Epoxy resin for high-leveling, low-temperature, fast-curing powder coating and preparation method thereof
By using castor oil and other raw materials, the problems of high total chlorine content and stickiness of epoxy resin are solved, and the combination of low-temperature rapid curing and high leveling performance is achieved. It is suitable for surface coating of precision instruments and provides new epoxy Industrialization of resin products and biomass castor oil with high value added value.
Patent Information
- Application Number
- CN202310059452.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-01-18
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2043-01-18
AI Technical Summary
The epoxy resin in existing powder coatings has a high total chlorine content, which cannot meet the requirements of low chlorine and low temperature rapid curing on the surface of precision instruments. It is also difficult to achieve high leveling performance, resulting in poor storage stability and sticky hands.
Castor oil, dimethyl adipic acid, 4,4'-biphenyl acid, bisphenol A diglycidyl ether, methylallyl alcohol, acetonitrile and hydrogen peroxide as the main raw materials, and expand through specific transesterification The chain, carboxy-terminated end capping and epoxidation reaction was used to prepare an epoxy resin with an epoxy equivalent of 560-610 g/mol, with a total chlorine content less than 200 ppm. Combined with a phosphotungstic acid catalyst, it achieves fast curing and high leveling performance at low temperature.
The obtained epoxy resin has no stickiness at room temperature, good storage stability, can cure quickly under low temperature conditions, is suitable for surface coating of precision instruments, and achieves high leveling performance, meeting application requirements in special fields.
Smart Images

Figure BDA0004061007570000081 
Figure BDA0004061007570000091 
Figure BDA0004061007570000092
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of chemical products, and particularly relates to an epoxy resin for high-leveling, low-temperature, fast-curing powder coating and a preparation method thereof. Background Art
[0002] Powder coatings are widely used in the general coating industry due to their advantages of environmental protection, energy saving, no VOC emissions, and convenient recycling and reuse, as well as their excellent protective and decorative properties. With the extension of powder coatings to special coating fields, such as coatings on the surface of precision instruments such as chromatographic instruments, this type of coating has lower requirements for the total chlorine content in the resin of powder coatings, generally required to be below 300ppm, so as not to corrode the surface of the instrument. At the same time, some precision instruments cannot withstand high temperatures for a long time due to poor high temperature resistance (such as needing to be below 130℃ / 10min), which requires new products to be able to achieve low-temperature rapid curing to avoid affecting the performance of precision instruments, and at the same time have excellent surface leveling properties to achieve beautiful effects. At present, the epoxy resin in the field of powder coatings is mainly E-12 epoxy resin, which is prepared by epichlorohydrin and bisphenol A under the catalysis of sodium hydroxide. The total chlorine content of the obtained epoxy resin product is relatively high, basically above 4000ppm, which is far from meeting the application requirements of the above special fields. At the same time, due to the high softening point and insufficient branching degree of E-12 epoxy resin, it is difficult to achieve low-temperature rapid curing and film formation. Although there are some low-temperature curing epoxy resin products, either there are problems with the molecular structure design, resulting in the final product being sticky and very easy to agglomerate, resulting in poor storage stability and difficulty in industrialization, or it is impossible to achieve a true combination of low-temperature rapid curing and high leveling performance. Summary of the invention
[0003] In view of the above problems, the epoxy resin for powder coating of the present invention is obtained by reaction using castor oil, dimethyl adipate, 4,4'-biphenyldicarboxylic acid, bisphenol A diglycidyl ether, methyl allyl alcohol, acetonitrile, and hydrogen peroxide as main raw materials. The epoxy equivalent of the obtained epoxy resin is 560-610g / mol, the total chlorine is basically below 200ppm, there is no sticky phenomenon at room temperature, the storage stability is good, and it can be used for surface coating of some precision instruments and equipment.
[0004] An epoxy resin for powder coating, the raw material composition comprises, by molar fraction:
[0005] 7-11 parts of castor oil;
[0006] 8-13 parts of dimethyl adipate;
[0007] 15-20 parts of 4,4'-biphenyldicarboxylic acid;
[0008] Bisphenol A diglycidyl ether 11-17 parts;
[0009] 7-10 parts of methyl allyl alcohol;
[0010] Acetonitrile 50-70 parts;
[0011] 45-55 parts of hydrogen peroxide;
[0012] The raw materials also include a catalyst.
[0013] Furthermore, the catalyst is phosphotungstic acid, and the amount used is 0.8-1.5% of the total mass of castor oil.
[0014] Furthermore, the hydrogen peroxide adopts a hydrogen peroxide aqueous solution with a mass concentration of 25-50%.
[0015] A method for preparing an epoxy resin for powder coating comprises the following steps:
[0016] A. Stir and mix the castor oil and catalyst in the formula amount, raise the temperature to 90-100° C., start the vacuum system, and drop the formula amount of dimethyl adipate to carry out ester exchange and chain extension reaction. After the dropwise addition is completed, continue the heat preservation reaction;
[0017] B. Take samples and test them by gas chromatography. When the content of free dimethyl adipate is less than 2%, a chain extension intermediate is obtained, and a formula amount of 4,4'-biphenyldicarboxylic acid is added to continue the chain extension and carboxyl end-capping reaction with the hydroxyl groups on the intermediate. The reaction temperature is controlled at 115-120°C;
[0018] C. Sampling and testing the hydroxyl value of the above polymer, when the hydroxyl value of the polymer is lower than 5 mgKOH / g, releasing the vacuum, adding the formulated amount of bisphenol A diglycidyl ether to carry out chain extension reaction, and the temperature is still maintained at 115-120° C.;
[0019] D. Take samples to test the epoxy equivalent of the polymer. When the epoxy equivalent is greater than 5000 g / mol, lower the reaction temperature to 102-105° C. and add a formula amount of methyl allyl alcohol to carry out esterification and end-capping reaction;
[0020] E. Detect the acid value of the polymer in the system. When the acid value of the polymer drops below 3 mgKOH / g, start the vacuum system;
[0021] F. When the methyl allyl alcohol content in the system is less than 0.5%, the temperature is lowered to 57-63°C, acetonitrile is added to the formula amount to fully dissolve the polymer into one phase, and then a hydrogen peroxide solution is added dropwise. After the addition is completed, the epoxidation reaction is continued at the temperature;
[0022] G. Take samples to detect the iodine value of the polymer. When the iodine value is less than 1 (g / 100g), heat to 110-115°C and start the vacuum system to fully remove the solvent and unreacted hydrogen peroxide solution. When no obvious distillate is evaporated, stop the reaction, discharge the material while hot, and obtain the epoxy resin through post-treatment.
[0023] Furthermore, in step A, the vacuum degree is controlled at -0.095 to -0.097 MPa; and the dropping time is controlled at 1 to 1.5 h.
[0024] Furthermore, in step B, the vacuum degree of the chain extension and carboxyl termination reaction is still maintained at -0.095 to -0.097 MPa to fully remove the esterified water molecules to promote the reaction; in step E, the vacuum degree is controlled at -0.096 to -0.098 MPa to remove excess unreacted methyl allyl alcohol.
[0025] Furthermore, in step F, the dropping time is controlled within 2-3 hours.
[0026] Furthermore, in step G, the vacuum degree of the vacuum system is controlled at -0.097 to -0.099 MPa; no obvious distillate is evaporated means that less than 1 drop of distillate is evaporated within 30 seconds; and post-processing includes cooling the epoxy resin with a steel belt with condensed water, and then crushing and granulating.
[0027] The present invention also relates to the use of the epoxy resin for powder coating as described above or the epoxy resin for powder coating obtained by the preparation method in low-temperature fast-curing powder coating; preferably, the powder coating is sprayed with an electrostatic spray gun and then baked and cured to obtain a coating film.
[0028] For example, a method for preparing an epoxy resin for powder coating comprises the following steps:
[0029] A. Add the formulated amount of castor oil and catalyst into the reactor, start stirring and mix evenly, then heat to 90-100°C, start the vacuum system, control the vacuum degree at -0.095 to -0.097Mpa, then dropwise add the formulated amount of dimethyl adipate to carry out ester exchange chain extension reaction, the dropping time is controlled at 1-1.5h, and after the dropping is completed, continue the heat preservation reaction;
[0030] B. Take samples and test them by gas chromatography. When the content of free dimethyl adipate is less than 2%, it means that dimethyl adipate has been subjected to ester exchange reaction with the hydroxyl groups on the castor oil molecules to obtain a chain extension intermediate. At this time, add the formulated amount of 4,4'-biphenyldicarboxylic acid to continue the chain extension and carboxyl end-capping reaction with the hydroxyl groups on the intermediate. The reaction temperature is controlled at 115-120°C, and the vacuum degree is still maintained at -0.095 to -0.097Mpa to fully remove the esterified water molecules to promote the reaction;
[0031] C. Sampling and testing the hydroxyl value of the above polymer, when the hydroxyl value of the polymer is lower than 5 mgKOH / g, releasing the vacuum, adding the formulated amount of bisphenol A diglycidyl ether to carry out chain extension reaction, and the temperature is still maintained at 115-120° C.;
[0032] D. Take samples to test the epoxy equivalent of the polymer. When the epoxy equivalent is greater than 5000 g / mol, it indicates that the reaction of bisphenol A diglycidyl ether has been completed. At this time, the reaction temperature is lowered to 102-105° C., and methyl allyl alcohol is added in the formula amount to carry out esterification and end-capping reaction;
[0033] E. Detect the acid value of the polymer in the system. When the acid value of the polymer drops below 3 mgKOH / g, it indicates that the carboxyl groups in the polymer chain segments have been basically esterified. Start the vacuum system and control the vacuum degree at -0.096 to -0.098 MPa to remove excess unreacted methyl allyl alcohol.
[0034] F. When the methyl allyl alcohol content in the system is less than 0.5%, cool to 57-63°C, add the formulated amount of acetonitrile to fully dissolve the polymer into one phase, then drip hydrogen peroxide solution, the dripping time is controlled within 2-3h, and after the dripping is completed, continue to heat and keep the epoxidation reaction;
[0035] G. Take samples to detect the iodine value of the polymer. When the iodine value is less than 1 (g / 100g), it means that the unsaturated double bonds in the polymer have been completely epoxidized. At this time, the temperature is raised to 110-115°C, and the vacuum system is started to fully remove the solvent and unreacted hydrogen peroxide solution. The vacuum degree is controlled at -0.097 to -0.099Mpa. After no obvious distillate is evaporated (less than 1 drop of distillate within 30s), the reaction is stopped, the material is discharged while hot, and the epoxy resin is cooled with a steel belt with condensed water, and then crushed and granulated to obtain the epoxy resin.
[0036] The obtained product has the appearance of light yellow transparent particles, an epoxy equivalent of 560-610 g / mol, a softening point of 75-80°C, and a total chlorine content of <200 ppm.
[0037] The epoxy resin system powder coating formula used in the present invention may include 2-phenyl-4,5-dihydroimidazole, titanium dioxide, barium sulfate and other commonly used auxiliary fillers in the field in addition to the epoxy resin prepared above. The coating preparation method is: mix the materials, extrude, tablet and crush them with a twin-screw extruder, and then crush and sieve the tablets to make powder coating. The powder coating is sprayed on the tinplate substrate after surface treatment with an electrostatic spray gun, with a film thickness of 70-80μm, and then baked and cured to obtain a coating film.
[0038] Beneficial effects of the present invention:
[0039] The epoxy resin of the present invention is obtained by using castor oil, dimethyl adipate, 4,4'-biphenyl dicarboxylic acid, bisphenol A diglycidyl ether, methyl allyl alcohol, acetonitrile, hydrogen peroxide and the like as main raw materials for reaction. The epoxy resin obtained has an epoxy equivalent of 560-610 g / mol, a total chlorine content of substantially below 200 ppm, no stickiness at room temperature, good storage stability, and can be used for surface coating of some precision instruments and equipment. At the same time, the epoxy resin uses a special castor oil chain extension product as the main structure, has a good degree of branching and an extremely low softening point of the product, has excellent low-temperature fluidity (under 125°C conditions), has highly active epoxy groups, and can achieve low-temperature rapid curing with 2-phenyl-4,5-dihydroimidazole, etc., and has excellent leveling performance, and other properties of the coating film can meet conventional application requirements. The method is prepared using castor oil as the main raw material, which not only develops a new epoxy resin product for the powder coating industry, but also provides a new way for the high value-added industrialization of biomass castor oil series products. DETAILED DESCRIPTION
[0040] To facilitate understanding of the present invention, various exemplary embodiments of the present invention are now described in detail. This detailed description should not be regarded as a specific limitation of the present invention, but should be understood as a more detailed description of certain aspects, features and embodiments of the present invention.
[0041] The raw materials are all commercially available ordinary industrial grade raw materials.
[0042] Example 1
[0043] An epoxy resin for powder coating, the raw material composition comprises, by molar fraction:
[0044] 7 parts of castor oil;
[0045] 8 parts of dimethyl adipate;
[0046] 16 parts of 4,4'-biphenyldicarboxylic acid;
[0047] 12 parts of bisphenol A diglycidyl ether;
[0048] 7 parts of methyl allyl alcohol;
[0049] Acetonitrile 52 parts;
[0050] 46 parts of hydrogen peroxide;
[0051] The catalyst is phosphotungstic acid, and the dosage is 1% of the total mass of castor oil.
[0052] The hydrogen peroxide adopts a hydrogen peroxide aqueous solution with a mass concentration of 48%.
[0053] The preparation method of epoxy resin for powder coating comprises the following steps:
[0054] A. Add the formulated amount of castor oil and catalyst into the reactor, start stirring and mix evenly, then heat to 100°C, start the vacuum system, control the vacuum degree at -0.097Mpa, then drop the formulated amount of dimethyl adipate to carry out ester exchange chain extension reaction, the dropping time is controlled at 1.5h, and after the dropping is completed, continue the insulation reaction;
[0055] B. Take samples and test them by gas chromatography. When the content of free dimethyl adipate is less than 2%, it means that dimethyl adipate has undergone ester exchange reaction with the hydroxyl groups on the castor oil molecules to obtain a chain extension intermediate. At this time, add the formulated amount of 4,4'-biphenyldicarboxylic acid to continue the chain extension and carboxyl end-capping reaction with the hydroxyl groups on the intermediate. The reaction temperature is controlled at 120°C and the vacuum degree is still maintained at -0.097Mpa to fully remove the esterified water molecules to promote the reaction;
[0056] C. Sampling and testing the hydroxyl value of the above polymer, when the hydroxyl value of the polymer is lower than 5 mgKOH / g, releasing the vacuum, adding the formulated amount of bisphenol A diglycidyl ether to carry out chain extension reaction, and the temperature is still maintained at 120° C.;
[0057] D. Take samples to test the epoxy equivalent of the polymer. When the epoxy equivalent is greater than 5000 g / mol, it indicates that the reaction of bisphenol A diglycidyl ether has been completed. At this time, the reaction temperature is lowered to 105° C., and methyl allyl alcohol is added in the formula amount to carry out esterification and end-capping reaction;
[0058] E. Detect the acid value of the polymer in the system. When the acid value of the polymer drops below 3 mgKOH / g, it indicates that the carboxyl groups in the polymer chain segments have been basically esterified. Start the vacuum system and control the vacuum degree at -0.098 MPa to remove excess unreacted methyl allyl alcohol.
[0059] F. When the methyl allyl alcohol content in the system is less than 0.5%, the temperature is lowered to 63°C, acetonitrile is added to the formula amount to fully dissolve the polymer into one phase, and then a hydrogen peroxide solution is added dropwise. The addition time is controlled within 3 hours. After the addition is completed, the epoxidation reaction is continued at the temperature;
[0060] G. Take samples to detect the iodine value of the polymer. When the iodine value is less than 1 (g / 100g), it means that the unsaturated double bonds in the polymer have been completely epoxidized. At this time, the temperature is raised to 115°C, and the vacuum system is started to fully remove the solvent and unreacted hydrogen peroxide solution. The vacuum degree is controlled at -0.099Mpa. After no obvious distillate is evaporated (less than 1 drop of distillate within 30s), the reaction is stopped, the material is discharged while hot, and the epoxy resin is cooled with a steel belt with condensed water, and then crushed and granulated to obtain the epoxy resin.
[0061] The prepared epoxy resin has an epoxy equivalent of 589 g / mol, a softening point of 78°C, and a total chlorine content of 188 ppm.
[0062] Example 2
[0063] An epoxy resin for powder coating, the raw material composition comprises, by molar fraction:
[0064]
[0065] The catalyst is phosphotungstic acid, and the amount used is 1.5% of the total mass of castor oil.
[0066] The hydrogen peroxide adopts a hydrogen peroxide aqueous solution with a mass concentration of 30%.
[0067] The preparation method is the same as that of Example 1.
[0068] The obtained product has the appearance of light yellow transparent particles, an epoxy equivalent of 575 g / mol, a softening point of 77° C., and a total chlorine content of 182 ppm.
[0069] Example 3
[0070] An epoxy resin for powder coating, the raw material composition comprises, by molar fraction:
[0071]
[0072]
[0073] The catalyst is phosphotungstic acid, and the amount used is 1.5% of the total mass of castor oil.
[0074] The hydrogen peroxide adopts a hydrogen peroxide aqueous solution with a mass concentration of 40%.
[0075] The preparation method is the same as that of Example 1.
[0076] The obtained product has the appearance of light yellow transparent particles, an epoxy equivalent of 597 g / mol, a softening point of 79° C., and a total chlorine content of 173 ppm.
[0077] Example 4
[0078] An epoxy resin for powder coating, the raw material composition comprises, by molar fraction:
[0079]
[0080] The catalyst is phosphotungstic acid, and the amount used is 0.8% of the total mass of castor oil.
[0081] The hydrogen peroxide adopts a hydrogen peroxide aqueous solution with a mass concentration of 40%.
[0082] The preparation method is the same as that of Example 1.
[0083] The obtained product has the appearance of light yellow transparent particles, an epoxy equivalent of 566 g / mol, a softening point of 75° C., and a total chlorine content of 168 ppm.
[0084] Comparative Example 1: Commercially available ordinary E-12 epoxy resin, epoxy equivalent 838 g / mol, softening point 89° C., total chlorine 4850 ppm; purchased from Anhui Hengyuan New Materials Co., Ltd.
[0085] Comparative Example 2: The rest is the same as Comparative Example 1, and the curing condition is 180°C / 10min.
[0086] Application example: The epoxy resin system powder coating formula used is usually as follows in parts by weight:
[0087]
[0088] The powder coating formula used in Comparative Example 1 is the same as above. Due to the difference in epoxy equivalent, only the amount of 2-phenyl-4,5-dihydroimidazole as a curing agent is adjusted to 42 parts.
[0089] Preparation of coating: Mix all materials according to the requirements of the above powder coating formula, extrude, tablet and crush with a twin-screw extruder, and then crush and sieve the tablets to make powder coating. The powder coating is sprayed on the surface treated tinplate substrate with an electrostatic spray gun, with a film thickness of 70-80μm, and then cured by baking at 125℃ / 8min to obtain the coating film.
[0090] The determination method of total chlorine is based on GB / T 12007.3-1989 "Determination method of total chlorine content of epoxy resin", the coating index detection is based on GB / T 21776-2008 "Guide to the detection standard of powder coatings and their coatings", the leveling is carried out according to the PCI leveling grade, 1-10, the larger the number, the better the leveling, and the adhesion grade is based on GB / T 9286-1998 "Scratch test for paint and varnish films".
[0091] Table 1 Comparison of storage stability of Examples 1-4 and Comparative Example 1
[0092]
[0093] Note: Because the epoxy resin used in Comparative Example 1 and Comparative Example 2 is the same resin, only Comparative Example 1 is used for comparison of storage stability.
[0094] As can be seen from Table 1, the storage stability of the product of the present invention at different temperatures is not much different from that of the common bisphenol A type E-12 epoxy resin product currently on the market, and can basically meet the conventional storage and application requirements of downstream customers.
[0095] Table 2 Coating properties of coatings obtained from Examples 1-4 and Comparative Examples 1-2
[0096]
[0097]
[0098] As can be seen from Table 2, the epoxy resin of the present invention, under the structure with castor oil as the main chain segment, realizes the characteristics of relatively low softening point and high active epoxy group through the chain extension reaction of relevant flexible and rigid structural segments, the total chlorine of the product is less than 200ppm, and the storage stability of the product can meet the requirements of conventional products in the market. It also performs better in coating application effect. After rapid curing at low temperature of 125℃ / 8min, the appearance, impact and gloss of the coating film are good, while taking into account the excellent leveling and adhesion performance, the leveling grade is above level 6, and the adhesion is all at level 0; it can meet the application requirements of some special fields such as chromatographic instruments; this method is prepared with castor oil as the main raw material, which not only develops a new epoxy resin product for the powder coating industry, but also provides a new way for the high value-added industrialization of biomass castor oil series products.
[0099] Comparative Example 1-2 uses common E-12 epoxy resin, which not only has too high total chlorine to meet the requirements, but also has too high softening point and low epoxy activity due to its linear segment structure and low-density epoxy group characteristics, resulting in it being unable to achieve effective curing at 125°C / 8min. Comparative Example 2 raises its curing conditions to conventional curing conditions (180°C / 10min), which can achieve full curing. The gloss, impact resistance, adhesion, etc. after curing are not much different from those of the product of the present invention, but the leveling performance, etc. are slightly worse than those of the product of the present invention.
[0100] Obviously, the above embodiments are merely examples for the purpose of clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived from these are still within the scope of protection of the invention.
Claims
1. An epoxy resin for powder coating, characterized in that: The raw materials including castor oil, dimethyl adipate, 4,4'-biphenyldicarboxylic acid, bisphenol A diglycidyl ether, methyl allyl alcohol, acetonitrile and hydrogen peroxide are used to react to obtain the product; Wherein, the raw material composition comprises by mole fraction: The raw materials also include a catalyst, phosphotungstic acid, the amount of which is 0.8-1.5% of the total mass of castor oil; The preparation method of the epoxy resin for powder coating comprises the following steps: A. Stir and mix the castor oil and catalyst in the formula amount, raise the temperature to 90-100° C., start the vacuum system, and drop the formula amount of dimethyl adipate to carry out ester exchange and chain extension reaction. After the dropwise addition is completed, continue the heat preservation reaction; B. Take samples and test them by gas chromatography. When the content of free dimethyl adipate is less than 2%, a chain extension intermediate is obtained, and a formula amount of 4,4'-biphenyldicarboxylic acid is added to continue the chain extension and carboxyl end-capping reaction with the hydroxyl groups on the intermediate. The reaction temperature is controlled at 115-120°C; C. Sampling and testing the hydroxyl value of the product in step B. When the hydroxyl value of the product is lower than 5 mgKOH / g, releasing the vacuum, adding the formulated amount of bisphenol A diglycidyl ether to carry out chain extension reaction, and maintaining the temperature at 115-120° C.; D. Sampling and testing the epoxy equivalent of the product in step C. When the epoxy equivalent is greater than 5000 g / mol, lowering the reaction temperature to 102-105° C., adding a formulated amount of methyl allyl alcohol to carry out an esterification and capping reaction; E. Detect the acid value of the product of step D. When the acid value of the product drops below 3 mgKOH / g, start the vacuum system; F. When the methyl allyl alcohol content in the system is less than 0.5%, the temperature is lowered to 57-63° C., acetonitrile is added in a formula amount to fully dissolve the product into one phase, and then a hydrogen peroxide solution is added dropwise. After the addition is completed, the epoxidation reaction is continued at the temperature; G. Take samples to detect the iodine value of the product in step F. When the iodine value is less than 1 (g / 100g), heat to 110-115° C., start the vacuum system to fully remove the solvent and unreacted aqueous hydrogen peroxide solution, and stop the reaction when no obvious distillate is evaporated. Discharge the material while hot and obtain the epoxy resin through post-treatment.
2. The epoxy resin for powder coating according to claim 1, further characterized in that the hydrogen peroxide is a hydrogen peroxide aqueous solution with a mass concentration of 25-50%.
3. An epoxy resin for powder coating as claimed in claim 1, further characterized in that, in step A of the preparation method, the vacuum degree is controlled at -0.095 to -0.097 MPa; and the dropping time is controlled at 1 to 1.5 h.
4. An epoxy resin for powder coatings as claimed in claim 1, further characterized in that, in step B of the preparation method, the vacuum degree of the chain extension and carboxyl termination reaction is maintained at -0.095 to -0.097 MPa to fully remove the esterified water molecules to promote the reaction; in step E, the vacuum degree is controlled at -0.096 to -0.098 MPa to remove excess unreacted methyl allyl alcohol.
5. The epoxy resin for powder coating according to claim 1, further characterized in that in step F of the preparation method, the dropping time is controlled to be 2-3 hours.
6. An epoxy resin for powder coating as claimed in claim 1, further characterized in that, in step G of the preparation method, the vacuum degree of the vacuum system is controlled at -0.097 to -0.099 MPa; no obvious distillate is evaporated means that less than 1 drop of distillate is produced within 30 seconds; post-treatment includes cooling the epoxy resin with a steel belt with condensed water, and then crushing and granulating.
7. Use of the epoxy resin for powder coating according to any one of claims 1 to 6 in low temperature fast curing powder coating, characterized in that: The powder coating is sprayed with an electrostatic spray gun and then baked and cured to obtain a coating film.
Citation Information
Patent Citations
Powder coatings compositions
CN103068941A
Phosphate modified cationic microgel, preparation method and application