility of silicon dioxide with polylactic acid and thermoplastic polyurethane elastomer.
[0019] Optionally, the nanocellulose organogel comprises nanocellulose and graphene in a mass ratio of 1:0.1-0.12.
[0020] By adopting the above technical scheme, graphene and nanocellulose are physically compounded, and graphene is attached to the nanocellulose skeleton, thereby increasing the structural stability of the nanocellulose skeleton, so that the nanocellulose organic gel can increase the welding strength, and due to the dispersing effect of nanocellulose, graphene is evenly dispersed in the thermoplastic polyurethane elastomer, and plays a role of crystal nucleus when the thermoplastic polyurethane elastomer is melted and cooled, which significantly promotes the crystallization of the thermoplastic polyurethane elastomer, and can also enhance the melt strength and improve the pore density.
[0021] Optionally, the preparation method of the nanocellulose organogel is as follows:
[0022] Dissolving nanocellulose in deionized water to prepare a dispersion with a mass fraction of 2-3%;
[0023] Chitosan powder, graphene and anhydrous sodium sulfate are added to the dispersion, ultrasonicated for 2-5 minutes, injected into a mold for molding, and after molding, placed in 50-55°C water for curing and washing for 40-48 hours, frozen with liquid nitrogen for 1-1.5 hours, and then vacuum freeze-dried and crushed to obtain nanocellulose organogel. The mass ratio of chitosan, anhydrous sodium sulfate and dispersion is (0.01-0.03):(2-3):1.
[0024] By adopting the above technical scheme, nanocellulose forms hydrogen bonds through hydroxyl groups to complete physical crosslinking and form a gel. After freezing, a rigid network structure is formed. Graphene, chitosan powder and anhydrous sodium sulfate are added to the network structure. Anhydrous sodium sulfate serves as a pore-forming agent and occupies a certain space in the dispersion. After water washing and solidification, nanocellulose is regenerated and precipitated to form a skeleton, and the pore-forming agent is dissolved in water to form a pore structure. The amino groups on the chitosan molecular chain and the hydroxyl groups on the nanocellulose molecular chain undergo hydrogen bonding. After water washing, solidification and regeneration, the chitosan particles are embedded in the nanocellulose macromolecular chain and serve as a fulcrum to connect the porous network structure of nanocellulose, thereby playing a role. The plasticizing effect makes the structure of the nanocellulose organic gel more stable, and the hydroxyl groups on the chitosan and nanocellulose molecules interact with each other. The chitosan powder as a filler and the nanocellulose as a matrix have good interface compatibility, which helps to improve the fracture strength of the gel. In addition, the hydrogen bonding effect formed increases the intermolecular interaction force, making the three-dimensional network structure more stable and improving the thermal stability. It is not easy to decompose when the thermoplastic foamed particles are welded. As a result, when the polylactic acid and thermoplastic polyurethane elastomer are mixed and hot-melted, the nanocellulose organic gel is dispersed in the mixed melt with a rigid network structure, thereby increasing the tensile strength after welding.
[0025] Optionally, the chain extender is selected from at least one of ADR-4370 and 4,4'-diphenylmethane diisocyanate.
[0026] In a second aspect, the present application provides a method for preparing thermoplastic foamed particles, using the following technical solution:
[0027] A method for preparing thermoplastic foamed particles comprises the following steps:
[0028] The polylactic acid and nanocellulose organogel are mixed, extruded and granulated to obtain modified polylactic acid;
[0029] The modified polylactic acid, thermoplastic polyurethane elastomer, chain extender and polytetrafluoroethylene fiber are mixed, extruded and granulated to obtain polymer pellets;
[0030] Heat the autoclave to the foaming temperature, add polymer pellets, introduce carbon dioxide to exclude air, close the autoclave, introduce high-pressure carbon dioxide gas to the foaming pressure, foam, release the pressure to atmospheric pressure within 0.5-1s, cool, and obtain thermoplastic foamed particles.
[0031] By adopting the above technical scheme, the nanocellulose organogel and polylactic acid are first mixed. The nanocellulose organogel has good dispersion in the polylactic acid, which improves the melt strength of the polylactic acid. Then, the modified polylactic acid is mixed with raw materials such as thermoplastic polyurethane elastomer, and supercritical carbon dioxide is used as a foaming agent. The production process is environmentally friendly, the preparation process is simple, and it is easy to industrialize.
[0032] Optionally, the pressure is 14-20 MPa, the foaming temperature is 160-180° C., and the foaming time is 3-4 h.
[0033] By adopting the above technical solution, when the foaming pressure is high, the concentration of carbon dioxide in the polymer increases, the polymer molecular chain moves more easily, the melt strength decreases, and the resistance to the growth of the bubbles decreases, thereby increasing the average diameter of the bubbles. Secondly, since more carbon dioxide is dissolved in the polymer and the pressure difference becomes larger, the number of nucleation points formed at the moment of pressure relief increases, thereby increasing the density of the bubbles. If the foaming temperature is too high or too low, it will cause the bubbles to merge easily, collapse, or be difficult to grow.
[0034] In a third aspect, the present application provides a method for preparing a foamed particle formed body, using the following technical solution:
[0035] A foamed particle formed body is made by filling thermoplastic foamed particles in a mold for foaming.
[0036] By adopting the above technical scheme, the thermoplastic foamed particles are foamed into foamed particle molded bodies. According to the shape of the mold, the shape of the foamed particle molded body can be selected as needed to be made into automotive parts, sole materials, cushioning materials or shockproof materials, etc.
[0037] In summary, this application has the following beneficial effects:
[0038] 1. Since the present application adopts thermoplastic polyurethane elastomer as the base material and incorporates polylactic acid, polytetrafluoroethylene fiber, nanocellulose organic gel and other materials, polylactic acid can enhance the melt strength and increase the open porosity, and the nanocellulose organic sol is dispersed in the blended melt in the form of a three-dimensional network structure, which can increase the melt strength and improve the pore density. Moreover, when the thermoplastic foamed particles are hot-melted, they can overlap each other to form an anti-stretching structure, thereby improving the tensile resistance of the thermoplastic foamed particles after hot-melting. Moreover, the polytetrafluoroethylene fiber has good heat resistance and can form an overlapping network in the thermoplastic foamed particles to improve the elasticity and tensile strength of the foamed particles.
[0039] 2. In the present application, polylactic acid and hydrophobically modified silica are preferably used to pretreat the polytetrafluoroethylene fiber. The hydrophobically modified silica can increase the interfacial adhesion between the polylactic acid shell on the polytetrafluoroethylene fiber and the thermoplastic polyurethane elastomer, increase the pore density, and improve the hot-melt interfacial tensile strength of the thermoplastic foamed particles. Moreover, the polylactic acid as the shell can improve the compatibility of the polytetrafluoroethylene fiber with the matrix resin and improve the mechanical strength of the thermoplastic foamed particles.
[0040] 3. In the present application, nanocellulose, graphene and chitosan powders are preferably used to prepare nanocellulose organogel. Graphene and chitosan powders can improve the structural stability of nanocellulose organogel and facilitate the dispersion of nanocellulose organogel in thermoplastic foamed particles to improve the welding strength of thermoplastic foamed particles. Chitosan powder can also increase the porosity of nanocellulose organogel and improve the elasticity of thermoplastic foamed particles. Implementation
[0041] Preparation Example 1: Dissolve nanocellulose in deionized water to prepare a dispersion with a mass fraction of 3%;
[0042] Chitosan powder, graphene and anhydrous sodium sulfate were added to the dispersion, ultrasonicated for 5 minutes, injected into a mold for forming, put into 50°C water for curing and washing for 48 hours, frozen with liquid nitrogen for 1.5 hours, and then vacuum freeze-dried at -50°C for 60 hours, and crushed to obtain nanocellulose organogel. The mass ratio of chitosan, anhydrous sodium sulfate and dispersion was 0.03:3:1, and the mass ratio of nanocellulose and graphene was 1:0.12.
[0043] Preparation Example 2: Dissolve nanocellulose in deionized water to prepare a dispersion with a mass fraction of 2%;
[0044] Chitosan powder, graphene and anhydrous sodium sulfate were added to the dispersion, ultrasonicated for 2 minutes, injected into a mold for forming, put into 55°C water for curing and washing for 40 hours, frozen with liquid nitrogen for 1 hour, and then vacuum freeze-dried at -50°C for 60 hours, and crushed to obtain nanocellulose organogel. The mass ratio of chitosan, anhydrous sodium sulfate and dispersion was 0.01:2:1, and the mass ratio of nanocellulose and graphene was 1:0.1.
[0045] Preparation Example 3: Dissolve nanocellulose in deionized water to prepare a dispersion with a mass fraction of 3%;
[0046] Graphene was added to the dispersion, ultrasonicated for 5 minutes, frozen with liquid nitrogen for 1.5 hours, and then vacuum freeze-dried at -50°C for 60 hours and crushed to obtain nanocellulose organogel. The mass ratio of nanocellulose to graphene was 1:0.12.
[0047] Preparation Example 4: 2.16 g of nanocellulose was dissolved in deionized water to prepare a dispersion with a mass fraction of 3%, 100 mL of tert-butanol was added, and the mixture was frozen with liquid nitrogen for 1.5 h, then vacuum freeze-dried at -50°C for 60 h, and crushed. Example
[0048] Example 1: A thermoplastic foamed particle comprises the following raw materials by weight: 9.5 kg thermoplastic polyurethane elastomer, 4 kg polylactic acid, 1.4 kg chain extender, 3.2 kg nanocellulose organogel and 4 kg polytetrafluoroethylene fiber, wherein the density of polylactic acid is 1.24 g / cm 3 , brand 4032D, thermoplastic polyurethane elastomer density 1.2g / cm 3 , brand WHT-1185, chain extender is 4,4'-diphenylmethane diisocyanate, nanocellulose organogel is prepared by Preparation Example 1, and the length of polytetrafluoroethylene fiber is 10 mm.
[0049] The method for preparing the thermoplastic foamed particles comprises the following steps:
[0050] S1, mixing, extruding and granulating polylactic acid and nanocellulose organogel to obtain modified polylactic acid, the extrusion temperature being 160° C.;
[0051] S2, mixing modified polylactic acid, thermoplastic polyurethane elastomer, chain extender and polytetrafluoroethylene fiber, extruding and granulating to obtain polymer pellets, setting the temperature from the feed port to the die to 160-180-180-180°C, and the screw speed to 60rpm;
[0052] S3. Heat the autoclave to the foaming temperature, add polymer pellets, pass carbon dioxide to exclude air, close the autoclave, pass high-pressure carbon dioxide gas to the foaming pressure, foam, release the pressure to atmospheric pressure within 1 second, cool, and obtain thermoplastic foamed particles. The foaming temperature is 180°C, the foaming pressure is 14 MPa, and the foaming time is 4 hours.
[0053] Example 2: A thermoplastic foamed particle, comprising the following raw materials by weight: 6 kg thermoplastic polyurethane elastomer, 1.5 kg polylactic acid, 0.6 g chain extender, 1.2 kg nanocellulose organogel and 2 kg polytetrafluoroethylene fiber, the density of polylactic acid being 1.24 g / cm 3 , brand 4032D, thermoplastic polyurethane elastomer density 1.2g / cm 3 , brand is WHT-1185, chain extender is ADR-4370, nanocellulose organogel is prepared by Preparation Example 2, and the length of polytetrafluoroethylene fiber is 10 mm.
[0054] The method for preparing the thermoplastic foamed particles comprises the following steps:
[0055] S1, mixing, extruding and granulating polylactic acid and nanocellulose organogel to obtain modified polylactic acid, the extrusion temperature being 165° C.;
[0056] S2, mixing modified polylactic acid, thermoplastic polyurethane elastomer, chain extender and polytetrafluoroethylene fiber, extruding and granulating to obtain polymer pellets, setting the temperature from the feed port to the die to 160-180-180-180°C, and the screw speed to 60rpm;
[0057] S3. Heat the autoclave to the foaming temperature, add polymer pellets, pass carbon dioxide to exclude air, close the autoclave, pass high-pressure carbon dioxide gas to the foaming pressure, foam, release the pressure to atmospheric pressure within 0.5s, cool, and obtain thermoplastic foamed particles. The foaming temperature is 160°C, the foaming pressure is 20MPa, and the foaming time is 3h.
[0058] Example 3: A thermoplastic foamed particle, comprising the following raw materials by weight: 7.5 kg thermoplastic polyurethane elastomer, 3 kg polylactic acid, 1 g chain extender, 2.2 kg nanocellulose organogel and 3 kg polytetrafluoroethylene fiber, the density of polylactic acid being 1.24 g / cm 3 , brand 4032D, thermoplastic polyurethane elastomer density 1.2g / cm 3 The brand is WHT-1185, the chain extender is ADR-4370 and 4,4'-diphenylmethane diisocyanate in a mass ratio of 1:1, the nanocellulose organogel is prepared by Preparation Example 1, and the length of the polytetrafluoroethylene fiber is 10 mm.
[0059] The method for preparing the thermoplastic foamed particles comprises the following steps:
[0060] S1, mixing, extruding and granulating polylactic acid and nanocellulose organogel to obtain modified polylactic acid, the extrusion temperature being 170° C.;
[0061] S2, mixing modified polylactic acid, thermoplastic polyurethane elastomer, chain extender and polytetrafluoroethylene fiber, extruding and granulating to obtain polymer pellets, setting the temperature from the feed port to the die to 160-180-180-180°C, and the screw speed to 60rpm;
[0062] S3. Heat the autoclave to the foaming temperature, add polymer pellets, pass carbon dioxide to exclude air, close the autoclave, pass high-pressure carbon dioxide gas to the foaming pressure, foam, release the pressure to atmospheric pressure within 0.8 s, cool, and obtain thermoplastic foamed particles. The foaming temperature is 170°C, the foaming pressure is 17 MPa, and the foaming time is 3.5 h.
[0063] Example 4: A thermoplastic foamed particle, which is different from Example 1 in that the nanocellulose organogel is prepared by Preparation Example 3.
[0064] Example 5: A thermoplastic foamed particle, which is different from Example 1 in that the nanocellulose organogel is prepared by Preparation Example 4.
[0065] Embodiment 6: A thermoplastic foamed particle, which is different from Embodiment 1 in that the polytetrafluoroethylene fiber is pretreated as follows:
[0066] Dissolving hexamethyldisilazane in water to prepare a solution with a concentration of 5 wt%, adding silicon dioxide, impregnating, filtering, and drying to obtain hydrophobically modified silicon dioxide;
[0067] Polylactic acid was dissolved in DCM and DMF in a volume ratio of 6.5:3.5 to prepare a polylactic acid solution with a concentration of 15 wt%, and hydrophobically modified silica was added to prepare a coating solution, wherein the mass ratio of polylactic acid to hydrophobically modified silica was 1:0.5;
[0068] The coating liquid is evenly applied on the polytetrafluoroethylene fiber, and then the polytetrafluoroethylene is placed in an ethanol solution, immersed for 10 minutes, washed, and dried. The mass ratio of the coating liquid to the polytetrafluoroethylene is 0.5:1.
[0069] Embodiment 7: A thermoplastic foamed particle, which is different from Embodiment 1 in that the polytetrafluoroethylene fiber is pretreated as follows:
[0070] Dissolving hexamethyldisilazane in water to prepare a solution with a concentration of 5 wt%, adding silicon dioxide, impregnating, filtering, and drying to obtain hydrophobically modified silicon dioxide;
[0071] Polylactic acid was dissolved in DCM and DMF in a volume ratio of 6.5:3.5 to prepare a polylactic acid solution with a concentration of 13 wt%, and hydrophobically modified silica was added to prepare a coating solution, wherein the mass ratio of polylactic acid to hydrophobically modified silica was 1:0.2;
[0072] The coating liquid is evenly applied on the polytetrafluoroethylene fiber, and then the polytetrafluoroethylene is placed in an ethanol solution, immersed for 5 minutes, washed, and dried. The mass ratio of the coating liquid to the polytetrafluoroethylene is 0.3:1.
[0073] Example 8: A thermoplastic foamed particle, which is different from Example 6 in that no hydrophobically modified silica is added to the coating liquid.
[0074] Example 9: A thermoplastic foamed particle, which is different from Example 6 in that the silicon dioxide is not hydrophobically modified.
[0075] Example 10: A thermoplastic foam particle, which differs from Example 6 in that a polyvinyl alcohol aqueous solution with an equal concentration of 5 wt % is used instead of the polylactic acid solution.
[0076] Example 11: A thermoplastic foam particle, which differs from Example 6 in that before the polytetrafluoroethylene fiber is coated with the coating liquid, the polytetrafluoroethylene fiber is first treated as follows: 0.6 kg POE, 0.05 kg ethylene-methacrylate copolymer, 0.5 kg polyvinyl alcohol and 10 kg water are mixed evenly to prepare a treatment liquid, the polytetrafluoroethylene fiber is added, the mixture is mixed evenly, filtered and dried, and the mass ratio of the treatment liquid to the polytetrafluoroethylene fiber is 0.4:1.
[0077] Example 12: A thermoplastic foam particle, which differs from Example 6 in that before the polytetrafluoroethylene fiber is coated with the coating liquid, the polytetrafluoroethylene fiber is first treated as follows: 0.4 kg POE, 0.02 kg ethylene-methacrylate copolymer, 0.2 kg polyvinyl alcohol and 10 kg water are mixed evenly to prepare a treatment liquid, the polytetrafluoroethylene fiber is added, the mixture is mixed evenly, filtered and dried, and the mass ratio of the treatment liquid to the polytetrafluoroethylene fiber is 0.2:1.
[0078] Example 13: A thermoplastic foamed particle, which is different from Example 11 in that ethylene-glycidyl methacrylate copolymer is not added.
[0079] Comparative Example 1: A thermoplastic foamed particle, which is different from Example 1 in that polytetrafluoroethylene fibers are not added.
[0080] Comparative Example 2: A thermoplastic foamed particle, which differs from Example 1 in that polylactic acid is not added.
[0081] Comparative Example 3: A thermoplastic foamed particle, which differs from Example 1 in that no nanocellulose organogel is added.
[0082] Comparative Example 4: A method for preparing thermoplastic polyurethane foam particles, comprising the following steps:
[0083] (1) According to the mass percentage, 2670g of thermoplastic polyether polyurethane (8190RV) and 330g of polyethylene grafted glycidyl methacrylate (EPA-860H) were mixed evenly. The mixed composition was melt-blended in a φ42mm co-rotating twin-screw extruder at a blending extrusion temperature of 210°C, and TPU blended alloy particles were obtained after underwater pelletization and drying;
[0084] (2) Add the TPU blended alloy particles into an autoclave, introduce carbon dioxide, and allow the carbon dioxide to impregnate the TPU blended alloy particles. The temperature of the autoclave is 160°C, the pressure is 10 MPa, and the impregnation time is 1 hour.
[0085] (3) After impregnation, the material in the autoclave is discharged into the atmosphere at a pressure release rate of 5 MPa / s to obtain foamed particles.
[0086] Application Example 1: A foamed particle molded body, in which the thermoplastic foamed particles prepared in Example 1 are filled into a mold with a mold size of 40cm×40cm×8cm. After saturated steam at a pressure of 2.5kg is introduced into the mold to preheat the thermoplastic foamed particles, the thermoplastic foamed particles are heated by saturated steam at a pressure of 3.3kg, and then cooled to obtain a foamed molded body.
[0087] Application Example 2-13: A foamed particle molded body, which is different from Application Example 1 in that the thermoplastic foamed particles prepared in Examples 2-13 are respectively filled into a mold and foamed.
[0088] Application Examples 14-17: A foamed particle molded body, which differs from Application Example 1 in that the thermoplastic foamed particles prepared in Comparative Examples 1-4 are respectively filled into a mold and foamed.
[0089] The foamed particle molded body was prepared according to the method of Application Examples 1-17, and the properties of the foamed particle molded body were tested with reference to the following method. The test results are recorded in Table 1.
[0090] 1. Cell density: measured by the method described in JISA9511:1995 "Foamed plastic insulation board". Cut out 10 cm × 10 cm × 3 cm (300 cm 3 ) of the test piece, weigh its mass W (g) to 2 decimal places, and calculate the foam density (kg / m 3 )=W / 300×1000.
[0091] 2. Welding rate: Cut the foamed particle molded body into samples of 170mm×30mm×33mm, and cut a 15mm incision on one side of the sample by using a cutting knife to divide the longitudinal length of the foamed particle molded body into two equal parts. The foamed particle molded body is bent and broken from the incision. The ratio of the number of foamed particles m after the damage on the fracture surface to the number of foamed particles n on the fracture surface is taken as the welding rate. The number of foamed particles n is the combination of the number of foamed particles m after the material is damaged and the number of foamed particles peeled between the foamed particles. The larger the m value, the higher the welding rate between the foamed particles, thus forming a foamed particle molded body with excellent mechanical properties such as bending strength or tensile strength. In addition, if the molded body does not break even if it is bent, the welding rate is 100%.
[0092] 3. Tensile strength and elongation at break: Tested in accordance with GB / T6344-2008 "Determination of tensile strength and elongation at break of soft foam polymer materials".
[0093] Table 1 Performance test results of expanded particle moldings
[0094]
[0095] Combining Application Examples 1-3 and the data in Table 1, it can be seen that the thermoplastic foamed particles prepared in Examples 1-3 have high cell density and uniform molding after foaming, and the foamed particle molded body has high welding rate, high tensile strength and strong mechanical properties.
[0096] In Application Example 4, the nanocellulose organogel prepared in Preparation Example 4 was used, to which no chitosan powder was added. Table 1 shows that, compared with Application Example 1, the pore density of the foamed particle molded body decreased, and the tensile strength and elongation at break all decreased, indicating that chitosan powder can increase the structural stability of the nanocellulose organosol and improve the pore density and mechanical properties of the foamed particle molded body.
[0097] In Application Example 5, the nanocellulose organogel prepared in Preparation Example 5 was used, to which chitosan powder and graphene were not added. Compared with Application Example 1, the foaming density of the foamed particle molded body did not change much, but the fusion rate and tensile strength decreased, indicating that graphene and chitosan powder can increase the structural stability of the nanocellulose organogel, thereby improving the fusion strength of the foamed particle molded body.
[0098] Compared with Application Example 1, Application Examples 6 and 7 further pre-treated the polytetrafluoroethylene fiber by using hydrophobically modified silica and polylactic acid. The pore density of the foamed particle molded bodies prepared in Application Examples 6 and 7 increased, the tensile strength and elongation at break increased, and the welding strength was further improved.
[0099] Compared with Application Example 6, Application Example 8 does not add hydrophobically modified silica to the coating liquid, and the silica in Application Example 9 is not hydrophobically modified. The pore density of the foamed particle molding in Application Example 8 is reduced, and the mechanical strength is deteriorated, while the decrease in properties such as pore density and tensile strength in Application Example 9 is smaller than that in Application Example 8, indicating that hydrophobic modification can increase the effect of silica on the pore opening effect and mechanical strength.
[0100] In Application Example 10, polyvinyl alcohol aqueous solution is used instead of polylactic acid solution, and the welding rate of the foamed particle molding is significantly reduced, and the pore density, tensile strength and elongation at break are reduced, indicating that the addition of polylactic acid can improve the foaming density and welding strength of thermoplastic foamed particles.
[0101] Compared with Application Example 6, Application Examples 11 and 12 also pre-treat the polytetrafluoroethylene fibers with POE or the like before applying the coating liquid. The tensile strength and elongation at break of the foamed particle moldings made in Examples 11 and 12 are significantly improved, and the welding rate is increased.
[0102] In Application Example 13, no ethylene-glycidyl methacrylate copolymer was added. As shown in Table 1, the tensile strength and elongation at break of the foamed particle molded body prepared in Application Example 13 decreased, and the strength after welding decreased.
[0103] Application Example 14 uses the thermoplastic foamed particles prepared in Comparative Example 1, in which no polytetrafluoroethylene fibers are added. The foamed particle molded body prepared in Application Example 14 has a significantly reduced welding rate, and also weakened tensile strength and elongation at break.
[0104] Application Example 15 uses the thermoplastic foamed particles prepared in Comparative Example 2. Compared with Application Example 1, the pore density of the foamed particle molded body prepared in Application Example 15 is reduced, foaming molding is difficult, and it is difficult to maintain a complete pore structure, indicating that the addition of polylactic acid can improve the open-cell properties of the foamed particles.
[0105] Application Example 16 uses the thermoplastic foamed particles prepared in Comparative Example 3, in which no nanocellulose organic gel is added. Compared with Application Example 1, the foaming density of the foamed particle molded body prepared in Application Example 16 decreases, and the welding rate and mechanical strength are weakened, indicating that the nanocellulose organic gel can improve the melt strength of the foamed particles, maintain the pore shape, and increase the pore density.
[0106] In Application Example 17, the foamed particles prepared in Comparative Example 4 are used. Comparative Example 4 is the prior art. Compared with Application Example 1, the foamed particle molded body prepared in Application Example 17 has a reduced pore density and weakened mechanical properties.
[0107] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.
Claims
1. A thermoplastic foamed particle, characterized in that: The invention comprises the following components in parts by weight: 6-9.5 parts of thermoplastic polyurethane elastomer, 1.5-4 parts of polylactic acid, 0.6-1.4 parts of chain extender, 1.2-3.2 parts of nanocellulose organogel, and 2-4 parts of polytetrafluoroethylene fiber; The method for preparing the thermoplastic foamed particles comprises the following steps: The polylactic acid and nanocellulose organogel are mixed, extruded and granulated to obtain modified polylactic acid; The modified polylactic acid, thermoplastic polyurethane elastomer, chain extender and polytetrafluoroethylene fiber are mixed, extruded and granulated to obtain polymer pellets; Heat the autoclave to the foaming temperature, add polymer pellets, introduce carbon dioxide to exclude air, close the autoclave, introduce high-pressure carbon dioxide gas to the foaming pressure, foam, release the pressure to atmospheric pressure within 0.5-1s, cool, and obtain thermoplastic foamed particles, wherein the pressure is 14-20MPa, the foaming temperature is 160-180°C, and the foaming time is 3-4h.
2. The thermoplastic foamed particles according to claim 1, characterized in that: The polytetrafluoroethylene fiber is pretreated as follows: The silicon dioxide is hydrophobically modified to obtain hydrophobically modified silicon dioxide; Dissolving polylactic acid to prepare a polylactic acid solution with a concentration of 13-15wt%, adding the hydrophobically modified silica to prepare a coating liquid, wherein the mass ratio of polylactic acid to hydrophobically modified silica is 1:(0.2-0.5); The coating liquid is evenly applied on the polytetrafluoroethylene fiber, and then the polytetrafluoroethylene fiber is placed in an ethanol solution, immersed for 5-10 minutes, washed, and dried. The mass ratio of the coating liquid to the polytetrafluoroethylene fiber is (0.3-0.5):
1.
3. The thermoplastic foamed particles according to claim 2, characterized in that Before being coated with the coating liquid, the polytetrafluoroethylene fiber is subjected to the following treatment: 0.4-0.6 parts of POE, 0.02-0.05 parts of ethylene-methacrylate copolymer, 0.2-0.5 parts of polyvinyl alcohol and 10 parts of water are mixed evenly by weight to prepare a treatment liquid, and the polytetrafluoroethylene fiber is added. After mixing evenly, it is filtered and dried. The mass ratio of the treatment liquid to the polytetrafluoroethylene fiber is (0.2-0.4):
1.
4. The thermoplastic foamed particles according to claim 2, characterized in that The hydrophobically modified silica is prepared by modifying hexamethyldisilazane.
5. The thermoplastic foamed particles according to claim 1, characterized in that: The nanocellulose organic gel comprises nanocellulose and graphene in a mass ratio of 1:0.1-0.
12.
6. The thermoplastic foamed particles according to claim 5, characterized in that The preparation method of the nanocellulose organogel is as follows: Dissolving nanocellulose in deionized water to prepare a dispersion with a mass fraction of 2-3%; Chitosan powder, graphene and anhydrous sodium sulfate are added to the dispersion, ultrasonicated for 2-5 minutes, injected into a mold for molding, and after molding, placed in 50-55°C water for curing and washing for 40-48 hours, frozen with liquid nitrogen for 1-1.5 hours, and then vacuum freeze-dried and crushed to obtain nanocellulose organogel. The mass ratio of chitosan, anhydrous sodium sulfate and dispersion is (0.01-0.03):(2-3):
1.
7. The thermoplastic foamed particles according to claim 1, characterized in that The chain extender is selected from at least one of ADR-4370 and 4,4'-diphenylmethane diisocyanate.
8. A foamed particle molded body, characterized in that: The thermoplastic foamed particles according to any one of claims 1 to 7 are filled in a mold for foaming.