Preparation method of bistable multi-stimulus responsive Janus color-changing fiber
By combining sodium alginate with thermochromic microcapsules and functional nanomaterials in multi-stimulus responsive color discoloration materials, the color occlusion of dark nanomaterials in discolored fibers was solved. The problem, achieving triple stimulation response of light, thermal and electrical, demonstrates potential in smart textiles and wearable devices.
Patent Information
- Application Number
- CN202310139227.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-02-20
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2043-02-20
AI Technical Summary
Multi-stimulus responsive color discoloration materials cannot effectively utilize dark nanoparticles, and the demand for heat source supply is large, which limits its development.
The bistable multi-stimulation responsive Janus color-discolored fiber is prepared by using a dual-channel microfluidic control device. By combining sodium alginate with thermochromic microcapsules and functional nanomaterials, axially symmetric cylindrical structure is formed to achieve light, heat, Electric triple stimulus response.
The introduction of photothermal and electrothermal functions of dark nanomaterials in asymmetric fiber structures has been achieved, solving the problem of color depth affecting color of discolored fibers, and demonstrating its potential in smart textiles and wearable devices.
Smart Images

Figure CN116103786B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a preparation method of a bistable multi-stimulus responsive Janus color-changing fiber, and belongs to the technical field of fine chemicals and material science. Background Art
[0002] The bistable phenomenon refers to two different, interchangeable stable states, which is widely present in nature and life, such as brain activity, Venus flytraps, circuit switches, etc. Its unique characteristics of adjustability, memory and energy saving provide a series of new additional functions that cannot be achieved by traditional materials.
[0003] At present, the application fields of bistable energy-saving materials have attracted widespread attention in the fields of textiles, soft robotics, bionics and display. The structural design of shape memory materials, including one-dimensional beam structure, two-dimensional curved bistable structure and three-dimensional dome structure, is the main way to achieve the bistable state of soft brakes. In addition, color-changing materials with bistable properties can enable samples to maintain color information without any external energy supply. For electrochromic materials, the bistable electrochromic effect is achieved by stabilizing the oxidation state of the color-changing material. Because its color-changing mechanism is clear and it is simple and easy to achieve the bistable goal, the research on bistable color change is also mainly concentrated in the field of electrochromic.
[0004] For thermochromic materials, they mainly use the supercooling characteristics of phase change materials and spatial confinement to achieve bistability. In the process of wearing, thermochromic materials are the first choice for bistable smart color-changing textiles because they are simple to process and very easy to finish on fabrics. However, in practical applications, the single thermal stimulus response makes the supply of heat source increasingly an issue that cannot be ignored. Therefore, multi-stimulus responsive color-changing textiles are born.
[0005] Usually, some photothermal and electrothermal conversion materials are used as thermal energy storage and conversion bridges to enrich the supply and transmission of heat sources. 2 , graphene, carbon black, etc.) and nanoparticles with photon capture ability give materials photothermal conversion ability and electrothermal conversion ability. However, they are rarely used as a heat source supply device for thermochromic materials because their inherent black color has a strong color masking ability for color-changing materials, thus limiting the development of multi-stimulus responsive color-changing materials. Summary of the invention
[0006] [Technical issues]
[0007] Multi-stimulus responsive color-changing materials cannot use dark-colored nanoparticles, and they require a large supply of heat sources.
[0008] [Technical solution]
[0009] In order to solve the above problems, the present invention constructs a simple and reusable dual-channel microfluidic device, and prepares a bistable multi-stimulus responsive Janus color-changing fiber by dynamic sol-gel spinning. The bistable multi-stimulus responsive Janus color-changing fiber described in the present invention is an axisymmetric cylindrical structure, one half of which is composed of sodium alginate and bistable thermochromic dye microcapsules, and has bright colors, fast response rate and good bistability, and the other half is composed of sodium alginate and functional nanomaterials, and has good Joule heating effect and excellent light-heat conversion ability.
[0010] The first object of the present invention is to provide a method for preparing a bistable multi-stimulus responsive Janus color-changing fiber, comprising the following steps:
[0011] (1) dissolving sodium alginate in water to obtain a spinning solution;
[0012] (2) taking a portion of the spinning solution and mixing it evenly with the thermochromic microcapsules to obtain a bistable thermochromic spinning solution, which is recorded as Janus A spinning solution; taking another portion of the spinning solution and mixing it evenly with the functional nanomaterials to obtain a spinning solution with photothermal and electrothermal conversion effects, which is recorded as Janus B spinning solution;
[0013] (3) The Janus A spinning solution and the Janus B spinning solution are allowed to stand for defoaming and are respectively placed in two syringes. The two syringes are then injected into a coagulation bath through the same needle hole to prepare the bistable multi-stimulus responsive Janus color-changing fiber.
[0014] In one embodiment of the present invention, the dosage ratio of sodium alginate and water in step (1) is 1 to 10:100, g / mL.
[0015] In one embodiment of the present invention, in step (2), the mass ratio of the spinning solution in the Janus A spinning solution to the spinning solution in the Janus B spinning solution is 1:1.
[0016] In one embodiment of the present invention, the preparation method of the thermochromic microcapsules described in step (2) is:
[0017] (1) mixing urea, formaldehyde, melamine and water uniformly, adjusting the pH value to 9-10, and polymerizing at 60-70° C. for 30-60 min to obtain a melamine / urea / formaldehyde prepolymer (MUF);
[0018] (2) stirring a phase change material, a thermoacid, and a fluorane dye at 65-85° C. for 30-45 minutes to prepare a bistable thermochromic compound (BTC), and then adding the bistable thermochromic compound (BTC) to an emulsifier aqueous solution to emulsify and form a bistable thermochromic compound (BTC) emulsion;
[0019] (3) adding the melamine / urea / formaldehyde prepolymer prepared in step (1) to the bistable thermochromic compound emulsion prepared in step (2), adjusting the pH to 4-5, and reacting at 60-75° C. for 2-5 hours; after the reaction is completed, cooling, washing, and drying to obtain thermochromic microcapsules;
[0020] The mass ratio of urea, formaldehyde, melamine and water is 6:12:1:1; the substances used to adjust the pH are triethanolamine and 1 mol / L hydrochloric acid;
[0021] The phase change material is one or more of glyceryl stearate, glyceryl distearate, methyl benzyl stearate, pentadecyl acetate, heptyl decanoate, nonyl decanoate, undecyl decanoate, tridecyl decanoate, pentadecyl decanoate, stearyl decanoate, 4-benzyloxyphenylethyl octanoate, 4-benzyloxyphenylethyl decanoate, 4-benzyloxyphenylethyl undecanoate, 1,1-diphenylmethyl decanoate, and diphenyl carbonate;
[0022] The thermal acid includes one or more of bisphenol A, gallic acid, methyl gallate, ethyl gallate, and propyl gallate;
[0023] The fluoran dye includes one or more of a green fluoran dye, a red fluoran dye, a yellow fluoran dye, a crystal violet lactone (blue), and an orange fluoran dye;
[0024] The mass ratio of the phase change material, the thermal acid, and the fluorane dye is selected from 80 / 2 / 1, 60 / 2 / 1, 50 / 2 / 1, 40 / 2 / 1, and 30 / 2 / 1;
[0025] The emulsifier is one or more of polyvinyl alcohol, sodium dodecylbenzene sulfonate, sodium dodecyl sulfate, sodium dodecyl sulfonate, potassium oleate, sodium alkylnaphthalene sulfonate, polyoxyethylene fatty alcohol ether (Tween series, BRIJ-721 / 721S), alkyl glycoside compound (M68, ML), gelatin, OP-10, SG-10, SE-10, OE-15, 1-allyloxy-3-(4-nonylphenol)-2-propanol polyoxyethylene (10) ether ammonium sulfate DNS-86;
[0026] The mass ratio of emulsifier to water in the emulsifier aqueous solution is 1 / 99;
[0027] The dosage ratio of the bistable thermochromic compound (BTC) and the emulsifier aqueous solution is 2:100, g mL;
[0028] The emulsification is performed at 65° C. for 15 min, 20 min, 25 min, and 30 min (to control the size of the microcapsules);
[0029] The volume ratio of the melamine / urea / formaldehyde prepolymer (MUF) to the bistable thermochromic compound (BTC) emulsion is 1:2;
[0030] The washing was performed by ethanol washing 3 times and water washing 3 times; and the drying was performed at room temperature.
[0031] In one embodiment of the present invention, the amount ratio of the spinning mother solution and the thermochromic microcapsules in the Janus A spinning solution of step (2) is 50:0.5-2, mL / g.
[0032] In one embodiment of the present invention, the mass ratio of the spinning solution mother solution to the functional nanomaterial in the Janus B described in step (2) is 200:3-9.
[0033] In one embodiment of the present invention, the functional nanomaterial described in step (2) is Ti 3 C 2 T x , one or more of modified MXene, graphene, modified graphene, graphene oxide, molybdenum disulfide, modified molybdenum disulfide, carbon black, carbon nanotubes, carbon nanorods, silver nanowires, copper nanowires, and gold nanowires.
[0034] In one embodiment of the present invention, the static degassing in step (3) is performed for 12-24 hours.
[0035] In one embodiment of the present invention, the injection speed ratio of the injectors of the Janus A spinning solution and the Janus B spinning solution in step (3) is 1-3:1.
[0036] In one embodiment of the present invention, the coagulation bath in step (3) is a 5 wt % calcium chloride aqueous solution.
[0037] The second objective of the present invention is the bistable multi-stimulus responsive Janus color-changing fiber prepared by the method described in the present invention.
[0038] The third object of the present invention is to provide a color-changing yarn, which is obtained by spinning the bistable multi-stimulus responsive Janus color-changing fiber of the present invention.
[0039] The fourth object of the present invention is to provide a color-changing fabric, which is woven using the bistable multi-stimulus responsive Janus color-changing fiber or color-changing yarn described in the present invention.
[0040] The fifth objective of the present invention is to use the bistable multi-stimulus responsive Janus color-changing fibers, color-changing yarns, and color-changing fabrics described in the present invention in the preparation of smart textiles.
[0041] [Beneficial Effects]
[0042] The present invention uses an asymmetric fiber structure to introduce the photothermal and electrothermal functions of dark nanomaterials into color-changing fibers, making them respond to light, heat, and electricity and have bistable properties, solving the problem of color-changing fibers being affected by the dark color of functional nanomaterials. These properties and Janus structural design strongly demonstrate its unlimited potential in weaving smart textiles, flexible programmable devices, and wearable devices. BRIEF DESCRIPTION OF THE DRAWINGS
[0043] Figure 1 The present invention is a process flow chart for preparing bistable multi-stimulus responsive Janus color-changing fibers. DETAILED DESCRIPTION
[0044] The preferred embodiments of the present invention are described below. It should be understood that the embodiments are for better explaining the present invention and are not used to limit the present invention.
[0045] Test method:
[0046] 1. Color change performance test
[0047] The Janus fiber was fixed on a glass slide and placed on a hot stage. The heating (cooling) rate of the hot stage was set to 1°C / min. The color change temperature, color change temperature range and color change process of the thermochromic dye complex during the temperature rise and fall process were observed under a microscope.
[0048] The Janus fiber is placed under a xenon lamp, which is controlled to simulate the intensity of sunlight. A thermal infrared imager is used to detect changes in fiber surface temperature, and the color changes are recorded by photographing. Both ends of the Janus fiber are connected to a power source, and the electrothermal conversion drives the fiber to change color. A thermal infrared imager is used to detect changes in fiber surface temperature, and the color changes are recorded by photographing.
[0049] 2. Strong performance test
[0050] Microcomputer controlled electronic universal testing machine tests fiber strength.
[0051] Example 1
[0052] A method for preparing green bistable thermochromic microcapsules comprises the following steps:
[0053] Urea, formaldehyde, melamine and water were added into a flask in a mass ratio of 6:12:1:1 and mixed evenly. The pH value was adjusted to 9-10 with triethanolamine. The flask was placed in an oil bath at 70° C. for polymerization for 60 min to obtain a melamine / urea / formaldehyde prepolymer (MUF).
[0054] Capric acid ester, bisphenol A, and green fluoran dye (commercially available, purity 99%) were stirred at 65°C for 30 minutes in a mass ratio of 60:2:1 to prepare a bistable thermochromic compound (BTC) and use it as a core material; then 2 g of the bistable thermochromic compound (BTC) was added to 100 mL of polyvinyl alcohol aqueous solution (the mass ratio of emulsifier to water was 1:99), and emulsified at 65°C for 20 minutes to form a bistable thermochromic compound (BTC) emulsion;
[0055] 1 g of melamine / urea / formaldehyde prepolymer (MUF) was added to 100 mL of bistable thermochromic compound (BTC) emulsion, and the pH of the solution was adjusted to 4-5 with 1 mol / L hydrochloric acid. The solution was reacted at 75°C for 2 h. After the reaction, the solution was cooled, washed with ethanol 3 times, washed with water 3 times, and dried at room temperature to obtain green bistable thermochromic microcapsules.
[0056] Example 2
[0057] A method for preparing green bistable thermochromic microcapsules comprises the following steps:
[0058] Urea, formaldehyde, melamine and water were added into a flask in a mass ratio of 6:12:1:1 and mixed evenly. The pH value was adjusted to 9-10 with triethanolamine. The flask was placed in an oil bath at 70° C. for polymerization for 60 min to obtain a melamine / urea / formaldehyde prepolymer (MUF).
[0059] Diphenyl carbonate, bisphenol A, and green fluorane dye (commercially available, purity 99%) were stirred at 85°C for 30 minutes in a mass ratio of 60:2:1 to prepare a bistable thermochromic compound (BTC) as a core material; then 2 g of the bistable thermochromic compound (BTC) was added to 100 mL of polyvinyl alcohol aqueous solution (the mass ratio of emulsifier to water was 1:99), and emulsified at 65°C for 20 minutes to form a bistable thermochromic compound (BTC) emulsion;
[0060] 1 g of melamine / urea / formaldehyde prepolymer (MUF) was added to 100 mL of bistable thermochromic compound (BTC) emulsion, the pH was adjusted to 4-5 with 1 mol / L hydrochloric acid, and the reaction was carried out at 75°C for 2 h. After the reaction, the mixture was cooled, washed with ethanol 3 times, washed with water 3 times, and dried at room temperature to obtain green bistable thermochromic microcapsules.
[0061] Example 3
[0062] A method for preparing red bistable thermochromic microcapsules comprises the following steps:
[0063] Urea, formaldehyde, melamine and water were added into a flask in a mass ratio of 6:12:1:1 and mixed evenly. The pH value was adjusted to 9-10 with triethanolamine. The flask was placed in an oil bath at 70° C. for polymerization for 60 min to obtain a melamine / urea / formaldehyde prepolymer (MUF).
[0064] Diphenyl carbonate, bisphenol A, and red fluorane dye (commercially available, purity 99%) were stirred at 85°C for 30 minutes in a mass ratio of 60:2:1 to prepare a bistable thermochromic compound (BTC) as a core material; then 2 g of the bistable thermochromic compound (BTC) was added to 100 mL of polyvinyl alcohol aqueous solution (the mass ratio of emulsifier to water was 1:99), and emulsified at 65°C for 20 minutes to form a bistable thermochromic compound (BTC) emulsion;
[0065] 1 g of melamine / urea / formaldehyde prepolymer (MUF) was added to 100 mL of bistable thermochromic compound (BTC) emulsion, the pH was adjusted to 4-5 with 1 mol / L hydrochloric acid, and the reaction was carried out at 75°C for 2 h. After the reaction, the mixture was cooled, washed with ethanol 3 times, washed with water 3 times, and dried at room temperature to obtain red bistable thermochromic microcapsules.
[0066] Example 4
[0067] A method for preparing a bistable multi-stimulus responsive Janus color-changing fiber comprises the following steps:
[0068] (1) dissolving 5 g of sodium alginate in 100 mL of water to obtain a spinning mother solution of sodium alginate;
[0069] (2) 50 mL of spinning solution and 0.5 g of the green bistable thermochromic microcapsules of Example 1 were stirred at room temperature for 1 h to uniformly mix to obtain a bistable thermochromic spinning solution, which was recorded as Janus A spinning solution;
[0070] 50 mL of spinning solution and 2.5 mL of Mxene (mass concentration of 80 wt%) were mixed by ultrasonic stirring for 2 h to obtain a spinning solution with photothermal and electrothermal conversion effects, which was recorded as Janus B spinning solution;
[0071] (3) The Janus A spinning solution and the Janus B spinning solution were allowed to stand for 12 h to defoam and were placed in two syringes respectively. Then, the two syringes injected 5 wt% CaCl at a speed of 1 mL / min through the same needle hole. 2 In aqueous solution, a bistable multi-stimulus responsive Janus color-changing fiber with one side green and the other side black (the color-changing fiber diameter is 0.3 mm) was prepared.
[0072] Example 5
[0073] A method for preparing a bistable multi-stimulus responsive Janus color-changing fiber comprises the following steps:
[0074] (1) Dissolve 5 g of sodium alginate in 100 mL of water to obtain a spinning solution;
[0075] (2) 50 mL of spinning solution and 0.5 g of the green bistable thermochromic microcapsules of Example 2 were stirred at room temperature for 1 h to uniformly mix to obtain a bistable thermochromic spinning solution, which was recorded as Janus A spinning solution;
[0076] 50 mL of spinning solution and 2.5 mL of Mxene (mass concentration 80 wt%) were mixed by ultrasonic stirring for 2 h to obtain a spinning solution with photothermal and electrothermal conversion effects, which was recorded as Janus B spinning solution;
[0077] (3) The Janus A spinning solution and the Janus B spinning solution were allowed to stand for 12 h to defoam and were placed in two syringes respectively. Then, the two syringes injected 5 wt% CaCl at a speed of 1 mL / min through the same needle hole. 2 In aqueous solution, a bistable multi-stimulus responsive Janus color-changing fiber with one side green and the other side black (the color-changing fiber diameter is 0.3 mm) was prepared.
[0078] Example 6
[0079] A method for preparing a bistable multi-stimulus responsive Janus color-changing fiber comprises the following steps:
[0080] (1) Dissolve 5 g of sodium alginate in 100 mL of water to obtain a spinning solution;
[0081] (2) 50 mL of spinning solution and 0.5 g of the red bistable thermochromic microcapsules of Example 3 were stirred at room temperature for 1 h to uniformly mix to obtain a bistable thermochromic spinning solution, which was recorded as Janus A spinning solution;
[0082] 50 mL of spinning solution and 2.5 mL of Mxene (mass concentration 80 wt%) were mixed by ultrasonic stirring for 2 h to obtain a spinning solution with photothermal and electrothermal conversion effects, which was recorded as Janus B spinning solution;
[0083] (3) The Janus A spinning solution and the Janus B spinning solution were allowed to stand for 12 h to defoam and were placed in two syringes respectively. Then, the two syringes injected 5 wt% CaCl at a speed of 1 mL / min through the same needle hole. 2 In aqueous solution, a bistable multi-stimulus responsive Janus color-changing fiber with one side red and the other side black (the color-changing fiber has a diameter of 0.3 mm) was prepared.
[0084] Example 7
[0085] A method for preparing a bistable multi-stimulus responsive Janus color-changing fiber comprises the following steps:
[0086] (1) dissolving 5 g of sodium alginate in 100 mL of water to obtain a spinning mother solution of sodium alginate;
[0087] (2) 50 mL of spinning solution and 2 g of the green bistable thermochromic microcapsules of Example 1 were stirred at room temperature for 1 h to uniformly mix to obtain a bistable thermochromic spinning solution, which was recorded as Janus A spinning solution;
[0088] 50 mL of spinning solution and 2.5 mL of Mxene (mass concentration of 80 wt%) were mixed by ultrasonic stirring for 2 h to obtain a spinning solution with photothermal and electrothermal conversion effects, which was recorded as Janus B spinning solution;
[0089] (3) The Janus A spinning solution and the Janus B spinning solution were allowed to stand for 12 h to defoam and were placed in two syringes respectively. Then, the two syringes injected 5 wt% CaCl at a speed of 1 mL / min through the same needle hole. 2 In aqueous solution, a bistable multi-stimulus responsive Janus color-changing fiber with one side green and the other side black was prepared.
[0090] Example 8
[0091] A method for preparing a bistable multi-stimulus responsive Janus color-changing fiber comprises the following steps:
[0092] (1) dissolving 1 g of sodium alginate in 100 mL of water to obtain a spinning mother solution of sodium alginate;
[0093] (2) 50 mL of spinning solution and 2 g of the green bistable thermochromic microcapsules of Example 1 were stirred at room temperature for 1 h to uniformly mix to obtain a bistable thermochromic spinning solution, which was recorded as Janus A spinning solution;
[0094] 50 mL of spinning solution and 2.5 mL of Mxene (mass concentration of 80 wt%) were mixed by ultrasonic stirring for 2 h to obtain a spinning solution with photothermal and electrothermal conversion effects, which was recorded as Janus B spinning solution;
[0095] (3) The Janus A spinning solution and the Janus B spinning solution were allowed to stand for 12 h to defoam and were placed in two syringes respectively. Then, the two syringes injected 5 wt% CaCl at a speed of 1 mL / min through the same needle hole. 2 In aqueous solution, a bistable multi-stimulus responsive Janus color-changing fiber with one side green and the other side black was prepared.
[0096] Example 9
[0097] A method for preparing a bistable multi-stimulus responsive Janus color-changing fiber comprises the following steps:
[0098] (1) dissolving 10 g of sodium alginate in 100 mL of water to obtain a spinning mother solution of sodium alginate;
[0099] (2) 50 mL of spinning solution and 0.5 g of the green bistable thermochromic microcapsules of Example 1 were stirred at room temperature for 1 h to uniformly mix to obtain a bistable thermochromic spinning solution, which was recorded as Janus A spinning solution;
[0100] 50 mL of spinning solution and 2.5 mL of Mxene (mass concentration of 80 wt%) were mixed by ultrasonic stirring for 2 h to obtain a spinning solution with photothermal and electrothermal conversion effects, which was recorded as Janus B spinning solution;
[0101] (3) The Janus A spinning solution and the Janus B spinning solution were allowed to stand for 12 h to defoam and were placed in two syringes respectively. Then, the two syringes injected 5 wt% CaCl at a speed of 1 mL / min through the same needle hole. 2 In aqueous solution, a bistable multi-stimulus responsive Janus color-changing fiber with one side green and the other side black was prepared.
[0102] Comparative Example 1: Omitting Nanomaterials
[0103] The addition of MXene to the Janus B spinning solution of Example 4 was omitted, and the other parts were kept consistent with Example 4 to obtain color-changing fibers.
[0104] Comparative Example 2: Pure Sodium Alginate
[0105] The addition of green thermochromic microcapsules and MXene in Example 4 was omitted, and the other steps were kept the same as in Example 4 to obtain color-changing fibers.
[0106] The bistable multi-stimulus responsive Janus color-changing fibers obtained in Examples 4-6 and Comparative Examples 1-2 were subjected to performance tests, and the test results are as follows:
[0107] Table 1 Response performance of Janus fibers
[0108]
[0109] Comparative Example 3
[0110] The sodium alginate in Example 4 was adjusted to polyacrylonitrile, and the other parts were kept the same as in Example 4 to obtain a color-changing fiber.
[0111] Result: Fiber strength is almost zero and cannot be woven.
[0112] Comparative Example 4
[0113] The sodium alginate in Example 4 was adjusted to polyvinyl alcohol, and the other parts were kept consistent with Example 4 to obtain color-changing fibers.
[0114] Result: No spinning possible.
[0115] Comparative Example 5
[0116] Step (3) in Example 4 was adjusted to mix the Janus A spinning solution and the Janus B spinning solution evenly, and inject 5 wt% CaCl at a speed of 1 mL / min through the same needle hole. 2 In aqueous solution, color-changing fibers are prepared.
[0117] The results showed that the black Janus B spinning solution has a strong covering power and completely covers the color of Janus A. This is also the main reason why color-changing materials cannot be introduced into the corresponding materials according to the stimulus.
[0118] Example 10
[0119] The mass concentrations of Mxene in the Janus B spinning solution of Example 4 were adjusted to 30, 50, 80, and 90 wt %, respectively, and the rest were kept consistent with Example 4 to obtain color-changing fibers.
[0120] The obtained color-changing fiber was subjected to performance testing, and the test results are as follows:
[0121] Table 2 Effect of Mxene concentration on the response performance of Janus fibers
[0122]
[0123]
[0124] Although the present invention has been disclosed as above in the form of a preferred embodiment, it is not intended to limit the present invention. Anyone familiar with this technology can make various changes and modifications without departing from the spirit and scope of the present invention. Therefore, the scope of protection of the present invention should be based on the definition of the claims.
Claims
1. A method for preparing a bistable multi-stimulus responsive Janus color-changing fiber, characterized in that: The method comprises the following steps: (1) Dissolving sodium alginate in water to obtain a spinning solution; (2) taking a portion of the spinning solution and mixing it evenly with the thermochromic microcapsules to obtain a bistable thermochromic spinning solution, which is recorded as Janus A spinning solution; taking another portion of the spinning solution and mixing it evenly with the functional nanomaterials to obtain a spinning solution with photothermal and electrothermal conversion effects, which is recorded as Janus B spinning solution; The preparation method of the thermochromic microcapsules is as follows: 1) Mix urea, formaldehyde, melamine and water evenly, adjust the pH value to 9-10, and polymerize at 60-70°C for 30-60 minutes to obtain melamine / urea / formaldehyde prepolymer MUF; 2) Stirring the phase change material, the thermoacid and the fluorane dye at 65-85° C. for 30-45 min to prepare a bistable thermochromic compound BTC, and then adding the bistable thermochromic compound BTC into an emulsifier aqueous solution to emulsify and form a bistable thermochromic compound emulsion; 3) adding the melamine / urea / formaldehyde prepolymer prepared in step 1) to the bistable thermochromic compound emulsion prepared in step 2), adjusting the pH to 4-5, and reacting at 60-75° C. for 2-5 hours; after the reaction, cooling, washing, and drying to obtain thermochromic microcapsules; The functional nanomaterial is Ti3C2T x , one or more of modified MXene, graphene, graphene oxide, molybdenum disulfide, modified molybdenum disulfide, carbon black, carbon nanotubes, carbon nanorods, silver nanowires, copper nanowires, and gold nanowires; (3) The Janus A spinning solution and the Janus B spinning solution are allowed to stand for defoaming and are placed in two syringes respectively. The two syringes are then injected into a coagulation bath through the same needle hole to prepare the bistable multi-stimulus responsive Janus color-changing fiber.
2. The method according to claim 1, characterized in that The dosage ratio of sodium alginate and water in step (1) is 1-10:100, g / mL.
3. The method according to claim 1, characterized in that In step (2), the mass ratio of the spinning mother solution in the Janus A spinning solution to the spinning mother solution in the Janus B spinning solution is 1:
1.
4. The method according to claim 1, characterized in that The amount ratio of the spinning mother solution and the thermochromic microcapsules in the Janus A spinning solution described in step (2) is 50:0.5~2, mL / g.
5. The method according to claim 1, characterized in that The mass ratio of the spinning solution mother liquid to the functional nanomaterial in the Janus B described in step (2) is 200:3-9.
6. The method according to claim 1, characterized in that The coagulation bath in step (3) is a 5 wt % calcium chloride aqueous solution.
7. A bistable multi-stimulus responsive Janus color-changing fiber prepared by the method described in any one of claims 1 to 6.
8. A color-changing yarn, characterized in that: The color-changing yarn is obtained by spinning the bistable multi-stimulus responsive Janus color-changing fiber described in claim 7.
9. A color-changing fabric, characterized in that: The color-changing fabric is woven by using the bistable multi-stimulus responsive Janus color-changing fiber described in claim 7 or the color-changing yarn described in claim 8.
10. Use of the bistable multi-stimulus responsive Janus color-changing fiber according to claim 7, the color-changing yarn according to claim 8, and the color-changing fabric according to claim 9 in the preparation of smart textiles.
Citation Information
Patent Citations
Method for preparing electrochromic fibers without additional electrodes by coaxial microfluid spinning method
CN112267174A
Preparation method and application of wet response color-changing fiber
CN112962164A
Stimulation responsive yarn with asymmetric structure as well as preparation method and application of stimulation responsive yarn
CN112981653A
Preparation method of coaxial electro-thermochromic liquid crystal fiber
CN113186618A
Electric / thermochromic fluorescent fiber and preparation method and application thereof
CN113969434A