A method for pre-treating pure cotton woven fabric with high-bottom whitening
Through the bleaching process of low alkali cold rolling pile and oxygen-induced double bleaching one-bath method, combined with wet merceration treatment, the problem of large strong damage and insufficient whiteness in the pretreatment of pure cotton shuttle fabrics is solved, and the whiteness of the whiteness is not white enough is achieved. Improved whiteness, wetting performance and elasticity simplifies process flow and reduces costs and pollution.
Patent Information
- Application Number
- CN202310075439.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-02-07
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2043-02-07
AI Technical Summary
The existing cotton shuttle fabric pretreatment process has problems such as large strength damage, insufficient whiteness, large pollution, long process and high cost.
The bleaching process of low alkali cold rolling pile pretreatment and oxygen-efficient double bleaching one-bath method are used, combined with wet merceration treatment, which achieves the high whiteness, wetting performance and elasticity of the fabric, while reducing fibers. Damage and pollution simplify the process flow.
It effectively reduces the strong damage of the fabric, improves the whiteness and wetting performance, improves the feel and elasticity, saves energy and water resources, simplifies the process flow, and is suitable for high-support yarn varieties and high-whiteness requirements.
Smart Images

Figure BDA0004065944070000061
Abstract
Description
Technical Field
[0001] The invention relates to a high-bottom-white pretreatment method for pure cotton woven fabrics, belonging to the technical field of dyeing and finishing. Background Art
[0002] Pretreatment is an important process for dyeing and finishing pure cotton woven fabrics. It is not only the main production process of natural white products, whitening and extra white products, but also the key process to provide good semi-finished products for dyeing varieties. The quality indicators of pretreatment such as whiteness, wetting performance, strength, etc. directly affect the wearing performance and grade of the final product.
[0003] The pre-treatment process of pure cotton woven fabrics includes desizing, scouring and bleaching. Most traditional pre-treatment processes use alkali rolling high-temperature steam desizing, scouring, and high-temperature steam oxygen bleaching processes, which cause great damage to the fabric strength, poor hand feel, large consumption of water, electricity and steam, large sewage discharge, and high cost. For high-count yarn varieties with low strength and non-ironing finishing, post-baking of ready-made garments, and non-ironing varieties with high strength requirements, it is difficult to meet the wearing performance requirements. For bleached white and extra-white fabrics with relatively high whiteness requirements and light-colored fabrics with bright colors, even if the amount of hydrogen peroxide is increased or a bleaching process is added, the whiteness cannot meet the requirements and the fiber damage is increased.
[0004] Although the bio-enzyme pretreatment process can reduce the strong damage to cotton fibers, there are still many problems, such as unsatisfactory removal of PVA slurry, low removal efficiency of cottonseed hulls and pectin substances, and difficulty in unifying the application conditions of various enzyme preparations. This limits the application scope of bio-enzymes to a certain extent, and the strong alkali pretreatment process is still used in actual production.
[0005] The cold pad-batch pretreatment process has a mild effect and causes less damage to the fiber than the traditional hot alkali bath process. It is an economical, environmentally friendly, simple and easy short-process process. However, the existing conventional cold pad-batch pretreatment process also has the problems of using a high concentration of caustic soda, a high alkali content in the wastewater, low fabric whiteness, poor hair effect, and unsatisfactory impurity removal effect. It often cannot meet the requirements of dyeing and printing and requires steaming and oxygen bleaching processes. There is also the problem of greater fiber damage caused by increasing the amount of hydrogen peroxide and alkali agent used to improve whiteness. Summary of the invention
[0006] [Technical issues]
[0007] The existing technology has the problems of great strength damage to pure cotton fabrics, insufficient whiteness, great pollution, long process and high cost in the pretreatment process of pure cotton woven fabrics.
[0008] [Technical solution]
[0009] In view of the defects and shortcomings of the prior art, the present invention provides a high-bottom-white pretreatment method for pure cotton woven fabrics, which can effectively solve the problems of great strength damage, insufficient whiteness, great pollution, long process and high cost in the current pretreatment process of pure cotton woven fabrics.
[0010] The present invention uses a one-bath de-boiling, bleaching and low-alkali cold pad-batch pre-treatment process to effectively reduce the strong damage of the fabric while having good whiteness and wetting performance; through a one-bath sub-oxygen double bleaching bleaching process, sub-oxygen bleaching and oxygen bleaching are combined to greatly reduce the strong damage of the fabric caused by the traditional oxygen bleaching process; the scouring and bleaching are combined to further remove impurities such as cottonseed hulls, lignin and pectin remaining in the one-bath de-boiling, bleaching and low-alkali cold pad-batch pre-treatment process; the whiteness, wetting performance, feel and elasticity of the fabric are improved, and the process flow is short.
[0011] The object of the present invention is to provide a method for pre-treating pure cotton woven fabric with high bottom whitening, the method comprising the following steps:
[0012] (1) Low-alkali cold pad-batch pretreatment using one-bath deboiling and bleaching method
[0013] The pure cotton grey fabric is double dipped and double rolled, and the dipped and rolled pure cotton grey fabric is wrapped with a plastic film to keep it moist; then cold stacked; and washed with water after stacking;
[0014] The double dipping and double rolling working solution is prepared as follows: an aqueous solution prepared from 10-20 g / L sodium hydroxide, 10-20 g / L hydrogen peroxide, 4-6 g / L multifunctional refining agent, and 20-30 g / L clean cotton element;
[0015] (2) Wet mercerization
[0016] Mercerizing the washed pure cotton fabric in step (1);
[0017] (3) Suboxide double bleaching one-bath bleaching treatment
[0018] The pure cotton grey fabric after the wet mercerization treatment in step (2) is placed in an air flow cylinder for bleaching treatment, and then washed and dried after the bleaching treatment;
[0019] The working solution for bleaching treatment comprises: 80% sodium chlorite by mass: 2-8 g / L, activator ammonium sulfate: 2-8 g / L, 30% hydrogen peroxide: 2-5 g / L, refining penetrant: 2-3 g / L, bath ratio: 1:5-9, and glacial acetic acid is used to adjust the pH value to 3.5-4.0.
[0020] In one embodiment, the working liquid temperature of the double dipping and double rolling in step (1) is 50-60° C., and the liquid rate after dipping and rolling is 80%-110%.
[0021] In one embodiment, the cold stacking conditions in step (1) are as follows: the temperature is 30° C. to 40° C.; the rotation speed of the stacked cloth rolls is 5 to 10 rpm; and the stacking time is 24 to 30 hours.
[0022] In one embodiment, the water washing temperature in step (1) is 60-90°C, and there are 6 washing boxes; the water washing temperatures of the first 4 sections are all 90°C, and the water washing temperatures of the last 2 sections are all 60°C; after washing (without drying), the liquid carrying rate of the fabric is 20%.
[0023] In one embodiment, the mercerization finishing in step (2) is specifically as follows: a cloth clip mercerizing machine is used, the machine speed is 70±5m / min, the mercerizing alkali concentration is (NaOH) 170-180g / L, the temperature of the water washing box before the alkali tank is 95°C, the liquid rate of the fabric after rolling in 1# and 2# alkali tanks is 73%-78%, the rolling in 3# alkali tank is 4kg, and the temperature of the flushing alkali water is 75°C-85°C.
[0024] In one embodiment, the bleaching conditions of the air flow cylinder in step (3) are: temperature 90°C to 100°C, time 80min to 100min, and heating rate 1 to 3°C / min.
[0025] In one embodiment, the water washing temperature in step (3) is 80°C to 100°C, the time is 10min to 15min, and the water washing is performed 2 to 3 times.
[0026] Another object of the present invention is to provide an application of the above-mentioned pure cotton fabric high bottom white pre-treatment method in fabric finishing.
[0027] [Beneficial Effects]
[0028] (1) The present invention systematically reduces the problem of large strength damage in the current pre-treatment process through a one-bath low-alkali cold pad-batch pre-treatment process of descaling and bleaching and a one-bath bleaching process of sub-oxygen double bleaching. The cotton fabric pre-treated by the present invention has small strength damage, and is particularly suitable for high-count pure cotton varieties, non-ironing finishing with high strength requirements, post-baking of ready-made garments, and non-ironing varieties of ready-made garments; it has the advantages of energy saving and emission reduction, economy, short process, and simple operation.
[0029] (2) The pure cotton woven fabric high-bottom white pretreatment process of the present invention solves the contradiction between whiteness improvement and strong damage of semi-finished products after the current pretreatment process through the sub-oxygen double bleaching one-bath bleaching process. The cotton fabric after the pretreatment of the present invention has the advantages of high whiteness, good wetting performance, soft hand feeling and good elasticity, and is particularly suitable for the requirements of raw white, extra white fabrics and bright light-colored fabrics.
[0030] (3) The present invention adopts mercerization before bleaching to reduce the influence of the mercerization process on whiteness, and adopts wet mercerization to avoid surface mercerization, improve mercerization uniformity, save a drying process that affects the whiteness of the fabric, and save energy consumption. DETAILED DESCRIPTION
[0031] Unless otherwise specified, the process methods used in the following examples are conventional methods.
[0032] 1. Determination method of whiteness
[0033] The test was conducted in accordance with GB / T 8424.2-2001 “Textile Colour Fastness Tests - Instrumental Assessment of Relative Whiteness”. Specifically, each pre-treated fabric sample was folded twice to form a four-layer opaque sample, and the test was conducted at different locations on the fabric surface.
[0034] 2. Tensile strength measurement
[0035] The test method is in accordance with GB / T 3923.1-2013 Tensile properties of textile fabrics Part 1: Determination of breaking strength and elongation at break (strip method).
[0036] 3. Tear strength measurement
[0037] The test method is in accordance with GB / T 3917.1-2009 Tear properties of textile fabrics Part 1: Determination of tear strength by impact pendulum method.
[0038] 4. Gross effect test
[0039] Refer to FZ / 01071-2008 "Test Method for Capillary Effect of Textiles", measure the height of distilled water rising along the fabric within 30 minutes, and take the average of 3 times. Cut the fabric into strips of 25cm×3cm (warp×weft), fix one end on the rack, let it droop naturally, clamp a certain mass of clip at the end to ensure that the fabric is naturally placed vertically in the water, and measure the height of the liquid rising at 3min and 30min.
[0040] Multifunctional refining agent: the main ingredient is fatty alcohol polyoxyethylene ether, purchased from Hangzhou Doen Textile Technology Co., Ltd.;
[0041] Cotton-free: main ingredients: sodium gluconate and soda ash, purchased from Qingdao Fukai Rubber & Plastic New Materials Co., Ltd.
[0042] Refined penetrant: main ingredients are sodium dodecylbenzene sulfonate, fatty alcohol polyoxyethylene ether, polyoxyethylene oleate; purchased from Hangzhou Doen Textile Technology Co., Ltd.
[0043] Example 1
[0044] The pure cotton woven fabric involved in this embodiment is specifically a pure cotton grey fabric with specifications of 100S / 2*100S / 2*137 strands / inch*100 strands / inch, 3 / 1 twill, and a grey fabric width of 165 cm.
[0045] A pure cotton woven fabric high-bottom white pre-treatment process specifically comprises the following steps:
[0046] (1) Low-alkali cold pad-batch pretreatment using one-bath deboiling and bleaching method
[0047] The singed pure cotton grey fabric rolls are dipped into the working liquid: the padding is double dipped and double rolled, the padding working liquid temperature is 55°C, and the liquid carrying rate after padding is 90%; the padded pure cotton fabric is rolled up and wrapped with a plastic film to keep it moist; then cold stacking is carried out, and the cold stacking temperature is 30°C; the speed of the stacked fabric rolls is 8 rpm; the stacking time is 28 hours; then washing is carried out, the washing temperature is 90°C, and 6 washing boxes (the washing temperatures of the first 4 sections are all 90°C, and the washing temperatures of the last 2 sections are all 60°C); the liquid carrying rate of the fabric after washing (without drying) is 20%;
[0048] The padding working solution is prepared by: an aqueous solution prepared from 15 g / L sodium hydroxide, 15 g / L hydrogen peroxide, 4 g / L multifunctional refining agent, and 24 g / L pure cotton.
[0049] (2) Wet mercerization
[0050] The fabric washed in step (1) is mercerized; the mercerization is performed using a cloth clip mercerizer, the machine speed is 70±5m / min, the mercerization alkali concentration is (NaOH) 180g / L, the width of the machine during mercerization is 165cm, the temperature of the washing box before the alkali tank is 95°C, the liquid carrying rate of the fabric after rolling in 1# and 2# alkali tanks is 78%, the rolling pressure in 3# alkali tank is 4kg, and the temperature of the flushing alkali water is 75°C.
[0051] (3) Suboxide double bleaching one-bath bleaching treatment
[0052] The fabric after the wet mercerization treatment in step (2) is placed in an air flow cylinder for bleaching treatment, treated at 90°C for 90 minutes, and the heating rate is 2°C / min; the working liquid in the air flow cylinder includes 4 g / L of sodium chlorite with a mass fraction of 80%, 4 g / L of ammonium sulfate as an activator, 1.5 g / L of hydrogen peroxide, 1.5 g / L of a refining penetrant, a bath ratio of 1:7, and the pH value is adjusted to 3.5-4.0 with glacial acetic acid;
[0053] (4) Washing: Wash in air flow cylinder at 80℃ for 15min, wash twice and dry.
[0054] Example 2
[0055] The pure cotton woven fabric involved in this embodiment is specifically a pure cotton grey fabric with specifications of 80S / 2*80S / 2*144 strands / inch*72 strands / inch, flat weft weight, and a grey fabric width of 162.5 cm.
[0056] A pure cotton woven fabric high-bottom white pre-treatment process specifically comprises the following steps:
[0057] (1) Low-alkali cold pad-batch pretreatment using one-bath deboiling and bleaching method
[0058] The singed pure cotton grey cloth roll is dipped into the working liquid: the padding is double dipped and double rolled, the padding working liquid temperature is 55°C, and the liquid carrying rate after padding is 90%; the cotton fabric after padding is rolled up and wrapped with a plastic film to keep it moist; then cold stacking is carried out, and the cold stacking temperature is 32°C; the speed of the stacked cloth roll is 8 rpm; the stacking time is 24 hours; then washing is carried out, the washing temperature is 90°C, and 6 washing boxes (the washing temperature of the first 4 sections is 90°C, and the washing temperature of the last 2 sections is 60°C); after washing (without drying), the fabric liquid carrying rate is 20%;
[0059] The padding working solution is prepared by: an aqueous solution prepared from 18 g / L sodium hydroxide, 18 g / L hydrogen peroxide, 4 g / L multifunctional refining agent, and 24 g / L pure cotton.
[0060] (2) Wet mercerization
[0061] The fabric washed in step (1) is mercerized. The mercerization is performed using a clip mercerizer, with a speed of 70±5 m / min, a mercerization alkali concentration of (NaOH) 180 g / L, a width of 165 cm during mercerization, a temperature of 95°C for the washing box before the alkali tank, a liquid rate of 78% for the fabric after rolling in the 1# and 2# alkali tanks, a rolling pressure of 4 kg in the 3# alkali tank, and a temperature of 85°C for the flushing alkali water.
[0062] (3) Suboxide double bleaching one-bath bleaching treatment
[0063] The fabric after the wet mercerization treatment in step (2) is placed in an air flow cylinder for bleaching treatment, treated at 90°C for 90 minutes, and the heating rate is 2°C / min; the working liquid in the air flow cylinder includes 5 g / L of sodium chlorite with a mass fraction of 80%, 4 g / L of ammonium sulfate as an activator, 2 g / L of hydrogen peroxide, 2 g / L of a refining penetrant, a bath ratio of 1:7, and the pH value is adjusted to 3.5-4.0 with glacial acetic acid;
[0064] (4) Washing: Wash in air flow cylinder at 80℃ for 10min, wash twice and dry.
[0065] Comparative Example 1
[0066] The difference from Example 1 is that the step (3) oxygen bleaching in one bath is adjusted to oxygen bleaching + oxygen bleaching in two steps, and the other conditions are the same as those in Example 1. The specific steps are: oxygen bleaching → neutralization washing → oxygen bleaching → washing.
[0067] Sub-bleaching: the fabric after the wet mercerization treatment in step (2) is placed in an air flow cylinder for sub-bleaching treatment, treated at 90°C for 90 min, and the heating rate is 2°C / min; the working liquid in the air flow cylinder includes 80% sodium chlorite: 5g / L, activator ammonium sulfate: 4g / L, refining penetrant: 2g / L, bath ratio: 1:7, and the pH value is adjusted to 3.5 with glacial acetic acid.
[0068] Neutralization water washing: baking soda (sodium thiosulfate) 1.5g / L, temperature 80℃, time 15min.
[0069] Oxygen bleaching: Oxygen bleaching bath ratio 1:10, multifunctional refining agent 2g / L, hydrogen peroxide 5g / L, clean cotton 7g / L, adjust pH value to 10.5-11 with NaOH, temperature 98℃ (heating rate 2℃ / min), time 60min.
[0070] Washing: Wash in air flow cylinder at 80℃ for 10min, wash twice and dry.
[0071] Comparative Example 2
[0072] The difference from Example 1 is that the step (3) of oxygen double bleaching in one bath is adjusted to steam oxygen bleaching using only a long vehicle, and the other conditions are the same as those in Example 1; the specific steps are: padding oxygen bleaching liquid → stacking steaming → water washing.
[0073] The fabric treated with wet mercerization in step (2) is subjected to steaming oxygen bleaching treatment using a long car, with a stacking temperature of 98°C and a stacking steaming time of 30 minutes; the oxygen bleaching working solution is 9g / L hydrogen peroxide; the pH value is adjusted to 10.5-11 with NaOH; the multifunctional refining agent is 2g / L; and the clean cotton element is 8g / L.
[0074] Water washing: air flow cylinder water washing, water washing temperature is 90℃, 6-section water washing box (the first 4 sections are 90℃, the last 2 sections are 60℃).
[0075] Comparative Example 3
[0076] The difference from Example 1 is that the step (3) of oxygen-oxygen double bleaching in one bath bleaching is adjusted to only oxygen-oxygen bleaching, and the other conditions are the same as those in Example 1; the specific steps are: oxygen-oxygen bleaching → neutralization washing.
[0077] Sub-bleaching: placing the fabric after the wet mercerization treatment in step (2) in an air flow cylinder for sub-bleaching treatment, treating at 90°C for 90 min, with a heating rate of 2°C / min; the working liquid in the air flow cylinder includes 80% sodium chlorite: 8 g / L, activator ammonium sulfate: 8 g / L, refining penetrant: 2 g / L, bath ratio: 1:7, and adjusting the pH value to 3.5-4.0 with glacial acetic acid.
[0078] Neutralization water washing: baking soda (sodium thiosulfate) 3g / L, temperature 80℃, time 15min.
[0079] The properties of the pure cotton woven fabrics treated in Example 1 and Comparative Examples 1 to 3 were measured, and the results are shown in Table 1:
[0080] Table 1 Effect of semi-finished products after pretreatment of the present invention
[0081]
[0082] From the data in Table 1, it can be seen that the strength, whiteness and wool effect of the semi-finished products treated by the high-bottom white pretreatment process of pure cotton woven fabrics of the present invention are better than those of the two-step bleaching process of deboiling, boiling and bleaching, one-bath low-alkali cold pad-batch pretreatment + sub-bleaching + oxygen bleaching, deboiling, boiling and bleaching, one-bath low-alkali cold pad-batch pretreatment + long-car steaming oxygen bleaching, and deboiling, boiling and bleaching, one-bath low-alkali cold pad-batch pretreatment + sub-bleaching. In particular, the tear strength is improved by about 11% compared with the sub-bleaching + oxygen bleaching process, about 17% compared with the long-car steaming oxygen bleaching process, and about 8% compared with the sub-bleaching process.
Claims
1. A method for pre-treatment of pure cotton woven fabrics with high bottom whitening, characterized in that: The method comprises the following steps: (1) Low-alkali cold pad-batch pretreatment using one-bath deboiling and bleaching method The pure cotton grey fabric is double dipped and double rolled, and the dipped and rolled pure cotton grey fabric is wrapped with a plastic film to keep it moist; then cold stacked; and washed with water after stacking; The double dipping and double rolling working solution is prepared as follows: an aqueous solution prepared from 15-18 g / L sodium hydroxide, 15-18 g / L hydrogen peroxide, 4-6 g / L multifunctional refining agent, and 20-30 g / L clean cotton element; The cold stacking conditions are as follows: the temperature is 30°C to 40°C; the rotation speed of the stacked cloth rolls is 5 to 10 rpm; and the stacking time is 24 to 30 hours; (2) Wet mercerization The pure cotton grey fabric washed in step (1) is mercerized; the specific steps of the mercerization finishing are: mercerization finishing is performed using a cloth clip mercerizing machine, the machine speed is 70±5m / min, the concentration of mercerizing alkali NaOH is 170-180g / L, the temperature of the washing box before the alkali tank is 95°C, the liquid carrying rate of the fabric after rolling in the alkali tank is 73%-78%, and the temperature of the flushing alkali water is 75°C-85°C; (3) Suboxide double bleaching one-bath bleaching treatment The pure cotton grey fabric after the wet mercerization treatment in step (2) is placed in an air flow cylinder for bleaching treatment, and then washed and dried after the bleaching treatment; The working solution for bleaching treatment comprises: 80% sodium chlorite by mass: 2-8 g / L, activator ammonium sulfate: 2-8 g / L, 30% hydrogen peroxide: 2-5 g / L, refining penetrant: 2-3 g / L, bath ratio: 1:5-9, and glacial acetic acid is used to adjust the pH value to 3.5-4.
0.
2. The method according to claim 1, characterized in that The working liquid temperature of the double dipping and double rolling in step (1) is 50-60° C., and the liquid rate after dipping and rolling is 80%-110%.
3. The method according to claim 1, characterized in that The water washing temperature in step (1) is 60-90°C, and there are 6 water washing boxes; the water washing temperatures of the first 4 sections are all 90°C, and the water washing temperatures of the last 2 sections are all 60°C.
4. The method according to claim 1, characterized in that: After the washing in step (1), the liquid carrying rate of the pure cotton fabric is 20%.
5. The method according to claim 1, characterized in that The bleaching conditions of the air flow cylinder in step (3) are: temperature 90°C to 100°C, time 80min to 100min, and heating rate 1 to 3°C / min.
6. The method according to claim 1, characterized in that The water washing temperature in step (3) is 80°C to 100°C, the time is 10min to 15min, and the water washing is performed 2 to 3 times.
7. Use of the high-bottom-white pretreatment method for pure cotton woven fabrics according to any one of claims 1 to 6 in fabric finishing.
Citation Information
Patent Citations
Ultra-low shrinkage rate purified cotton lining cloth and production method thereof
CN101353842A
Sodium chlorite-hydrogen peroxide bleaching integrated bath process of flax
CN102691113A
Non-steaming cold pad-batch process of all-cotton or polyester-cotton fabric
CN102817240A
Textile continuous cold-batch pretreatment method, auxiliary used for method and preparation method of auxiliary
CN103147276A
Fast turquoise shades on cellulose fibres - obtained by dyeing with CI sulphur green 25 type dyes, alkylation and oxidn.
DE2343091A1