A method for improving the microscopic morphology of aluminum oxide and the aluminum oxide obtained and its application

By grinding and roasting high-purity alumina, primary crystalline spherical alumina particles are formed, which solves the problems of poor micromorphology and crystalline destruction of alumina powder in the existing technology, and achieves high sphericity, α-alumina The preparation of high-content alumina powder is suitable for the production of a variety of high-performance materials.

CN116216754BActive Publication Date: 2024-10-01CHALCO SHANDONG CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310080258.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-01-31
Publication Date
2024-10-01
Estimated Expiration
2043-01-31

AI Technical Summary

Technical Problem

In the existing preparation methods of high-purity alumina powder, the microscopic morphology is poor, the sphericity is low, the process is complex, and the cost is high. It is difficult to produce alumina powder with good sphericity, and the alumina crystal form is destroyed. , low α-alumina content.

Method used

By grinding high-purity alumina, fine materials with a particle size of D50 = 0.2 to 1 μm are obtained, and then roasted at a temperature of 1050 to 1350°C for 1 to 6 hours to form protocrystalline spherical alumina particles, thereby improving the sphericity and Alpha-alumina content, keeping the crystal form intact.

Benefits of technology

The prepared alumina powder has a spherical shape like the original crystal, with high sphericity, uniform size, and narrow macroscopic particle size distribution. It is suitable as a raw material for high-end ceramic products, battery separators, and high thermal conductivity aluminum nitride powder. The process is simple and suitable for scale. chemical production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116216754B_ABST
    Figure CN116216754B_ABST
Patent Text Reader

Abstract

The embodiment of the present invention provides a method for improving the microscopic morphology of aluminum oxide, and the aluminum oxide obtained and its application, the method comprising: obtaining high-purity aluminum oxide; grinding the high-purity aluminum oxide to obtain fine material with a particle size of D50=0.2-1 μm; calcining the fine material and then cooling it to room temperature to obtain aluminum oxide with good microscopic morphology; wherein the calcination temperature is 1050-1350°C, and the calcination time is 1-6 hours. The present invention grinds high-purity aluminum oxide and then calcines it, and the microscopic morphology of the aluminum oxide powder obtained is: it is original crystal-like spherical, and the original crystal particles have high sphericity, uniform size, and narrow macroscopic particle size distribution, which can be used as original crystal-like spherical aluminum oxide powder for preparing high-end ceramic products, battery separators, and raw materials for high thermal conductivity aluminum nitride powder.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The embodiments of the present invention relate to the technical field of aluminum oxide production, and in particular to a method for improving the microscopic morphology of aluminum oxide, and the aluminum oxide prepared and its application. Background Art

[0002] High-purity alumina powder is an alumina powder with a purity greater than 99.99%. It has excellent properties such as high hardness, wear resistance, abrasion resistance, high temperature resistance, oxidation resistance, good insulation performance, low thermal expansion coefficient, good thermal vibration resistance, and low dielectric loss. As a new functional material, it can be widely used in optical materials, catalyst carriers, single crystal materials, semiconductor substrates, turbine atomic energy and its equipment, bearings, cutting tools, refractory materials, laser materials, thermal insulation materials, etc. High-purity alumina is one of the most advanced materials with the largest output, the highest output value, and the widest application.

[0003] Based on the above-mentioned uses and advantages of high-purity alumina powder, scientific and technological workers at home and abroad are currently paying great attention to the development and application of high-purity alumina. At present, the main methods for preparing high-purity alumina powder are: modified Bayer process, aluminum powder hydrolysis method, hydrothermal method, alcohol aluminum method, and ammonium salt method. However, the high-purity alumina prepared at present has poor microscopic morphology, low sphericity, complex process, high cost, and the product morphology is mainly flake, needle, and flocculent. It is difficult to obtain alumina powder with good sphericity. Patent document 1: CN106241845A discloses a new method for preparing ultra-pure spherical alumina powder, in which gaseous aluminum chloride is pneumatically conveyed and sprayed into a heating area greater than or equal to 2500°C, and ultra-pure aluminum chloride is pyrolyzed to generate aluminum oxide to obtain ultra-pure spherical alumina powder. The product obtained by the method for preparing ultra-pure spherical alumina powder has the advantages of high sphericity, high bulk density, and high purity. However, the patent document shows that the spheres are formed by melting, which are round but the alumina crystal form is destroyed; and the spherical alumina has a low α-alumina content.

[0004] Therefore, how to develop a method to improve the microscopic morphology of alumina, that is, the original crystal particles of alumina with good microscopic morphology have high sphericity, uniform size, narrow macroscopic particle size distribution and high α-alumina content without destroying the crystalline form, has become a key issue for metallurgical workers to study. Summary of the invention

[0005] The purpose of the embodiments of the present invention is to provide a method for improving the microscopic morphology of aluminum oxide, and the aluminum oxide prepared and its application. The microscopic morphology of the prepared aluminum oxide is: spherical in shape of original crystals, and the original crystal particles have high sphericity, uniform size, narrow macroscopic particle size distribution, improved microscopic morphology, no broken crystal form, making the crystal form more complete and high in α-alumina content.

[0006] In order to achieve the above object, an embodiment of the present invention provides a method for improving the microscopic morphology of aluminum oxide, the method comprising:

[0007] Obtain high purity alumina;

[0008] Grinding the high-purity aluminum oxide to obtain fine material with a particle size of D50 = 0.2 to 1 μm;

[0009] The fine material is calcined and then cooled to room temperature to obtain alumina with good microscopic morphology; wherein the calcination temperature is 1050-1350° C. and the calcination time is 1-6 hours.

[0010] Furthermore, the purity of the high-purity alumina is greater than 99.99%; the mass fraction of α-alumina in the high-purity alumina is 80-95%.

[0011] Furthermore, the high-purity alumina is subjected to a grinding process to obtain a fine material with a particle size D50 of 0.2 to 1 μm, which specifically includes:

[0012] Grind the high-purity alumina to obtain a ground raw material with a particle size of D50 = 0.2 to 1 μm;

[0013] The ground raw material is dried and then broken up to obtain fine material with a particle size of D50 = 0.2 to 1 μm.

[0014] Furthermore, the ground raw material has the same particle size as the fine material.

[0015] Furthermore, the grinding process uses a sand mill.

[0016] Furthermore, the drying temperature is 100-150° C., and the drying time is 180-300 min.

[0017] Furthermore, the breaking up is carried out by air flow crushing.

[0018] Furthermore, the obtaining of high-purity alumina comprises:

[0019] Aluminum hydroxide is roasted to obtain high-purity aluminum oxide, wherein the roasting temperature is 1050-1350° C. and the roasting time is 60-360 minutes.

[0020] The embodiment of the present invention also provides aluminum oxide prepared by the method.

[0021] The embodiment of the present invention also provides an application of aluminum oxide, which includes: using the aluminum oxide as a raw material for preparing high-end ceramic products, battery separators and high thermal conductivity aluminum nitride powder.

[0022] One or more technical solutions in the embodiments of the present invention have at least the following technical effects or advantages:

[0023] The embodiment of the present invention provides a method for improving the microscopic morphology of aluminum oxide, the method comprising: obtaining high-purity aluminum oxide; grinding the high-purity aluminum oxide to obtain fine material with a particle size of D50=0.2-1 μm; calcining the fine material and then cooling it to room temperature to obtain aluminum oxide with good microscopic morphology; wherein the calcination temperature is 1050-1350°C and the calcination time is 1-6 hours. By calcining high-purity aluminum oxide with a fine particle size of D50=0.2-1 μm at a temperature of 1050-1350°C for 1-6 hours, aluminum oxide with good microscopic morphology can be obtained. The principle is that fine grinding of high-purity aluminum oxide obtains fine material with concentrated particle size distribution, and the grain size of the fine material is small and controllable; after drying, the fine material is dispersed to reduce soft agglomeration, and the distance between the crystals during calcination is far, which is not conducive to mutual adsorption and growth, thereby forming relatively dispersed spherical aluminum oxide original crystals.

[0024] The microscopic morphology of the aluminum oxide powder prepared by the method of the embodiment of the present invention is: a spherical original crystal, and the original crystal particles have high sphericity, uniform size, and narrow macroscopic particle size distribution. The original crystal spherical aluminum oxide powder can be used as a raw material for preparing high-end ceramic products, battery separators, and high thermal conductivity aluminum nitride powder. At the same time, the process flow is simple and more conducive to technology promotion and large-scale production of products. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] In order to more clearly illustrate the technical solutions in the embodiments of the present invention, the following briefly introduces the drawings required for use in the description of the embodiments. Obviously, the drawings described below are some embodiments of the embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.

[0026] Figure 1 is a flow chart of a method for improving the microscopic morphology of aluminum oxide provided by an embodiment of the present invention;

[0027] Figure 2 is a SEM image of alumina provided in Example 1 of the present invention;

[0028] Figure 3 is a SEM image of alumina provided in Example 2 of the present invention;

[0029] Figure 4 is a SEM image of alumina provided in Example 3 of the present invention;

[0030] Figure 5 is a SEM image of alumina provided in Example 4 of the present invention;

[0031] Figure 6 is a SEM image of alumina provided in Example 5 of the present invention;

[0032] Figure 7 is a SEM image of alumina provided in Example 6 of the present invention;

[0033] Figure 8 is a SEM image of alumina provided in Example 7 of the present invention;

[0034] Fig. 9 This is a SEM image of a high-purity aluminum oxide selected in Example 1 of the present invention before treatment;

[0035] Fig.10 is a SEM image of the aluminum oxide provided in Comparative Example 1 of the present invention;

[0036] Fig.11 is a SEM image of alumina provided in Comparative Example 2 of the present invention;

[0037] Fig.12 is a SEM image of alumina provided in Comparative Example 3 of the present invention;

[0038] Fig.13 It is a SEM picture of alumina provided in Comparative Example 4 of the present invention. DETAILED DESCRIPTION

[0039] The following will be combined with specific implementation methods and examples to specifically describe the embodiments of the present invention, and the advantages and various effects of the embodiments of the present invention will be more clearly presented. It should be understood by those skilled in the art that these specific implementation methods and examples are used to illustrate the embodiments of the present invention, rather than to limit the embodiments of the present invention.

[0040] Throughout the specification, unless otherwise specifically stated, the terms used herein should be understood according to the meanings commonly used in the art. Therefore, unless otherwise defined, all technical and scientific terms used herein have the same meanings as those generally understood by those skilled in the art to which the embodiments of the present invention belong. In the event of a conflict, this specification takes precedence.

[0041] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in the embodiments of the present invention can be purchased from the market or prepared by existing methods.

[0042] The technical solution provided by the embodiment of the present invention is to solve the above technical problems, and the overall idea is as follows:

[0043] According to a typical implementation of an embodiment of the present invention, a preparation method is provided, such as Figure 1 As shown, the method includes:

[0044] S1, obtaining high-purity alumina;

[0045] S2, grinding the high-purity alumina to obtain fine material with a particle size D50 = 0.2 ~ 1 μm;

[0046] S3, calcining the fine material and then cooling to room temperature to obtain alumina with good microscopic morphology; wherein the calcination temperature is 1050-1350°C and the calcination time is 1-6h.

[0047] The current methods for preparing high-purity alumina powder mainly include: modified Bayer process, aluminum powder hydrolysis method, hydrothermal method, aluminum alcohol method, ammonium salt method, etc. Most of them are obtained by calcining aluminum hydroxide; the high-purity alumina prepared at present has poor microscopic morphology, low sphericity, complex process, high cost, and the product morphology is mainly flake, needle and flocculent;

[0048] The applicant has found through experiments that high-purity alumina is ground to obtain fine material with a particle size of D50=0.2~1μm, and then the fine material is calcined and then cooled to room temperature, and the calcination temperature is controlled at 1050~1350℃, and the calcination time is controlled at 1~6h; the microscopic morphology of the prepared alumina powder is: it is spherical in shape of original crystals, and the original crystal particles have high sphericity, uniform size, and narrow macroscopic particle size distribution.

[0049] In this embodiment, the reason for calcining the fine material with a particle size of D50 = 0.2-1 μm is that the particle size of high-purity alumina is finer and the distribution is more concentrated after fine grinding, and the original crystals of high-purity alumina grow again after calcination, thereby improving the sphericity of the original crystal particles and the crystal morphology;

[0050] The reason for controlling the calcination temperature to 1050-1350°C and the calcination time to 1-6h is that under the calcination mechanism, the alumina primary crystals can be fully developed, the crystal morphology is improved, and the extremely small α grains produced in the grinding process do not grow; if the calcination temperature is lower than 1050°C, the temperature is too low, and the primary crystal particles are difficult to grow secondary, which has an adverse effect; if the calcination temperature is higher than 1350°C, the temperature is too high, causing the primary crystals to grow too large, contact each other, form a clustered structure, and finally develop into a worm-like network structure, which has an adverse effect; if the calcination time is less than 1h, the calcination time is too short, the primary crystals grow secondary but the partial crystal morphology is not improved, which has an adverse effect; if the calcination time is greater than 6h, the primary crystals have completed secondary development and the crystal morphology has been improved, and the calcination time is too long, the extremely small α grains produced in the grinding process grow and develop, causing the primary crystals to contact each other and finally develop into a worm-like network structure, which has an adverse effect.

[0051] In this embodiment, the purity of the high-purity alumina is greater than 99.99%; the mass fraction of α-alumina in the high-purity alumina is 80-95%. If the mass fraction of α-alumina in the high-purity alumina is less than 80%, part of the alumina undergoes a crystal phase transformation, the roasting time is long, and the loss on burnout rate increases, which has an adverse effect; if the mass fraction of α-alumina in the high-purity alumina is greater than 95%, the roasting temperature is high and the original crystal is difficult to grow again.

[0052] As an optional embodiment, the method of obtaining high-purity aluminum oxide comprises:

[0053] Aluminum hydroxide is calcined to obtain high-purity aluminum oxide.

[0054] The high-purity alumina can also be obtained by other methods, or can be directly purchased.

[0055] As an optional implementation,

[0056] The grinding of the high-purity alumina to obtain fine material with a particle size of D50 = 0.2 to 1 μm specifically includes:

[0057] Grind the high-purity alumina to obtain a ground raw material with a particle size of D50 = 0.2 to 1 μm;

[0058] The ground raw material is dried and then broken up to obtain fine material with a particle size of D50 = 0.2 to 1 μm.

[0059] The grinding process is performed by a sand mill. A sand mill is more convenient for grinding. Other methods to obtain fine materials with a particle size of D50 = 0.2 to 1 μm are also within the scope of protection of the present invention.

[0060] The above-mentioned dispersion adopts the air flow crushing method. Since the raw materials will be somewhat sticky after drying, the air flow crushing method is conducive to dispersion; other methods, such as a disperser, are likely to introduce impurities into the ground raw materials, reducing the purity. Therefore, high-purity alumina is suitable for air flow crushing, and the air flow pressure is 0.4~0.8MPa.

[0061] The particle size of the ground raw material is the same as that of the fine material. Since the alumina raw material and the fine material have the same particle size as that of the fine material, the alumina raw material and the fine material are only separated during the breaking process and the particle size is not affected.

[0062] According to another typical implementation of the present invention, there is provided an aluminum oxide with high sphericity prepared by the method;

[0063] According to another typical implementation of the embodiment of the present invention, an application of aluminum oxide is provided, and the application includes: using the aluminum oxide as a raw material for preparing high-end ceramic products, battery separators, and high thermal conductivity aluminum nitride powder. Since the microscopic morphology of the prepared aluminum oxide powder is: a spherical original crystal, and the original crystal particles have high sphericity, uniform size, and narrow macroscopic particle size distribution, it can be used as a spherical original crystal aluminum oxide powder for preparing high-end ceramic products, battery separators, and high thermal conductivity aluminum nitride powder raw materials.

[0064] The following will describe in detail the aluminum oxide with high sphericity and the preparation method thereof in combination with the embodiments, comparative examples and experimental data.

[0065] Example 1

[0066] A high-purity alumina (Chalco Shandong high-purity alumina) is selected as a raw material, with a purity of >99.99% and an α-alumina content of 80%; the high-purity alumina is ground with a sand mill until the macroscopic particle size D50=0.5μm; the ground alumina powder is dried, and then ground by air flow milling until the macroscopic particle size D50=0.5μm; the alumina powder treated by air flow milling is calcined at a high temperature, the calcination temperature is 1100°C, and the insulation time is 3h; after the calcination, the alumina powder is taken out when the temperature drops to room temperature, and the alumina powder with high sphericity of the original crystal particles and good microscopic morphology is obtained.

[0067] Example 2

[0068] A high-purity alumina (Chalco Shandong high-purity alumina) is selected as a raw material, with a purity of >99.99% and an α-alumina content of 85%; the high-purity alumina is ground with a sand mill until the macroscopic particle size D50=0.5μm; the ground alumina powder is dried, and then ground by air flow milling until the macroscopic particle size D50=0.5μm; the alumina powder treated by air flow milling is calcined at a high temperature, the calcination temperature is 1100℃, and the insulation time is 3h; after the calcination, the alumina powder is taken out when the temperature drops to room temperature, and the alumina powder with high sphericity of the original crystal particles and good microscopic morphology is obtained.

[0069] Example 3

[0070] A high-purity alumina (Chalco Shandong high-purity alumina) is selected as a raw material, with a purity of >99.99% and an α-alumina content of 90%; the high-purity alumina is ground with a sand mill until the macroscopic particle size D50=0.5μm; the ground alumina powder is dried, and then ground by air flow milling until the macroscopic particle size D50=0.5μm; the alumina powder treated by air flow milling is calcined at a high temperature, the calcination temperature is 1100°C, and the insulation time is 3h; after the calcination, the alumina powder is taken out when the temperature drops to room temperature, and the alumina powder with high sphericity of the original crystal particles and good microscopic morphology is obtained.

[0071] Example 4

[0072] A high-purity alumina (Chalco Shandong high-purity alumina) is selected as a raw material, with a purity of >99.99% and an α-alumina content of 90%; the high-purity alumina is ground with a sand mill until the macroscopic particle size D50=0.2μm; the ground alumina powder is dried, and then ground by air flow milling until the macroscopic particle size D50=0.2μm; the alumina powder treated by air flow milling is calcined at a high temperature, the calcination temperature is 1100℃, and the insulation time is 3h; after the calcination, the alumina powder is taken out when the temperature drops to room temperature, and the alumina powder with high sphericity of the original crystal particles and good microscopic morphology is obtained.

[0073] Example 5

[0074] A high-purity alumina (Chalco Shandong high-purity alumina) is selected as a raw material, with a purity of >99.99% and an α-alumina content of 90%; the high-purity alumina is ground with a sand mill until the macroscopic particle size D50=1.0μm; the ground alumina powder is dried, and then ground by air flow pulverization until the macroscopic particle size D50=1.0μm; the alumina powder pulverized by air flow is calcined at a high temperature, the calcination temperature is 1100℃, and the insulation time is 3h; after the calcination, the alumina powder is taken out when the temperature drops to room temperature, and the alumina powder with high sphericity of the original crystal particles and good microscopic morphology is obtained.

[0075] Example 6

[0076] A high-purity alumina (Chalco Shandong high-purity alumina) is selected as a raw material, with a purity of >99.99% and an α-alumina content of 90%; the high-purity alumina is ground with a sand mill until the macroscopic particle size D50=0.5μm; the ground alumina powder is dried, and then ground by air flow milling until the macroscopic particle size D50=0.5μm; the alumina powder treated by air flow milling is calcined at a high temperature, the calcination temperature is 1050°C, and the insulation time is 6h; after the calcination, the alumina powder is taken out when the temperature drops to room temperature, and the alumina powder with high sphericity of the original crystal particles and good microscopic morphology is obtained.

[0077] Example 7

[0078] A high-purity alumina (Chalco Shandong high-purity alumina) is selected as a raw material, with a purity of >99.99% and an α-alumina content of 90%; the high-purity alumina is ground with a sand mill until the macroscopic particle size D50=0.5μm; the ground alumina powder is dried, and then ground by air flow milling until the macroscopic particle size D50=0.5μm; the alumina powder treated by air flow milling is calcined at high temperature, the calcination temperature is 1350℃, and the insulation time is 1h; after the calcination, the alumina powder is taken out when the temperature drops to room temperature, and the alumina powder with high sphericity of original crystal particles and good microscopic morphology is obtained.

[0079] Comparative Example 1

[0080] The macroscopic particle size of the fine material in this comparative example is D50=0.1 μm, and the remaining steps are the same as those in Example 1.

[0081] Comparative Example 2

[0082] The macroscopic particle size of the fine material in this comparative example is D50=2 μm, and the remaining steps are the same as those in Example 1.

[0083] Comparative Example 3

[0084] In this comparative example, the calcination temperature is 1000° C., the calcination time is 8 h, and the remaining steps are the same as those in Example 1.

[0085] Comparative Example 4

[0086] In this comparative example, the calcination temperature is 1400° C., the calcination time is 0.5 h, and the remaining steps are the same as those in Example 1.

[0087] Experimental Example 1

[0088] The list of parameters for each group is shown in Table 1.

[0089] Table 1

[0090]

[0091] The particle size distribution (D90-D10) / D50 and the α-alumina content in each embodiment and comparative example are statistically shown in Table 2.

[0092] Table 2

[0093]

[0094] From the data in Table 2, we can see that:

[0095] (D90-D10) / D50 is approximately close to 1, indicating a narrower particle size distribution;

[0096] In Comparative Example 1, the macroscopic particle size of the fine material is D50 = 0.1 μm, which is smaller than the range of 0.2 to 1 μm in the embodiment of the present invention, (D90-D10) / D50 is 1.58, and the particle size distribution is wide;

[0097] In Comparative Example 2, the macroscopic particle size of the fine material is D50 = 2 μm, which is larger than the range of 0.2 to 1 μm in the embodiment of the present invention, (D90-D10) / D50 is 1.33, and the particle size distribution is wide;

[0098] In Comparative Example 3, the calcination temperature is 1000°C, which is lower than the range of 1050-1350°C in the embodiment of the present invention, (D90-D10) / D50 is 1.27, and the particle size distribution is wide;

[0099] In Comparative Example 4, the calcination temperature is 1400°C, which is greater than the range of 1050-1350°C in the embodiment of the present invention, (D90-D10) / D50 is 1.18, and the particle size distribution is wide;

[0100] In Examples 1 to 7, the ratio (D90-D10) / D50 of the alumina powder is 0.95-1.05, indicating that the macroscopic particle size distribution is narrow.

[0101] Attached Figure 2 -Attached Fig.13 Description:

[0102] Figure 2-Figure 8 From the SEM images of the alumina in Examples 1-7, it can be seen that the microscopic morphology of the prepared alumina powder is: it is spherical in shape of original crystals, and the original crystal particles have high sphericity, uniform size, unbroken crystal form, complete crystal form, good powder activity, and high thermal conductivity aluminum nitride powder is prepared with concentrated particle size distribution and perfect crystal morphology; high-end ceramic products are prepared to be denser, more wear-resistant, and have a high yield; and battery separators are prepared to be resistant to high temperatures, have high safety, and have good wettability.

[0103] Fig. 9 The SEM image of the high-purity alumina raw material before processing shows that the microscopic morphology is poor, the sphericity is low, the product morphology is mainly flake, needle and flocculent, the particle size distribution is wide, the activity is poor, and the crystal morphology of the aluminum nitride powder is difficult to control; the preparation of high-end ceramic products is prone to cracks and has poor wear resistance; the preparation of battery separators has weak high temperature resistance and poor wettability;

[0104] Figure 10-13 From the SEM images of the alumina of Comparative Examples 1-4, it can be seen that there are disadvantages such as uneven particle size distribution and incomplete crystal morphology of some original crystals.

[0105] Finally, it should be noted that the terms "comprises," "includes," or any other variations thereof are intended to cover non-exclusive inclusion, such that a process, method, article, or apparatus that includes a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements that are inherent to such process, method, article, or apparatus.

[0106] Although the preferred embodiments of the present invention have been described, those skilled in the art may make other changes and modifications to these embodiments once they have learned the basic creative concept. Therefore, the appended claims are intended to be interpreted as including the preferred embodiments and all changes and modifications that fall within the scope of the embodiments of the present invention.

[0107] Obviously, those skilled in the art can make various changes and modifications to the embodiments of the present invention without departing from the spirit and scope of the embodiments of the present invention. Thus, if these modifications and variations of the embodiments of the present invention fall within the scope of the claims of the embodiments of the present invention and their equivalents, the embodiments of the present invention are also intended to include these modifications and variations.

Claims

1. A method for improving the micromorphology of aluminum oxide, characterized in that: The method comprises: Obtain high purity alumina; Grind the high-purity alumina to obtain a ground raw material with a particle size of D50 = 0.2 to 1 μm; The ground raw material is dried and then broken up by air flow pulverization to obtain fine material with a particle size of D50 = 0.2-1 μm, and the air flow pressure is 0.4-0.8 MPa; The fine material is roasted and then cooled to room temperature to obtain alumina with good micromorphology; wherein the purity of the high-purity alumina is greater than 99.99%; the mass fraction of α-alumina in the high-purity alumina is 80-95%, the particle size of the ground raw material is the same as that of the fine material, the roasting temperature is 1050-1350°C, the roasting time is 1-6h, the micromorphology of the alumina with good micromorphology is original crystal spherical, (D90-D10) / D50 is 0.95-1.05, the drying temperature is 100-150°C, and the drying time is 180-300min.

2. A method for improving the microscopic morphology of aluminum oxide according to claim 1, characterized in that: The grinding process adopts a sand mill.

3. A method for improving the microscopic morphology of aluminum oxide according to claim 1, characterized in that: The method of obtaining high-purity aluminum oxide comprises: Aluminum hydroxide is roasted to obtain high-purity aluminum oxide, wherein the roasting temperature is 1050-1350° C. and the roasting time is 60-360 minutes.