A continuous multi-level porous titanium carbide conductive fiber and its preparation method and application

By preparing mesoporous titanium carbide powder and PMMA microspheres, multi-stage porous titanium carbide conductive fibers were constructed, which solved the problems of high electrode density and ion channel blocking of Ti3C2Tx fibers, and achieved high electrochemical performance and fast ion response.

CN116024699BActive Publication Date: 2024-11-19SHANGHAI UNIV OF ENG SCI
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211626916.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-16
Publication Date
2024-11-19
Estimated Expiration
2042-12-16

AI Technical Summary

Technical Problem

The internal assembly density of existing Ti3C2Tx fiber electrodes is too high, the utilization rate of active materials is low, and the ion channels inside the fibers are easily blocked by stacked sheets, resulting in low energy density. Research on the construction of macroporous structure of traditional mesoporous Ti3C2Tx fibers Imature.

Method used

By preparing mesoporous titanium carbide powder and PMMA microspheres, placing fiber spinning raw liquid, wet spinning and sintering, a continuous multi-stage porous titanium carbide conductive fiber is constructed, and the number of ion channels of the fiber is increased by using the mesoporous-macroporous structure and Electrochemical properties.

Benefits of technology

It improves the volume specific capacitance and electrochemical properties of the fiber, reduces the equivalent series resistance, enhances the ion response speed, and is suitable for industrial large-scale production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116024699B_ABST
    Figure CN116024699B_ABST
Patent Text Reader

Abstract

The present invention discloses a continuous multi-level porous titanium carbide conductive fiber and a preparation method and application thereof, belonging to the technical field of functional materials. x The sheet layer was treated with surface pores, and a multi-level porous fiber with a mesoporous-macroporous structure was prepared by the PMMA nano-microsphere hard template method, thereby further improving the volume specific capacitance of the fiber and solving the problem of Ti3C2T x The problem of poor electrochemical performance of conductive fibers. The continuous multi-level porous titanium carbide conductive fiber provided by the present invention constructs a multi-level pore structure of mesopores and macropores, which not only shows better electrochemical performance, but also improves the self-stacking defects between materials, increases the space inside the fiber, and the unique pore structure increases the ion transfer channel, thereby improving the transmission efficiency of electrons and ions.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of functional materials, and relates to a continuous multi-level porous titanium carbide conductive fiber and a preparation method and application thereof, and specifically relates to a mesoporous Ti3C2T x Preparation of sheet materials, preparation of hard template PMMA nanospheres, and a method for continuously and quickly preparing conductive fibers based on this, and applying the prepared fibers in the field of flexible electrode materials. Background Art

[0002] With the development of science and technology, the rise of portable and wearable devices has put forward new requirements for the capacity, volume and mechanical properties of energy storage devices. In recent years, wearable microelectronic devices such as artificial skin, wearable physiological monitoring equipment, and flexible sensors have been continuously developed, and there is an urgent need for energy supply devices with sufficient capacity, flexibility, and durability. At present, the main forms of flexible energy storage devices include flexible metal ion batteries, metal-air batteries, and supercapacitors. Fiber-based supercapacitors have the characteristics of high power density, fast charging and discharging speed, long cycle life, and safer and more stable. They also have good flexibility of fiber structure and can be easily woven into various types of textiles, thereby maximizing the comfort, aesthetics and designability of wearable electronic devices, showing great potential for wearable applications.

[0003] Based on Ti3C2T x MXenes are a new type of two-dimensional sheet material that exhibits high electrical conductivity and fast ion diffusion due to its unique crystal structure, making them very attractive for energy storage applications. x The nanosheets have small lateral dimensions and weak interaction between the sheets. x Nanosheets are difficult to assemble into macroscopic fibers individually.

[0004] Currently commonly used Ti3C2T x The preparation method of the fiber mainly adopts the methods of blending and electrostatic spinning. For example, the patent with the publication number CN109898179A provides a preparation method of titanium carbide fiber material, which mixes the titanium-containing polymer precursor solution obtained after the polycondensation of organic matter with polyvinyl pyrrolidone and stirs it evenly to obtain a stable spinning solution, and then electrostatically spins it. The spun fiber is heat-treated and then carbon-thermally reduced to obtain titanium carbide fiber, which solves the problems of poor stability of fiber precursor, complex process, and inability to prepare continuous long fibers. However, the problems of too high internal assembly density and low utilization rate of active materials in electrodes based on titanium carbide fibers still exist, which limits its practical application.

[0005] In response to the above problems, the existing patent with publication number CN112062230A provides an electrode material and a preparation method thereof. The patent designs the fiber electrode into a multilayer cavity structure consisting of a metal oxide layer, a carbon fiber matrix layer, and a MXene layer, and combines the technology of capacitive deionization to improve the electrode's large-capacity ion storage capacity, conductivity, and hydrophilicity. However, the preparation method provided by the patent has complicated steps, especially the operation of coating the MXene nanosheets on the fiber surface and drying it needs to be repeated many times, which is not suitable for industrial large-scale production.

[0006] In addition, the existing technology based on Ti3C2T x The fibers of the sheets all use non-mesoporous sheets, and the ion channels inside the fibers are easily blocked by the stacked sheets, resulting in a low energy density of the fiber electrode. The use of mesoporous sheet materials to prepare fibers can effectively increase the number and pass rate of ion channels in the fibers. In addition to selecting suitable fiber electrode materials, constructing a multi-level pore structure in the fiber can also give the material a larger specific surface area and more electrochemical reaction active sites, and also provide an effective way for the rapid diffusion of ions. Among them, the large-pore structure with open space (pore size > 50nm) can not only provide more locations for the rapid embedding and de-embedding of active substances, but also act as an ion buffer reservoir, which can greatly reduce the diffusion distance of ions in the electrolyte, which is beneficial to the capacitance output under high current density. In traditional membrane materials, such as graphene membranes, MXene membranes, etc., the technology of using hard templates to prepare large-pore structures is relatively mature, but currently in mesoporous Ti3C2T x The research on constructing macroporous structure in fibers is not mature yet, so it is necessary to provide a method for preparing continuous multi-level porous titanium carbide conductive fibers to solve the above problems. Summary of the invention

[0007] The present invention is to solve the existing continuous mesoporous Ti3C2T x The shortcomings of the fiber are overcome, and a method for preparing a continuous multi-level porous titanium carbide conductive fiber is provided.

[0008] The technical solution provided by the present invention is as follows:

[0009] A method for preparing continuous multi-level porous titanium carbide conductive fiber, comprising the following steps:

[0010] S1, prepare titanium carbide powder; S2, prepare mesoporous titanium carbide powder; S3, prepare PMMA microspheres; S4, prepare fiber spinning solution with titanium carbide powder, mesoporous titanium carbide powder and PMMA microspheres as raw materials, wash and sinter the obtained fibers after wet spinning to obtain titanium carbide conductive fibers.

[0011] As a preferred scheme for the preparation method of the continuous multi-level porous titanium carbide conductive fiber of the present invention, S1 is specifically: adding lithium fluoride powder to hydrochloric acid, stirring continuously for sufficient reaction, adding aluminum titanium carbide, stirring and reacting in a 35-40°C oil bath for 24 hours, centrifuging after the reaction, washing the reactant with deionized water until the upper layer of the solution is dark green and the pH is 6-7, ultrasonically treating the upper layer in an ice bath, collecting the supernatant by centrifugation, and continuing to centrifuge the supernatant, freeze-drying the upper layer into powder to obtain titanium carbide powder.

[0012] As a preferred solution of the method for preparing the continuous multi-level porous titanium carbide conductive fiber of the present invention, the mass ratio of lithium fluoride to aluminum titanium carbide is 1.6:1.

[0013] As a preferred embodiment of the method for preparing the continuous multi-level porous titanium carbide conductive fiber of the present invention, the concentration of hydrochloric acid is 9 mol / L and the amount used is 20 mL.

[0014] As a preferred embodiment of the method for preparing the continuous multi-level porous titanium carbide conductive fiber of the present invention, the ice bath ultrasonic treatment time is 2 hours.

[0015] As a preferred solution of the method for preparing the continuous multi-level porous titanium carbide conductive fiber of the present invention, the centrifugation time of the upper liquid is 5 minutes and the rotation speed is 7000 rpm.

[0016] As a preferred scheme for the preparation method of the continuous multi-level porous titanium carbide conductive fiber of the present invention, S2 is specifically: dispersing titanium carbide powder in deionized water, adding an equal volume of copper sulfate solution, stirring for 30 minutes, repeatedly centrifuging and washing with deionized water until the pH value of the solution is 6, adding hydrogen fluoride to the solution, etching for 10 minutes, ultrasonically dispersing, centrifuging and washing until the upper layer of liquid is dark green, taking the upper layer of liquid and freeze-drying it into powder to obtain mesoporous titanium carbide powder.

[0017] As a preferred embodiment of the method for preparing the continuous multi-level porous titanium carbide conductive fiber of the present invention, the concentration of the copper sulfate solution is 0.2 mol / L.

[0018] As a preferred solution of the method for preparing the continuous multi-level porous titanium carbide conductive fiber of the present invention, the mass concentration of the hydrogen fluoride solution is 10%.

[0019] As a preferred solution of the method for preparing the continuous multi-level porous titanium carbide conductive fiber of the present invention, titanium carbide powder is dispersed in deionized water at a rotation speed of 3500-4000 rpm.

[0020] As a preferred scheme for the preparation method of the continuous multi-level porous titanium carbide conductive fiber of the present invention, S3 is specifically: dissolving azoisobutyronitrile and polyvinyl pyrrolidone in methanol, adding methyl methacrylate after purging the mixed solution with nitrogen, stirring the reaction, centrifuging and washing, and obtaining a white product as PMMA microspheres.

[0021] As a preferred solution of the method for preparing the continuous multi-level porous titanium carbide conductive fiber of the present invention, the mass concentration of azoisobutyronitrile in the mixed solution is 0.1%, and the mass concentration of polyvinyl pyrrolidone is 4%.

[0022] As a preferred embodiment of the method for preparing the continuous multi-level porous titanium carbide conductive fiber of the present invention, the reaction temperature is 50-60°C.

[0023] As a preferred solution of the method for preparing the continuous multi-level porous titanium carbide conductive fiber of the present invention, the mass fraction of the added methyl methacrylate is 10-15%.

[0024] As a preferred scheme for the preparation method of the continuous multi-level porous titanium carbide conductive fiber of the present invention, S4 is specifically: dispersing titanium carbide powder and mesoporous titanium carbide powder in water, and at the same time dispersing the PMMA nanospheres prepared in S5 in water by ultrasonicating with an ultrasonic crusher for 30 minutes, and mixing the two to form a fiber spinning solution, and injecting the fiber spinning solution into a spinning tank equipped with a coagulation bath through a spinneret with model 23G at a spinning flow rate of 50 ml / h. After soaking for 20 minutes, the fiber is washed with sulfuric acid, ethanol solution and deionized water in turn, and after being fully dried, it is sintered to obtain titanium carbide conductive fiber.

[0025] As a preferred scheme for the preparation method of continuous multi-level porous titanium carbide conductive fiber of the present invention, the mixed concentration of titanium carbide and mesoporous titanium carbide in the spinning solution is 40-48 mg / mL, the mass fraction of mesoporous titanium carbide is 4-22%, and the concentration of PMMA microspheres is 8-12 mg / mL.

[0026] As a preferred solution of the method for preparing the continuous multi-level porous titanium carbide conductive fiber of the present invention, the mass fraction of the mesoporous titanium carbide is 4-6%, 8-12%, 13-17% or 18-22%.

[0027] As a preferred embodiment of the method for preparing the continuous multi-level porous titanium carbide conductive fiber of the present invention, the coagulation bath is a mixture of chitosan, acetic acid and deionized water.

[0028] As a preferred solution of the method for preparing the continuous multi-level porous titanium carbide conductive fiber of the present invention, the mass volume ratio of chitosan, acetic acid and deionized water is 2g:5mL:500mL, wherein the mass concentration of acetic acid is 36%.

[0029] As a preferred solution of the method for preparing the continuous multi-level porous titanium carbide conductive fiber of the present invention, the concentration of sulfuric acid used for washing is 1 mol / L, and the mass concentration of ethanol is 30%.

[0030] As a preferred solution of the method for preparing the continuous multi-level porous titanium carbide conductive fiber of the present invention, the sintering temperature is 500-650°C.

[0031] Another object of the present invention is to provide an application of the continuous multi-level porous titanium carbide conductive fiber obtained by the above-mentioned preparation method, specifically as a flexible electrode material.

[0032] Compared with the prior art, the present invention has the following beneficial effects:

[0033] (1) The present invention is based on Ti3C2T x The sheet layer was treated with surface pores, and a multi-level porous fiber with a mesoporous-macroporous structure was prepared by the PMMA nanosphere hard template method, thereby further improving the volume specific capacitance of the fiber and solving the problem of Ti3C2T x The problem of poor electrochemical performance of conductive fibers.

[0034] (2) The continuous multi-level porous titanium carbide conductive fiber provided by the present invention constructs a mesoporous-macroporous multi-level pore structure in structure. On the basis of the mesoporous titanium carbide fiber, it not only exhibits better electrochemical performance. In addition, the multi-level porous titanium carbide conductive fiber exhibits a lower equivalent series resistance and has a faster ion response. This is mainly because the preparation method, on the one hand, exerts the excellent physical and chemical properties of titanium carbide MXene itself, and on the other hand, improves the self-stacking defects between materials, increases the voids inside the fiber, and at the same time, the unique pore structure can increase the ion transfer channel and improve the transmission efficiency of electrons and ions. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] Figure 1 The preparation process and structural schematic diagram of the continuous multi-level porous titanium carbide conductive fiber provided by the present invention;

[0036] Figure 2 The optical morphology, Zeta potential and transmission electron microscopy images of the prepared mesoporous titanium carbide powder suspension;

[0037] Figure 3 The scanning electron microscope image of the prepared PMMA microspheres;

[0038] Figure 4 This is a scanning electron microscope image of the cross section of titanium carbide conductive fiber with a continuous multi-level pore structure;

[0039] Figure 5 This is a scanning electron microscope image of the cross section of the mesoporous titanium carbide conductive fiber prepared in Comparative Example 1. DETAILED DESCRIPTION

[0040] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the specific implementation methods of the present invention are described in detail below in conjunction with the embodiments of the specification.

[0041] In the following description, many specific details are set forth to facilitate a full understanding of the present invention, but the present invention may also be implemented in other ways different from those described herein, and those skilled in the art may make similar generalizations without violating the connotation of the present invention. Therefore, the present invention is not limited to the specific embodiments disclosed below.

[0042] Secondly, the term "one embodiment" or "embodiment" as used herein refers to a specific feature, structure, or characteristic that may be included in at least one implementation of the present invention. The term "in one embodiment" that appears in different places in this specification does not necessarily refer to the same embodiment, nor does it refer to a separate or selective embodiment that is mutually exclusive with other embodiments.

[0043] Unless otherwise specified, the raw materials used in the examples were purchased commercially.

[0044] Example 1

[0045] like Figure 1 As shown, the method for preparing continuous multi-level porous titanium carbide conductive fibers in this embodiment includes the following steps:

[0046] Step 1: Preparation of few-layer titanium carbide nanosheets: Add 1.6 g of lithium fluoride powder to 20 mL of 9 mol / L hydrochloric acid and stir for 5 min to allow for full reaction. Then add 1 g of aluminum titanium carbide and stir in a 35°C low-temperature oil bath for 24 h.

[0047] Step 2: Preparation of titanium carbide powder: Centrifuge at 3500 rpm and wash the reactants with deionized water several times until the upper layer of the solution is dark green (pH value is about 7). Then, ultrasonically treat the dispersion in an ice bath for 2 hours and collect the supernatant by centrifugation at 3500 rpm. Centrifuge the obtained upper layer at 7000 rpm for 5 minutes to obtain large-layer Ti3C2T x The nanosheets (upper layer of liquid) are freeze-dried into powder for later use.

[0048] Step 3: Preparation of mesoporous titanium carbide nanosheets: Take 100 mg of large Ti3C2T flakes obtained in step 2. xThe nanosheets were dispersed in 100 mL of deionized water and mixed with the same volume of 0.2 mol / L copper sulfate solution, stirred for 30 min using a magnetic stirrer, and then washed repeatedly by centrifugation with deionized water until the pH value of the solution reached 6.

[0049] Step 4, preparation of mesoporous titanium carbide powder: add 20mL of 10% hydrogen fluoride solution to the solution obtained in step 3, keep etching for 10 minutes and then ultrasonically disperse for 3 minutes, finally centrifuge and wash until the upper layer liquid is dark green (pH value between 5-6), take the upper layer liquid and freeze-dry it into powder for later use. The optical morphology, Zeta potential map and transmission electron microscopy map of the obtained mesoporous titanium carbide powder suspension are as follows: Figure 2 shown.

[0050] Step 5, Preparation of PMMA microspheres: Dissolve the free radical initiator (azoisobutyronitrile) and polyvinyl pyrrolidone as a stabilizer in methanol at room temperature at a mass fraction of 0.1% and 4%, respectively. Purge the solution with argon to remove oxygen from the mixture, and add 10wt.% of methyl methacrylate monomer (MMA). Then stir the reaction mixture at 50°C. After 24h, collect the white product by centrifugation and methanol washing. The obtained PMMA microspheres are shown in the scanning electron microscope image, as shown in the figure. Figure 3 shown.

[0051] Step six, preparation of continuous multi-level porous titanium carbide conductive fiber: disperse titanium carbide powder and mesoporous titanium carbide powder in water, and disperse PMMA nano-microspheres in water by ultrasonic crusher for 30 minutes, and mix the two to prepare a fiber spinning solution. The mixed concentration of titanium carbide and mesoporous titanium carbide in the spinning solution is 40 mg / mL, of which the mass fraction of mesoporous titanium carbide accounts for 15%, and the concentration of PMMA microspheres is 8 mg / mL. The fiber spinning solution is injected into a spinning tank equipped with a coagulation bath through a spinneret of model 23G at a spinning flow rate of 50 mL / h. After soaking for 20 minutes, the fiber is washed with sulfuric acid, ethanol solution and deionized water in turn. After sufficient drying, it is vacuum sintered at 550°C to obtain multi-level porous titanium carbide conductive fiber. The obtained multi-level porous titanium carbide fiber cross-section scanning electron microscope image is as follows Figure 4 As shown in Figure 2, PMMA microspheres are decomposed during the sintering process, leaving a regular spherical pore structure inside the fiber. The pore size can be adjusted by controlling the preparation parameters.

[0052] Comparative Example 1:

[0053] The method for preparing mesoporous titanium carbide conductive fibers in this comparative example comprises the following steps:

[0054] Step 1: Preparation of few-layer titanium carbide nanosheets: Add 1.6 g of lithium fluoride powder to 20 mL of 9 mol / L hydrochloric acid and stir for 5 min to allow for full reaction. Then add 1 g of aluminum titanium carbide and stir in a 35°C low-temperature oil bath for 24 h.

[0055] Step 2: Preparation of titanium carbide powder: Centrifuge at 3500 rpm and wash the reactants with deionized water several times until the upper layer of the solution is dark green (pH value is about 7). Then, ultrasonically treat the dispersion in an ice bath for 2 hours and collect the supernatant by centrifugation at 3500 rpm. Centrifuge the obtained upper layer at 7000 rpm for 5 minutes to obtain large-layer Ti3C2T x The nanosheets (upper layer of liquid) are freeze-dried into powder for later use.

[0056] Step 3: Preparation of mesoporous titanium carbide nanosheets: Take 100 mg of large Ti3C2T flakes obtained in step 2. x The nanosheets were dispersed in 100 mL of deionized water and mixed with the same volume of 0.2 mol / L copper sulfate solution, stirred for 30 min using a magnetic stirrer, and then washed repeatedly by centrifugation with deionized water until the pH value of the solution reached 6.

[0057] Step 4, preparation of mesoporous titanium carbide powder: add 20 mL of 10% hydrogen fluoride solution to the solution obtained in step 3, keep etching for 10 minutes and then ultrasonically disperse for 3 minutes, finally centrifuge and wash until the upper layer liquid is dark green (pH value between 5-6), take the upper layer liquid and freeze-dry it into powder for later use.

[0058] Step 5. Preparation of mesoporous titanium carbide conductive fiber: Disperse titanium carbide powder and mesoporous titanium carbide powder in water to prepare a fiber spinning solution. The mixed concentration of titanium carbide and mesoporous titanium carbide in the spinning solution is 40 mg / mL, of which the mass fraction of mesoporous titanium carbide accounts for 15%. The fiber spinning solution is injected into a spinning tank equipped with a coagulation bath through a spinneret of model 23G at a spinning flow rate of 50 ml / h. After soaking for 20 minutes, the fiber is washed with sulfuric acid, ethanol solution and deionized water in turn. After being fully dried, the mesoporous titanium carbide conductive fiber is obtained. The scanning electron microscope image of the cross-section of the obtained mesoporous titanium carbide fiber is as follows: Figure 5 As shown, the fiber has an irregular cross section and the entire cross section presents a wrinkled shape formed by stacking titanium carbide sheets.

[0059] Embodiment 2:

[0060] The differences between this embodiment and embodiment 1 are as follows: in step five, the amount of methyl methacrylate added is 12 wt.%, and the reaction temperature is 55°C; in step six, the mixed concentration of titanium carbide and mesoporous titanium carbide in the spinning solution is 42 mg / mL, of which the concentration of mesoporous titanium carbide is 5 wt.%, the concentration of PMMA microspheres is 9 mg / mL, and the sintering temperature is 600°C; the remaining operating steps and parameter settings are exactly the same as those in embodiment 1.

[0061] Embodiment 3:

[0062] The differences between this embodiment and embodiment 1 are as follows: in step five, the amount of methyl methacrylate added is 14 wt.%, and the reaction temperature is 55°C; in step six, the mixed concentration of titanium carbide and mesoporous titanium carbide in the spinning solution is 44 mg / mL, of which the concentration of mesoporous titanium carbide is 10 wt.%, the concentration of PMMA microspheres is 10 mg / mL, and the sintering temperature is 600°C; the remaining operating steps and parameter settings are exactly the same as those in embodiment 1.

[0063] Embodiment 4:

[0064] The differences between this embodiment and embodiment 1 are as follows: in step five, the amount of methyl methacrylate added is 15wt.%, and the reaction temperature is 60°C; in step six, the mixed concentration of titanium carbide and mesoporous titanium carbide in the spinning solution is 46mg / mL, of which the concentration of mesoporous titanium carbide is 15wt.%, the concentration of PMMA microspheres is 11mg / mL, and the sintering temperature is 650°C; the remaining operating steps and parameter settings are exactly the same as those in embodiment 1.

[0065] Embodiment 5:

[0066] The differences between this embodiment and embodiment 1 are as follows: in step five, the amount of methyl methacrylate added is 15wt.%, and the reaction temperature is 60°C; in step six, the mixed concentration of titanium carbide and mesoporous titanium carbide in the spinning solution is 48mg / mL, of which the concentration of mesoporous titanium carbide is 20wt.%, the concentration of PMMA microspheres is 12mg / mL, and the sintering temperature is 650°C; the remaining operating steps and parameter settings are exactly the same as those in embodiment 1.

[0067] It should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solutions of the present invention may be modified or replaced by equivalents without departing from the spirit and scope of the technical solutions of the present invention, which should all be included in the scope of the claims of the present invention.

Claims

1. A method for preparing multi-level porous titanium carbide conductive fiber, characterized in that: The following steps are involved: S1, preparing titanium carbide powder: adding lithium fluoride powder to hydrochloric acid, stirring continuously for sufficient reaction, adding aluminum titanium carbide, stirring and reacting in an oil bath at 35-40°C for 24 hours, centrifuging after the reaction, washing the reactant with deionized water until the upper layer of the solution is dark green and has a pH of 6-7, ultrasonically treating the upper layer in an ice bath, collecting the supernatant by centrifugation, further centrifuging the supernatant, and freeze-drying the supernatant into powder to obtain titanium carbide powder, wherein the mass ratio of lithium fluoride to aluminum titanium carbide is 1.6:1; S2, preparing mesoporous titanium carbide powder: dispersing titanium carbide powder in deionized water, adding an equal volume of 0.2 mol / L copper sulfate solution, stirring for 30 min, repeatedly centrifuging and washing with deionized water until the pH value of the solution is 6, adding hydrogen fluoride to the solution, etching for 10 min, ultrasonically dispersing, centrifugally washing until the upper layer liquid is dark green, taking the upper layer liquid and freeze-drying it into powder, to obtain mesoporous titanium carbide powder; S3, preparing PMMA microspheres: dissolving azoisobutyronitrile and polyvinyl pyrrolidone in methanol, adding methyl methacrylate after the mixed solution is purged with nitrogen, stirring for reaction, centrifuging, and washing to obtain a white product, which is PMMA microspheres, wherein the mass concentration of azoisobutyronitrile in the mixed solution is 0.1%, the mass concentration of polyvinyl pyrrolidone is 4%, and the reaction temperature is 50-60°C; S4, preparation of continuous multi-level porous titanium carbide conductive fiber: titanium carbide powder, mesoporous titanium carbide powder and PMMA microspheres are used as raw materials to prepare fiber spinning solution, the mixed concentration of titanium carbide and mesoporous titanium carbide in the spinning solution is 40-48 mg / mL, the mass fraction of mesoporous titanium carbide is 4-22%, and the concentration of PMMA microspheres is 8-12 mg / mL. After wet spinning, the obtained fiber is cleaned and sintered to obtain multi-level porous titanium carbide conductive fiber, wherein the spinning flow rate is 50 ml / h, the coagulation bath is a mixture of chitosan, acetic acid and deionized water, and the sintering temperature is 500-650 ° C.

2. A multi-level porous titanium carbide conductive fiber obtained by the preparation method according to claim 1, characterized in that: The multi-level porous titanium carbide conductive fiber has a continuous multi-level pore structure.

3. An application of the multi-level porous titanium carbide conductive fiber according to claim 2, characterized in that: Used as flexible electrode material.