A composite lithium battery separator and its preparation method
By coating the lithium-ion battery separator with a composite coating layer of fluorine-based or acrylic resin polymers and inorganic nanoparticles, the problems of high static electricity, poor adhesion, and poor liquid absorption caused by thinner separators are solved, thereby improving the safety and performance of lithium-ion batteries.
Patent Information
- Application Number
- CN202211639467.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2018-06-26
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2038-06-26
AI Technical Summary
During the thinning process of lithium-ion battery separators, problems such as high static electricity, poor adhesion to the electrode, easy melting and shrinkage leading to short circuits, and poor liquid absorption capacity occur, affecting battery performance and safety.
A composite lithium battery separator is adopted, with a coating layer composed of fluorine or acrylic resin polymers, inorganic nanoparticles and polymer adhesives. The coating layer thickness is 0.5-10μm and the porosity is 30%-60%. The base film thickness is 5-30μm. A porous structure is formed by slurry coating to improve liquid absorption capacity and lithium-ion conductivity.
It enhances the liquid absorption capacity and lithium-ion conductivity of the separator, reduces the risk of battery leakage, improves the adhesion to the electrode and the battery hardness, reduces the risk of short circuit, and is suitable for mass production.
Smart Images

Figure CN116130885B_ABST
Abstract
Description
[0001] This application is a divisional application of the invention patent application No. 201880000766.6, filed on June 26, 2018, entitled "A composite lithium battery separator and its preparation method". Technical Field
[0002] This disclosure relates to the field of lithium-ion batteries, and more specifically, to a composite lithium battery separator and its preparation method. Background Technology
[0003] In recent years, with the booming development of the 3C and electric vehicle markets, the demand for lithium-ion batteries has been increasing, placing new demands on them. The separator, as a crucial component of lithium-ion batteries, acts as an electronic insulator between the positive and negative electrode materials, ensuring mechanical isolation between them. The separator has a specific pore size and porosity to ensure low resistance and high ionic conductivity, allowing good lithium-ion permeability. The characteristics and quality of the separator significantly affect the battery's safety performance, rate performance, cycle life, and basic electrical performance. For example, in traditional consumer electronics, to achieve high battery energy density, more electrode material needs to be accommodated in a small volume, resulting in increasingly thinner separators. Similarly, the increasing range of electric vehicles also demands higher battery energy density, leading to even thinner separators.
[0004] However, the trend of increasingly thinner separators in lithium-ion batteries has also brought some performance issues: Excessive static electricity in the separator can lead to poor adhesion between the separator and the electrodes during battery assembly, or the separator may melt and shrink under high temperatures, causing a short circuit between the positive and negative electrodes; the thinner cells have poorer hardness and mechanical properties, resulting in a decrease in the performance of lithium battery products. Furthermore, from a structural perspective, the poor liquid absorption capacity of the separator in liquid batteries makes liquid leakage a possibility.
[0005] Therefore, improving the liquid absorption capacity of the separator and reducing battery short circuits have become urgent problems to be solved in lithium batteries. Summary of the Invention
[0006] To overcome at least one of the above-mentioned disadvantages, this disclosure provides a composite lithium battery separator with high ionic conductivity, good liquid absorption / retention capacity, strong anti-peeling force, and high adhesion to positive and negative electrode sheets.
[0007] This disclosure also provides a method for preparing a composite lithium battery separator, which is suitable for large-scale production.
[0008] At least one of the objectives of this disclosure can be achieved through the following technical measures.
[0009] A composite lithium battery separator includes a base film or a ceramic film, and a coating layer covering one or both sides of the base film or ceramic film. The coating layer is formed by applying a slurry. The slurry includes 5%-45% coating polymer and 55%-95% organic solvent by weight percentage. The coating polymer includes 10-100 parts of fluorine or acrylic resin polymer, 0.5-10 parts of polymeric adhesive and 0-90 parts of inorganic nanoparticles by weight percentage.
[0010] As a preferred embodiment, the thickness of the base film is 5-30 μm, preferably 10-20 μm; the porosity is 30%-60%, preferably 40%-50%; and the thickness of the coating layer is 0.5-10 μm, preferably 3-8 μm.
[0011] As a preferred embodiment, the base film is selected from a combination of polyethylene base film, polypropylene base film, polypropylene / polyethylene / polypropylene composite base film, polyimide base film, polyvinylidene fluoride film, polyethylene nonwoven base film, polypropylene nonwoven base film, and polyimide nonwoven base film.
[0012] As a preferred embodiment, the organic solvent comprises at least one selected from a combination of acetone, dimethylacetamide, dimethylformamide, chloroform, dichloromethane, dichloroethane, dimethyl sulfoxide, and N-methylpyrrolidone.
[0013] As a preferred embodiment, the fluorinated or acrylic resin polymer comprises at least one selected from the combination of polyvinylidene fluoride, polyvinylidene fluoride and hexafluoropropylene copolymer, polyvinylidene fluoride and dichloroethylene copolymer, polystyrene, n-butyl polyacrylate, polymethyl methacrylate, polyethyl methacrylate, tert-butyl polyacrylate, polyvinyl acetate, polyacrylonitrile, polyvinyl acetate, acrylamide, and polymethyl methacrylate; the molecular weight of the fluorinated or acrylic resin polymer is 50,000-500,000, preferably 200,000-300,000.
[0014] As a preferred embodiment, the polymeric adhesive comprises at least one selected from the combination of styrene-butadiene latex, styrene-acrylic latex, polyvinyl acetate, polyvinyl alcohol, ethyl polyacrylate, polybutyl methacrylate, ethylene-vinyl acetate copolymer, and polyurethane.
[0015] As a preferred method, the inorganic nanoparticles are mainly a mixture of conventional inorganic particles and inorganic particles with lithium-ion conductivity, with a weight ratio of conventional inorganic particles to inorganic particles with lithium-ion conductivity of 80-95:20-5.
[0016] As a preferred embodiment, the conventional inorganic particles comprise at least one selected from a combination of aluminum oxide, silicon dioxide, barium titanate, magnesium oxide, boehmite, titanium dioxide, calcium carbonate, and zirconium dioxide.
[0017] As a preferred method, the particle size range of conventional inorganic particles is 0.01-10 μm; the conventional inorganic particles are composed of low-size inorganic particles and high-size inorganic particles in a weight ratio of 20-10:80-90, with the particle size range of low-size inorganic particles being 0.01-0.2 μm and the particle size range of high-size inorganic particles being 0.2-10 μm.
[0018] As a preferred embodiment, the inorganic particles with lithium-ion conductivity comprise at least one selected from a combination of lithium phosphate, lithium titanium phosphate, lithium aluminum titanium phosphate, lithium nitrogen compounds, and lithium lanthanum titanate.
[0019] As a preferred embodiment, the coating polymer further comprises 0.5-10 parts by weight of a dispersant, the dispersant comprising at least one selected from a combination of carboxylate fluorinated dispersants, triethyl phosphate, sulfonate fluorinated dispersants, sodium polyacrylate, potassium polyacrylate, and polyethylene glycol.
[0020] As a preferred embodiment, the coating polymer further comprises 0.1-8 parts by weight of a wetting agent, the wetting agent comprising at least one selected from the combination of polycarbonate, sodium dodecyl sulfate, sodium dodecylbenzene sulfonate, sodium polyacrylate, polyvinyl alcohol, fluoroalkyl methoxy ether alcohol, fluoroalkyl ethoxy ether alcohol, alkylphenol polyoxyethylene ether, fatty alcohol polyoxyethylene ether, fatty acid polyoxyethylene ether, and polyoxyethylene alkylamide.
[0021] As a preferred embodiment, the coating polymer also includes 0.1-10 parts by weight of a pore-forming agent, wherein the pore-forming agent is deionized water.
[0022] As a preferred embodiment, the coating polymer further comprises 0.1-5 parts by weight of an antistatic agent, the antistatic agent comprising at least one selected from a combination of octadecyl dimethyl quaternary ammonium nitrate, trimethyl octadecyl ammonium acetate, N-hexadecylpyridine nitrate, N-alkyl amino acid salts, betaine-type and imidazoline salt derivatives.
[0023] A method for preparing the above-mentioned composite lithium battery separator includes the following steps:
[0024] S1. Stir the weighed fluorine or acrylic resin polymer and inorganic nanoparticles evenly.
[0025] S2. Add organic solvent according to the gradient of solid content change, and stir evenly;
[0026] S3. Add polymer adhesive, stir evenly, and filter to obtain slurry;
[0027] S4. The slurry is coated on one or both sides of the base film or ceramic film, and after solidification, washing, drying and shaping, the composite lithium battery separator is obtained.
[0028] As a preferred method, the stirring speed in step S1 is 40-80 RPM and the stirring time is 15-40 min; the stirring speed in step S3 is 20-60 RPM, the dispersion speed is 300-800 RPM, the stirring time is 15-30 min, and the slurry viscosity is 50-1000 cp.
[0029] As a preferred method, in step S2, 0.5-10 parts by weight of dispersant are added and stirred at a speed of 40-90 RPM for 10-20 min, and then organic solvent is added.
[0030] As a preferred method, the organic solvent is added gradually at 4%-5% of the total amount. The addition is stopped when the powder is just kneaded and agglomerated. The stirring speed after the powder is kneaded is 80-120 RPM and the stirring time is 30-90 min. Then, the organic solvent is added according to the gradient of solid content change, so that the solid content of the slurry decreases from high to low until it meets the specified solid content.
[0031] As a preferred method, when the solid content is higher than the specified solid content, the stirring speed is 40-100 RPM, the dispersion speed is 2000-4000 RPM, and the stirring time is 15-45 min; when the solid content meets the specified solid content, the stirring speed is 40-80 RPM, the dispersion speed is 3000-4500 RPM, and the stirring time is 30-90 min.
[0032] As a preferred method, in step S4, the coating method includes one of dip coating, microgravure coating, spray coating, slope coating or slot coating, and the drying temperature is 40-80℃.
[0033] Compared with existing technologies, the advantages and beneficial effects of this disclosure include at least the following:
[0034] 1. The composite lithium battery separator disclosed herein has both a porous structure existing on the base film or ceramic film and a porous structure in the coating layer formed by inorganic nanoparticles and adhesives on the base film or ceramic film. Therefore, the composite lithium battery separator has high coating porosity, which can increase the space volume for liquid electrolyte to penetrate, greatly improve the lithium ion conductivity and the liquid absorption and retention rate of the separator, form a gel-like electrolyte, and reduce the risk of battery leakage; it also has strong anti-peeling force and high adhesion to the positive and negative electrode sheets.
[0035] 2. The slurry prepared according to the preparation method of this disclosure has high stability and can still be used normally after being sealed and placed for more than 60 days. No obvious stratification or precipitation occurs, which is conducive to the continuous and large-scale production of the coating layer in the composite lithium battery separator. Therefore, the preparation method of this disclosure is suitable for large-scale production.
[0036] 3. The inorganic nanoparticles with lithium-ion conductivity disclosed herein can have a synergistic effect with conventional inorganic particles, thereby improving lithium-ion conductivity and battery performance.
[0037] 4. The present disclosure uses both high-particle-size and low-particle-size inorganic particles, which will cause the inorganic particles in the coating layer to form a more densely packed morphology, thereby improving the high-temperature resistance of the coating layer and reducing the thermal shrinkage of the diaphragm. Attached Figure Description
[0038] To more clearly illustrate the technical solutions in the specific embodiments of this disclosure or the prior art, the drawings used in the description of the specific embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of this disclosure. For those skilled in the art, other drawings can be obtained from these drawings without creative effort.
[0039] Figure 1 These are electron microscope images of the composite lithium battery separator of Embodiment 1 of this disclosure;
[0040] Figure 2 This is a graph showing the cycle test data of the pouch cells prepared in Example 1 and Comparative Example 2 of this disclosure. Detailed Implementation
[0041] The technical solutions of this disclosure will be clearly and completely described below with reference to the accompanying drawings and specific embodiments. However, those skilled in the art will understand that the embodiments described below are only some embodiments of this disclosure, not all embodiments, and are only used to illustrate this disclosure, and should not be regarded as limiting the scope of this disclosure. Based on the embodiments in this disclosure, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of this disclosure. Where specific conditions are not specified in the embodiments, conventional conditions or conditions recommended by the manufacturer shall be followed. Where the manufacturers of reagents or instruments are not specified, they are all conventional products that can be purchased commercially.
[0042] This disclosure provides a composite lithium battery separator, comprising a base film or a ceramic film, and a coating layer covering one or both sides of the base film or ceramic film. The coating layer is formed by slurry application, wherein the slurry comprises, by weight percentage, 5%-45% of a coating polymer and 55%-95% of an organic solvent, and the coating polymer comprises, by weight, 10-100 parts of a fluorine-based or acrylic resin polymer, 0.5-10 parts of a polymeric adhesive, and 0-90 parts of inorganic nanoparticles. Optionally, the base film thickness is 5-30 μm, preferably 10-20 μm; the porosity is 30%-60%, preferably 40%-50%; and the coating layer thickness is 0.5-10 μm, preferably 3-8 μm.
[0043] In this composite lithium-ion battery separator, fluorine-based or acrylic resin polymers serve as the first binder, and a polymeric adhesive serves as the second binder. These oily polymers and inorganic nanoparticles combine to form a coating layer. Therefore, the composite lithium-ion battery separator of this disclosure possesses both the porous structure present on the base film or ceramic film and the porous structure in the coating layer formed by inorganic nanoparticles and binders on the base film or ceramic film. This results in a high coating porosity, increasing the space volume for liquid electrolyte penetration, significantly improving lithium-ion conductivity and the separator's electrolyte absorption and retention rate, forming a gel-like electrolyte, and reducing the risk of battery leakage. Furthermore, the van der Waals forces between the polar functional groups on the molecular chains of the first and second binders and the electrode materials allow the separator to bond well with the electrodes, reducing the probability of battery short circuits and improving the battery's hardness and shape retention.
[0044] The base film in the composite lithium battery separator disclosed herein can be selected from a combination of polyethylene base film, polypropylene base film, polypropylene / polyethylene / polypropylene composite base film, polyimide base film, polyvinylidene fluoride film, polyethylene nonwoven base film, polypropylene nonwoven base film and polyimide nonwoven base film.
[0045] The organic solvent used in the composite lithium battery separator disclosed herein may specifically include at least one selected from a combination of acetone, dimethylacetamide (DMAC), dimethylformamide (DMF), chloroform, dichloromethane, dichloroethane, dimethyl sulfoxide, and N-methylpyrrolidone (NMP).
[0046] The composite lithium battery separator disclosed herein uses a fluorine-based or acrylic resin polymer that may specifically include at least one selected from the combination of polyvinylidene fluoride, polyvinylidene fluoride and hexafluoropropylene copolymer, polyvinylidene fluoride and dichloroethylene copolymer, polystyrene, n-butyl polyacrylate, polymethyl methacrylate, polyethyl methacrylate, tert-butyl polyacrylate, polyvinyl acetate, polyacrylonitrile, polyvinyl acetate, acrylamide, and polymethyl methacrylate; the molecular weight of the fluorine-based or acrylic resin polymer is 50,000-500,000, preferably 200,000-300,000.
[0047] The polymer adhesive used in the composite lithium battery separator disclosed herein may specifically include at least one selected from the combination of styrene-butadiene latex, styrene-acrylic latex, polyvinyl acetate (PVAC), polyvinyl alcohol (PVA), ethyl polyacrylate (PEA), polybutyl methacrylate (PBMA), ethylene-vinyl acetate copolymer (EVA), and polyurethane (PU).
[0048] The inorganic nanoparticles used in the composite lithium battery separator disclosed herein are primarily a mixture of conventional inorganic particles and inorganic particles with lithium-ion conductivity, with a weight ratio of conventional inorganic particles to lithium-ion conductivity inorganic particles of 80-95:20-5. The lithium-ion conductivity inorganic particles and the conventional inorganic particles (which possess piezoelectric properties) in the inorganic nanoparticles can produce a synergistic effect, improving lithium-ion conductivity and enhancing battery performance.
[0049] Optionally, the conventional inorganic particles comprise at least one selected from a combination of aluminum oxide, silicon dioxide, barium titanate, magnesium oxide, boehmite, titanium oxide, calcium carbonate, and zirconium dioxide. The particle size range of the conventional inorganic particles is 0.01-10 μm; the conventional inorganic particles are composed of low-size inorganic particles and high-size inorganic particles in a weight ratio of 20-10:80-90, where the particle size range of the low-size inorganic particles is 0.01-0.2 μm and the particle size range of the high-size inorganic particles is 0.2-10 μm. This disclosure uses both high-size and low-size inorganic particles simultaneously, resulting in a denser packing of inorganic particles in the coating layer, improving the high-temperature resistance of the coating layer and reducing the thermal shrinkage of the diaphragm.
[0050] Optionally, the inorganic particles with lithium-ion conductivity include at least one selected from a combination of lithium phosphate, lithium titanium phosphate, lithium aluminum titanium phosphate, lithium nitrogen compounds, and lithium lanthanum titanate.
[0051] Based on the above technical solution, the coating polymer in this disclosure may further include 0.5-10 parts by weight of dispersant, wherein the dispersant comprises at least one selected from the combination of carboxylate fluorinated dispersant, triethyl phosphate (TEP), sulfonate fluorinated dispersant, sodium polyacrylate (PAA-Na), potassium polyacrylate (PAA-K) and polyethylene glycol.
[0052] Based on the above technical solutions, the coating polymer in this disclosure may further include 0.1-8 parts by weight of a wetting agent, wherein the wetting agent comprises at least one selected from the combination of polycarbonate, sodium dodecyl sulfate, sodium dodecylbenzene sulfonate, sodium polyacrylate, polyvinyl alcohol, fluoroalkyl methoxy ether alcohol, fluoroalkyl ethoxy ether alcohol, alkylphenol polyoxyethylene ether (APEO), fatty alcohol polyoxyethylene ether (AEO), fatty acid polyoxyethylene ether (FMEE), and polyoxyethylene alkylamide.
[0053] Based on the above technical solution, the coating polymer in this disclosure may further include 0.1-10 parts by weight of a pore-forming agent, which is deionized water. The composite lithium battery separator of this disclosure possesses both the porous structure present in the base film or ceramic film and the porous structure in the coating layer. Simultaneously, the pore-forming agent significantly increases the number of pores in the coating layer, thereby further improving the performance of the composite lithium battery separator. The preferred pore-forming agent is deionized water, which is inexpensive and, during the coagulation and washing processes, does not release excessive impurities in the coagulation and washing tanks, reducing the difficulty of wastewater recovery from these tanks.
[0054] Based on the above technical solution, the coating polymer in this disclosure may further include 0.1-5 parts by weight of an antistatic agent. The antistatic agent comprises at least one selected from the combination of octadecyl dimethyl quaternary ammonium nitrate (SN), trimethyloctadecyl ammonium acetate, N-hexadecylpyridine nitrate, N-alkyl amino acid salts, betaine-type and imidazoline salt derivatives. The use of an antistatic agent in this disclosure results in a membrane surface with low static electricity, reducing the problem of uneven adhesion between the membrane and the electrode during assembly, facilitating battery assembly. The membrane exhibits high anti-peel resistance and strong adhesion to the positive and negative electrode sheets, improving battery rigidity and significantly reducing the risk of internal short circuits.
[0055] This disclosure also provides a method for preparing the above-mentioned composite lithium battery separator, comprising the following steps:
[0056] S1. Stir the weighed fluorine or acrylic resin polymer and inorganic nanoparticles (specifically including high-size inorganic particles, low-size inorganic particles and inorganic particles with lithium-ion conductivity) evenly. Optionally, place the above raw materials in a small-capacity mixing tank and stir evenly at a stirring speed of 40-80 RPM for 15-40 minutes.
[0057] S2. Add organic solvent according to the gradient of solid content change, and stir evenly.
[0058] Optionally, first add the dispersant to a small-capacity mixing tank, stir, and then gradually add the organic solvent. The stirring speed for adding the dispersant is 40-90 rpm, and the stirring time is 10-20 minutes. Then, add the organic solvent gradually at 4%-5% of the total amount. Stop adding the solvent when the powder is just kneaded and agglomerated. After the powder is kneaded, the stirring speed is 80-120 rpm, and the stirring time is 30-90 minutes. Transfer the slurry in the small-capacity mixing tank to a large-capacity mixing tank.
[0059] Next, add organic solvent to the large-capacity mixing tank according to the gradient of solid content changes, so that the solid content of the slurry decreases from high to medium until it meets the specified solid content (high → medium → specified solid content), and stir evenly. During this process, when the solid content is higher than the specified solid content, the stirring speed is 40-100 rpm, the dispersion speed is 2000-4000 rpm, and the stirring time is 15-45 min; when the solid content meets the specified solid content, the stirring speed is 40-80 rpm, the dispersion speed is 3000-4500 rpm, and the stirring time is 30-90 min.
[0060] S3. Add the polymer adhesive, stir evenly, and filter to obtain the slurry. Optionally, add the polymer adhesive, wetting agent, pore-forming agent, and antistatic agent to a large-capacity mixing tank and stir evenly. The stirring speed is 20-60 rpm, the dispersion speed is 300-800 rpm, and the stirring time is 15-30 minutes. The slurry viscosity is 50-1000 cp. Optionally, filter with a 200-mesh nylon screen. The slurry prepared by the above method has high stability and can still be used normally after being sealed and stored for more than 60 days without obvious stratification or precipitation, which is beneficial for the continuous and large-scale production of coatings in composite lithium battery separators.
[0061] S4. The slurry is coated onto one or both sides of the base film or ceramic film, and after solidification, washing, drying and shaping, the composite lithium battery separator is obtained. The coating method includes one of dip coating, microgravure coating, spray coating, slope flow coating or slot coating, and the drying temperature is 40-80℃.
[0062] The above solution will be further explained below with reference to specific embodiments and comparative examples.
[0063] Example 1
[0064] This embodiment provides a composite lithium battery separator, which is prepared according to the following steps:
[0065] ① Place 3 kg of polyvinylidene fluoride and hexafluoropropylene copolymer, 2.42 kg of high-particle-size alumina powder, 430 g of low-particle-size alumina powder and 150 g of lithium titanium phosphate in a small-capacity mixing tank and stir at 70 RPM for 25 min.
[0066] ② Add 120g of polyethylene glycol to a small-capacity mixing tank, and gradually add 1.5kg of NMP. Stir the powder to knead and agglomerate it into a ball, and continue stirring at 110R speed for 50 minutes under this condition. After stirring well, transfer the slurry in the small-capacity mixing tank to a large-capacity mixing tank.
[0067] ③ Add 3 kg of NMP to the large-capacity mixing tank to make the slurry solid content 58%, and stir at a stirring speed of 75R and a dispersion speed of 3000R for 20 minutes; continue to add 10 kg to make the slurry solid content 30%, and stir at a stirring speed of 75R and a dispersion speed of 3000R for 20 minutes; continue to add 11.15 kg to make the slurry solid content 19.3%, and stir at a stirring speed of 80R and a dispersion speed of 3500R for 50 minutes.
[0068] ④ Add 180g of polyvinyl alcohol, 60g of sodium dodecyl sulfate, 30g of deionized water and 60g of octadecyl dimethyl quaternary ammonium nitrate to a large-capacity mixing tank. Stir the slurry at a stirring speed of 30R and a dispersion speed of 600R for 30 minutes. After the slurry is stirred evenly, filter it through a 200-mesh nylon screen to obtain a slurry with a solid content of 20% and a viscosity of 210cp.
[0069] ⑤ A composite lithium battery separator was prepared by applying a slurry to both sides of a polypropylene base membrane with a thickness of 16 μm and a porosity of 47% using a micro-gravure coating method. After coagulation, washing, drying and shaping, the composite lithium battery separator was obtained. The thickness of the composite lithium battery separator was 23 μm, and the thickness of the coating layer on each side was 3.5 μm.
[0070] Example 2
[0071] This embodiment provides a composite lithium battery separator, which is prepared according to the following steps:
[0072] ① Place 3 kg of polyvinylidene fluoride and dichloroethylene copolymer, 2.42 kg of high-particle-size boehmite powder, 430 g of low-particle-size boehmite and 150 g of lithium phosphate in a small-capacity mixing tank and stir at 70 RPM for 25 min.
[0073] ②According to ②-④ of Example 1, a slurry with a solid content of 20% and a viscosity of 230cp can be obtained.
[0074] ③ A composite lithium battery separator was prepared by applying a slurry to both sides of a polypropylene base membrane with a thickness of 12 μm and a porosity of 42% using a micro-gravure coating method. After solidification, washing, drying and shaping, the composite lithium battery separator was obtained. The thickness of the composite lithium battery separator was 18 μm, and the thickness of the coating layer on each side was 3 μm.
[0075] Example 3
[0076] This embodiment provides a composite lithium battery separator, which is prepared according to the following steps:
[0077] ① Place 3 kg of the first binder (polymethyl methacrylate: polyvinylidene fluoride = 20:80), 3.6 kg of high-particle-size boehmite powder, 700 g of low-particle-size boehmite powder and 200 g of lithium aluminum titanium phosphate in a small-capacity mixing tank and stir at 60 RPM for 30 min.
[0078] ② Add 172.5g of sodium polyacrylate to a small-capacity mixing tank, and gradually add 2kg of acetone. Stir the powder to knead and agglomerate it into a ball, and continue stirring at 110R speed for 50 minutes under this condition. After stirring well, transfer the slurry in the small-capacity mixing tank to a large-capacity mixing tank.
[0079] ③ Add 4 kg of acetone to a large-capacity mixing tank to make the slurry solid content 52%, and stir at a stirring speed of 75R and a dispersion speed of 3000R for 20 minutes; continue to add 10 kg to make the slurry solid content 32%, and stir at a stirring speed of 75R and a dispersion speed of 3000R for 20 minutes; continue to add 7.9 kg to make the slurry solid content 24.3%, and stir at a stirring speed of 80R and a dispersion speed of 3500R for 50 minutes.
[0080] ④ Add 180g of styrene-acrylic latex, 60g of sodium dodecylbenzenesulfonate, 30g of deionized water and 60g of trimethyloctadecyl acetate to a large-capacity mixing tank. Stir the slurry at a stirring speed of 30R and a dispersion speed of 600R for 30 minutes. After the slurry is stirred evenly, filter it through a 200-mesh nylon screen to obtain a slurry with a solid content of 25% and a viscosity of 160cp.
[0081] ⑤ A high-adhesion slurry was coated on both sides of a polyethylene base membrane with a thickness of 12μm and a porosity of 40% by spraying. After coagulation, washing, drying and shaping, a composite lithium battery separator was obtained. The thickness of the composite lithium battery separator was 16μm and the thickness of the coating layer on each side was 2μm.
[0082] Example 4
[0083] This embodiment provides a composite lithium battery separator, which is prepared according to the following steps:
[0084] ① Place 3.5 kg of the first binder (polyvinylidene fluoride and hexafluoropropylene copolymer: polymethyl methacrylate = 90:10), 4.4 kg of high-particle-size titanium dioxide powder, 800 g of low-particle-size titanium dioxide powder and 300 g of lithium nitrogen compound in a small-capacity mixing tank and stir at 50 RPM for 30 min.
[0085] ② Add 180g of triethyl phosphate to a small-capacity mixing tank, and gradually add 2.5kg of DMAC. Stir the powder to knead and agglomerate it into a ball, and continue stirring at 110R speed for 50 minutes under this condition. After stirring well, transfer the slurry in the small-capacity mixing tank to a large-capacity mixing tank.
[0086] ③ Add 5 kg of DMAC to the large-capacity mixing tank to make the slurry solid content 55%, and stir at a stirring speed of 75R and a dispersion speed of 3000R for 20 minutes; continue to add 8 kg to make the slurry solid content 37%, and stir at a stirring speed of 75R and a dispersion speed of 3000R for 20 minutes; continue to add 6.9 kg to make the slurry solid content 29.1%, and stir at a stirring speed of 80R and a dispersion speed of 3500R for 50 minutes.
[0087] ④ Add 270g of polybutyl methacrylate, 60g of polycarbonate, 45g of deionized water and 90g of N-hexadecylpyridine nitrate to a large-capacity mixing tank. Stir the slurry at a stirring speed of 30R and a dispersion speed of 600R for 30 minutes. After the slurry is stirred evenly, filter it through a 200-mesh nylon screen to obtain a slurry with a solid content of 30% and a viscosity of 400cp.
[0088] ⑤ A high-adhesion slurry was coated on both sides of a PP / PE / PP composite base film with a thickness of 16μm and a porosity of 45% using an dip-coating method. After coagulation, washing, drying and shaping, a composite lithium battery separator was obtained. The thickness of the composite lithium battery separator was 20μm, and the thickness of the coating layer on each side was 2μm.
[0089] Example 5
[0090] This embodiment provides a composite lithium battery separator, which is prepared according to the following steps:
[0091] ① Place 4.8 kg of polyvinylidene fluoride and hexafluoropropylene copolymer, 969 g of high-particle-size alumina powder, 171 g of low-particle-size alumina powder and 60 g of lithium lanthanum titanate in a small-capacity mixing tank and stir at 70 RPM for 30 min.
[0092] ② Add 120g of sulfonate fluorinated dispersant to a small-capacity mixing tank, and gradually add 1.5kg of NMP. Stir the powder to knead and agglomerate it into a ball, and continue stirring at 110R speed for 50min under this condition. After stirring well, transfer the slurry in the small-capacity mixing tank to a large-capacity mixing tank.
[0093] ③ Add 3 kg of NMP to the large-capacity mixing tank to make the slurry solid content 58%, and stir at a stirring speed of 75R and a dispersion speed of 3000R for 20 minutes; continue to add 15 kg to make the slurry solid content 24%, and stir at a stirring speed of 75R and a dispersion speed of 3000R for 20 minutes; continue to add 17 kg to make the slurry solid content 14.4%, and stir at a stirring speed of 80R and a dispersion speed of 3500R for 50 minutes.
[0094] ④ Add 180g of ethylene-vinyl acetate copolymer, 80g of fluoroalkyl methoxy ether alcohol, 30g of deionized water and 60g of N-alkyl amino acid salt to a large-capacity mixing tank. Stir the slurry at a stirring speed of 30R and a dispersion speed of 600R for 30 minutes. After the slurry is stirred evenly, filter it through a 200-mesh nylon screen to obtain a slurry with a solid content of 15% and a viscosity of 280cp.
[0095] ⑤ A composite lithium battery separator is prepared by applying a slurry to both sides of a single-sided ceramic membrane with a thickness of 16 μm using a micro-gravure coating method. After solidification, washing, drying and shaping, the composite lithium battery separator has a thickness of 18 μm and the coating layer on each side has a thickness of 1 μm.
[0096] Comparative Example 1
[0097] This comparative example provides a lithium battery separator, which is a polypropylene base film with a thickness of 16 μm and a porosity of 47%, and is not coated.
[0098] Comparative Example 2
[0099] This comparative example provides a lithium-ion battery separator coated with a conventional ceramic slurry, with a separator thickness of 22 μm, wherein the base film is a polypropylene base film with a thickness of 16 μm and a porosity of 47%; a coating is formed by coating both sides with a conventional ceramic slurry, and the coating thickness on each side is 3 μm.
[0100] The following tests were conducted to evaluate the products of the examples and comparative examples.
[0101] 1. Electron microscopy was performed on the composite lithium battery separator of Example 1. Figure 1 These are electron microscope images.
[0102] Depend on Figure 1As can be seen, the composite lithium battery separator has a porous structure and a very high porosity. Therefore, the composite lithium battery separator prepared according to the preparation method of this disclosure has high ionic conductivity and good liquid absorption / retention capacity.
[0103] II. The coating porosity, thermal shrinkage data, interfacial adhesion between the coating and the electrode, and the bending strength of the cell of the composite lithium battery separators of Examples 1-5, the lithium battery separator of Comparative Example 1, and the lithium-ion battery separator of Comparative Example 2 were tested. The test conditions for interfacial adhesion were: temperature 90℃, pressure 8MPa, duration 1min, and the electrode was a lithium cobalt oxide electrode. The test data results are shown in Table 1 below.
[0104] Table 1 Product Test Data Results
[0105]
[0106] As can be seen from the table above, the composite lithium battery separator prepared according to the preparation method of this disclosure has good thermal shrinkage performance, high adhesion to the electrode sheet, and high cell bending strength, which is significantly better than the uncoated separator and the separator coated with ceramic slurry in the comparative example.
[0107] Comparative Examples 1 and 2 represent polyolefin and ceramic separators, respectively. While polyolefin separators offer sufficient mechanical strength and chemical stability at room temperature, they may exhibit significant thermal shrinkage at high temperatures. This can cause the positive and negative electrodes to come into contact and rapidly accumulate a large amount of heat, leading to high internal pressure and potentially causing battery combustion or explosion. With the trend towards thinner separators, smaller membrane thicknesses present a relatively high risk of puncture and lower thermal stability. To address this, separator manufacturers have implemented ceramic coatings or water-based polymer coatings on ceramic membranes to strengthen the separator. However, these methods do not effectively improve the adhesion between the separator and the electrodes, or the separator's ability to absorb electrolyte, thus compromising battery safety.
[0108] 3. Soft-pack batteries were prepared using the composite lithium battery separator of Example 1 and the lithium-ion battery separator of Comparative Example 2 under the same process and conditions, and cycle tests were conducted at a 1C charge-discharge rate. Figure 2 This is a data graph for the cyclic test.
[0109] Figure 2 Line a represents the cumulative change in capacity retention rate of the pouch cell corresponding to Example 1 with the number of cycles, and line b represents the cumulative change in capacity retention rate of the pouch cell corresponding to Comparative Example 2 with the number of cycles. Figure 2It can be seen that the capacity retention rate of Example 1 is stable compared with Comparative Example 2. This is because the polymer resin used in this disclosure has a lower specific gravity than the ceramic particles used in Comparative Example 2, which is beneficial to improving the energy density of lithium-ion batteries. Moreover, compared with traditional ceramic slurry, the polymer resin has a lower hardness than alumina, resulting in less wear and tear on equipment during the production process.
[0110] Although this disclosure has been illustrated and described with specific embodiments, it should be understood that the above embodiments are only used to illustrate the technical solutions of this disclosure, and not to limit them; those skilled in the art should understand that modifications can be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions can be made to some or all of the technical features therein, without departing from the spirit and scope of this disclosure; and these modifications or substitutions do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of this disclosure.
[0111] Industrial applicability
[0112] The composite lithium battery separator disclosed herein has high ionic conductivity, good liquid absorption / retention capacity, strong anti-peeling force, and high adhesion to positive and negative electrode sheets. The preparation method of the composite lithium battery separator disclosed herein is suitable for large-scale production, thereby improving its practicality and economy.
Claims
1. A composite lithium battery separator, characterized in that: It includes a base film or a ceramic film, and a coating layer covering one or both sides of the base film or the ceramic film. The coating layer is formed by applying a slurry. The slurry includes, by weight percentage, 5%-45% of a coating polymer and 55%-95% of an organic solvent. The coating polymer includes, by weight, 10-100 parts of a fluorinated or acrylic resin polymer, 0.5-10 parts of a polymeric adhesive, 0-90 parts of inorganic nanoparticles (not equal to 0), 0.5-10 parts of a dispersant, 0.1-8 parts of a wetting agent, and 0.1-5 parts of an antistatic agent. The inorganic nanoparticles are mainly a mixture of conventional inorganic particles and inorganic particles with lithium-ion conductivity. The weight ratio of the conventional inorganic particles to the inorganic particles with lithium-ion conductivity is 80-95:20-5. The conventional inorganic particles are composed of low-size inorganic particles and high-size inorganic particles in a weight ratio of 20-10:80-90. The particle size range of the low-size inorganic particles is 0.01-0.2 μm, and the particle size range of the high-size inorganic particles is 0.2-10 μm. The low-size inorganic particles and high-size inorganic particles form a densely packed structure in the coating layer. The polymeric adhesive comprises at least one selected from the combination of styrene-butadiene latex, styrene-acrylic latex, polyvinyl acetate, polyvinyl alcohol, ethyl polyacrylate, polybutyl methacrylate, ethylene-vinyl acetate copolymer, and polyurethane.
2. The composite lithium battery separator according to claim 1, characterized in that: The base film has a thickness of 5-30 μm and a porosity of 30%-60%; the coating layer has a thickness of 0.5-10 μm.
3. The composite lithium battery separator according to claim 2, characterized in that: The base film has a thickness of 10-20 μm and a porosity of 40%-50%; the coating layer has a thickness of 3-8 μm.
4. The composite lithium battery separator according to claim 1, characterized in that: The base film is selected from one of the following combinations: polyethylene base film, polypropylene base film, polypropylene / polyethylene / polypropylene composite base film, polyimide base film, polyvinylidene fluoride film, polyethylene nonwoven base film, polypropylene nonwoven base film, and polyimide nonwoven base film.
5. The composite lithium battery separator according to claim 1, characterized in that: The organic solvent comprises at least one selected from a combination of acetone, dimethylacetamide, dimethylformamide, chloroform, dichloromethane, dichloroethane, dimethyl sulfoxide, and N-methylpyrrolidone.
6. The composite lithium battery separator according to claim 1, characterized in that: The fluorinated or acrylic resin polymer comprises at least one selected from the combination of polyvinylidene fluoride, polyvinylidene fluoride and hexafluoropropylene copolymer, polyvinylidene fluoride and dichloroethylene copolymer, n-butyl polyacrylate, polymethyl methacrylate, polyethyl methacrylate, tert-butyl polyacrylate and polymethyl methacrylate; the molecular weight of the fluorinated or acrylic resin polymer is 50,000-500,000.
7. The composite lithium battery separator according to claim 6, characterized in that: The molecular weight of the fluorinated or acrylic resin polymer is 200,000-300,000.
8. The composite lithium battery separator according to claim 1, characterized in that: The conventional inorganic particles comprise at least one selected from a combination of aluminum oxide, silicon dioxide, barium titanate, magnesium oxide, boehmite, titanium oxide, calcium carbonate, and zirconium dioxide.
9. The composite lithium battery separator according to claim 1, characterized in that: The inorganic particles with lithium-ion conductivity comprise at least one selected from combinations of lithium phosphate, lithium titanium phosphate, lithium aluminum titanium phosphate, lithium nitrogen compounds, and lithium lanthanum titanate.
10. The composite lithium battery separator according to claim 1, characterized in that: The dispersant comprises at least one selected from the combination of carboxylate fluorinated dispersants, triethyl phosphate, sulfonate fluorinated dispersants, sodium polyacrylate, potassium polyacrylate, and polyethylene glycol.
11. The composite lithium battery separator according to any one of claims 1 to 10, characterized in that: The wetting agent comprises at least one selected from the combination of polycarbonate, sodium dodecyl sulfate, sodium dodecylbenzene sulfonate, sodium polyacrylate, polyvinyl alcohol, fluoroalkyl methoxy ether alcohol, fluoroalkyl ethoxy ether alcohol, alkylphenol polyoxyethylene ether, fatty alcohol polyoxyethylene ether, fatty acid polyoxyethylene ether, and polyoxyethylene alkylamide.
12. The composite lithium battery separator according to any one of claims 1 to 10, characterized in that: The coating polymer also includes 0.1-10 parts by weight of a pore-forming agent, wherein the pore-forming agent is deionized water.
13. The composite lithium battery separator according to any one of claims 1 to 10, characterized in that: The antistatic agent comprises at least one selected from the combination of octadecyl dimethyl quaternary ammonium nitrate, trimethyl octadecyl ammonium acetate, N-hexadecylpyridine nitrate, N-alkyl amino acid salts, betaine-type and imidazoline salt derivatives.
14. A method for preparing a composite lithium battery separator as described in any one of claims 1-13, characterized in that, Includes the following steps: S1. Stir the weighed fluorine or acrylic resin polymer and inorganic nanoparticles evenly. S2. Add organic solvent according to the gradient of solid content change, and stir evenly; S3. Add polymer adhesive, stir evenly, and filter to obtain slurry; S4. The slurry is coated on one or both sides of the base film or ceramic film, and after solidification, washing, drying and shaping, a composite lithium battery separator is obtained.
15. The method for preparing the composite lithium battery separator according to claim 14, characterized in that: The stirring speed in step S1 is 40-80 RPM and the stirring time is 15-40 min; the stirring speed in step S3 is 20-60 RPM, the dispersion speed is 300-800 RPM, the stirring time is 15-30 min, and the slurry viscosity is 50-1000 cp.
16. The method for preparing the composite lithium battery separator according to claim 14, characterized in that: In step S2, 0.5-10 parts by weight of dispersant are added and stirred at a speed of 40-90 RPM for 10-20 minutes, and then organic solvent is added.
17. The method for preparing the composite lithium battery separator according to claim 14 or 16, characterized in that: The method for adding organic solvent is as follows: first, add 4%-5% of the total amount of organic solvent gradually. Stop adding when the powder is just kneaded and agglomerated. After the powder is kneaded, the stirring speed is 80-120 RPM and the stirring time is 30-90 min. Then, add organic solvent according to the gradient of solid content change, so that the solid content of the slurry decreases from high to low until it meets the predetermined solid content.
18. The method for preparing the composite lithium battery separator according to claim 17, characterized in that: When the solid content is higher than the specified solid content, the stirring speed is 40-100 RPM, the dispersion speed is 2000-4000 RPM, and the stirring time is 15-45 min; when the solid content meets the specified solid content, the stirring speed is 40-80 RPM, the dispersion speed is 3000-4500 RPM, and the stirring time is 30-90 min.
19. The preparation method according to claim 14, characterized in that: In step S4, the coating method includes one of dip coating, microgravure coating, spray coating, slope coating or slot coating, and the drying temperature is 40-80℃.
Citation Information
Patent Citations
Organic / inorganic composite separator having morphology gradient, manufacturing method thereof and electrochemical device containing the same
CN101326658A
Lithium iron phosphate aqueous anode slurry and preparation method thereof
CN103943851A
Lithium ion battery diaphragm and preparation method thereof
CN104051696A
Electrode assembly having improved flexural rigidity, method for preparing same, and electrochemical battery comprising same
WO2015076602A1