A preparation method and application of guanidine-functionalized graphene
By modifying the guanidine functional group on the surface of graphene, the problem of removing azo dyes and pathogenic bacteria in wastewater is solved, the excellent antibacterial properties of graphene are realized, and its application in antibacterial materials is expanded.
Patent Information
- Application Number
- CN202310252313.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-16
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2043-03-16
AI Technical Summary
It is difficult to effectively remove azo dyes and pathogenic bacteria in wastewater with existing technology, and the application of graphene in the antibacterial field has not yet been fully developed.
After uniformly dispersing graphene oxide through ultrasonic, a series of reactions with polyethyleneimine, hydrochloric acid and cyanamide are carried out to form guanidine functional groups, modify the surface of graphene, and prepare guanidine functionalized graphene with excellent antibacterial properties. .
The functional modification of graphene surface was realized, and guanidine-functionalized graphene with rapid sterilization and broad-spectrum antibacterial properties was obtained, expanding its application in antibacterial materials.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of graphene, and in particular to a preparation method of guanidine-functionalized graphene and application thereof. Background Art
[0002] With the continuous development of urbanization, wastewater produced by various industries contains various organic and inorganic pollutants and pathogens, which seriously damage the environment and threaten human health. Therefore, it is an urgent task to develop a green, efficient and safe technology to remove azo dyes and pathogens from wastewater.
[0003] Graphene has a unique honeycomb network structure and is the thinnest, strongest, and most densely structured material. It has excellent application prospects in high-sensitivity sensors, composite materials, and biomedical equipment. In the field of antibacterial, graphene sheets can be physically and mechanically cut, and the bacterial cell membrane and outer barrier can be destroyed through the oxidative stress process, thereby transporting the antibacterial particles loaded on it into the cell, interrupting cell transduction, inactivating intracellular dehydrogenases, and damaging bacterial DNA, showing excellent antibacterial properties.
[0004] Guanidine-containing polymers are typical antibacterial polymers. Under physiological conditions, the positively charged guanidine head has a special rigid planar hydrogen bond donor array, which forms efficient bidentate hydrogen bonds with negatively charged carboxylates, phosphates and sulfates on the bacterial cell membrane, leading to membrane rupture and intracellular lipid outflow, causing bacterial death and bacterial rupture. Currently, guanidine-containing polymers have been widely used in the fields of antibacterial, anti-fouling, drug delivery and uranium adsorption. The present invention prepares a graphene material with excellent antibacterial properties and containing guanidine functional groups. Summary of the invention
[0005] 1. Technical issues to be resolved
[0006] In view of the shortcomings of the prior art, the present invention provides a method for preparing guanidine-functionalized graphene, which realizes the guanidine-functionalized modification of the surface of graphene.
[0007] (II) Technical solution
[0008] A method for preparing guanidine-functionalized graphene:
[0009] (1) adding graphene oxide to distilled water, and obtaining a uniformly dispersed graphene aqueous solution after ultrasonic treatment, and uniformly dispersing polyethyleneimine in distilled water by ultrasonic treatment to obtain a polyethyleneimine aqueous solution;
[0010] (2) adding the polyethyleneimine aqueous solution of step (1) dropwise to the graphene aqueous solution to carry out a reaction, and after the reaction, centrifuging, washing, and drying to obtain polyethyleneimine-grafted graphene;
[0011] (3) The polyethyleneimine-grafted graphene in step (2) is mixed with a hydrochloric acid solution, fully stirred, condensed and refluxed to obtain polyethyleneimine hydrochloride graphene;
[0012] (4) Add the polyethyleneimine hydrochloride graphene in step (3) dropwise into an N,N-dimethylformamide solution containing cyanamide, stir evenly, and heat to react. After the reaction, collect the precipitate by centrifugation, wash it with anhydrous ethanol, an aqueous NaOH solution, and distilled water in sequence until it is neutral, and then wash it with distilled water until it is neutral, to obtain guanidine-functionalized graphene.
[0013] Preferably, in step (1), the concentration of the graphene aqueous solution is 0.05%-0.2%, the concentration of the polyethyleneimine aqueous solution is 0.5%-2%, and the ultrasonic time is 2-4 h.
[0014] Preferably, the reaction time in step (2) is 18-36 h and the temperature is 25-40 °C.
[0015] Preferably, in step (2), the reaction weight ratio of polyethyleneimine to graphene is 3-10:1.
[0016] Preferably, the concentration of the hydrochloric acid solution in step (3) is 6-20%.
[0017] Preferably, in step (3), the reaction temperature is 60-80°C and the reaction time is 3-8 h.
[0018] Preferably, in step (4), the reaction weight ratio of polyethyleneimine hydrochloride graphene and cyanamide is 1:2-6.
[0019] Preferably, in step (4), the reaction temperature is 90-120° C. and the reaction time is 6-12 h.
[0020] 3. Beneficial technical effects
[0021] Polyethyleneimine is reacted with the epoxy group of graphene oxide to achieve polyethyleneimine grafted graphene, and then hydrochloric acid is used to react with the amino group of polyethyleneimine to form an aminohydrochloric acid structure, which is then reacted with monocyanamide to generate a guanidine functional group to obtain guanidine functionalized graphene, thereby modifying the graphene surface with abundant guanidine functional groups, thus achieving surface functional modification of graphene. The guanidine functional group modified with graphene has the advantages of fast sterilization rate, good broad-spectrum antibacterial property, and non-toxicity and safety, which expands the development and application of graphene in antibacterial materials. DETAILED DESCRIPTION
[0022] To achieve the above object, the present invention provides the following specific implementation methods and examples: A method for preparing guanidine-functionalized graphene, the preparation method comprising the following steps:
[0023] (1) adding 0.2 g of graphene oxide to distilled water, and obtaining a graphene aqueous solution with a uniform dispersion concentration of 0.05%-0.2% after ultrasonic treatment, and uniformly dispersing 0.6-2 g of polyethyleneimine in distilled water by ultrasonic treatment to obtain a polyethyleneimine aqueous solution with a concentration of 0.5%-2%;
[0024] (2) adding the polyethyleneimine aqueous solution of step (1) dropwise to the graphene aqueous solution to carry out the reaction at a temperature of 25-40°C for a time of 18-36 h, centrifuging, washing, and drying to obtain polyethyleneimine-grafted graphene;
[0025] (3) The polyethyleneimine-grafted graphene in step (2) is mixed with a 6-20% hydrochloric acid solution, fully stirred, condensed and refluxed at a reaction temperature of 60-80°C and a reflux time of 3-8 h to obtain polyethyleneimine hydrochloride graphene.
[0026] (4) Add dropwise 0.3 g of polyethyleneimine hydrochloride graphene in step (3) into a solution of N,N-dimethylformamide containing 0.6-1.8 g of cyanamide, stir evenly, and heat to react at a temperature of 90-120 °C for 6-12 h. After the reaction, collect the precipitate by centrifugation, wash it with anhydrous ethanol, a NaOH aqueous solution, and distilled water in sequence until it is neutral, and then wash it with distilled water until it is neutral to obtain guanidine-functionalized graphene. Example 1
[0027] (1) 0.2 g of graphene oxide was added to distilled water, and after ultrasonic treatment, a graphene aqueous solution with a uniform dispersion concentration of 0.15% was obtained. 0.8 g of polyethyleneimine was uniformly dispersed in distilled water by ultrasonic treatment to obtain a polyethyleneimine aqueous solution with a concentration of 0.1%;
[0028] (2) adding the polyethyleneimine aqueous solution of step (1) dropwise to the graphene aqueous solution to carry out a reaction at 25° C. for 18 h, centrifuging, washing, and drying to obtain polyethyleneimine-grafted graphene;
[0029] (3) The polyethyleneimine grafted graphene in step (2) is mixed with a 6% hydrochloric acid solution, fully stirred, condensed and refluxed at a reaction temperature of 60°C and a reflux time of 3 h to obtain polyethyleneimine hydrochloride graphene.
[0030] (4) Add dropwise 0.3 g of polyethyleneimine hydrochloride graphene in step (3) into a solution of N,N-dimethylformamide containing 1.6 g of cyanamide, stir evenly, and heat to react at 105 °C for 10 h. After the reaction, collect the precipitate by centrifugation, wash with anhydrous ethanol, NaOH aqueous solution, and distilled water in sequence until neutral, and then wash with distilled water until neutral to obtain guanidine-functionalized graphene. Example 2
[0031] (1) 0.2 g of graphene oxide was added to distilled water, and after ultrasonic treatment, a graphene aqueous solution with a uniform dispersion concentration of 0.05%-0.2% was obtained. 0.6 g of polyethyleneimine was uniformly dispersed in distilled water by ultrasonic treatment to obtain a polyethyleneimine aqueous solution with a concentration of 0.5%;
[0032] (2) adding the polyethyleneimine aqueous solution of step (1) dropwise to the graphene aqueous solution to carry out the reaction at 30°C for 25 h, centrifuging, washing and drying to obtain polyethyleneimine grafted graphene;
[0033] (3) The polyethyleneimine grafted graphene in step (2) is mixed with 8% hydrochloric acid solution, fully stirred, condensed and refluxed at a reaction temperature of 65°C and a reflux time of 5 h to obtain polyethyleneimine hydrochloride graphene.
[0034] (4) Add dropwise 0.3 g of polyethyleneimine hydrochloride graphene in step (3) into a solution of N,N-dimethylformamide containing 1.8 g of cyanamide, stir evenly, and heat to react at 120 °C for 12 h. After the reaction, collect the precipitate by centrifugation, wash with anhydrous ethanol, NaOH aqueous solution, and distilled water in sequence until neutral, and then wash with distilled water until neutral to obtain guanidine-functionalized graphene. Example 3
[0035] (1) 0.2 g of graphene oxide was added to distilled water, and after ultrasonic treatment, a graphene aqueous solution with a uniform dispersion concentration of 0.13% was obtained. 1.5 g of polyethyleneimine was uniformly dispersed in distilled water by ultrasonic treatment to obtain a polyethyleneimine aqueous solution with a concentration of 1.8%;
[0036] (2) adding the polyethyleneimine aqueous solution of step (1) dropwise to the graphene aqueous solution to carry out the reaction at a temperature of 28°C for 32 h, centrifuging, washing and drying to obtain polyethyleneimine grafted graphene;
[0037] (3) The polyethyleneimine-grafted graphene in step (2) is mixed with 20% hydrochloric acid solution, fully stirred, condensed and refluxed at a reaction temperature of 80°C and a reflux time of 8 h to obtain polyethyleneimine hydrochloride graphene.
[0038] (4) Add dropwise 0.3 g of polyethyleneimine hydrochloride graphene in step (3) into a solution of N,N-dimethylformamide containing 0.6 g of cyanamide, stir evenly, and heat to react at 90 °C for 6 h. After the reaction, collect the precipitate by centrifugation, wash with anhydrous ethanol, NaOH aqueous solution, and distilled water in sequence until neutral, and then wash with distilled water until neutral to obtain guanidine-functionalized graphene. Example 4
[0039] (1) 0.2 g of graphene oxide was added to distilled water, and after ultrasonic treatment, a graphene aqueous solution with a uniform dispersion concentration of 0.14% was obtained. 1.2 g of polyethyleneimine was uniformly dispersed in distilled water by ultrasonic treatment to obtain a polyethyleneimine aqueous solution with a concentration of 0.17%;
[0040] (2) adding the polyethyleneimine aqueous solution of step (1) dropwise to the graphene aqueous solution to carry out the reaction at a temperature of 32° C. for 35 h, centrifuging, washing, and drying to obtain polyethyleneimine-grafted graphene;
[0041] (3) The polyethyleneimine-grafted graphene in step (2) is mixed with 18% hydrochloric acid solution, fully stirred, condensed and refluxed at a reaction temperature of 65°C and a reflux time of 4 h to obtain polyethyleneimine hydrochloride graphene.
[0042] (4) Add dropwise 0.3 g of polyethyleneimine hydrochloride graphene in step (3) into a solution of N,N-dimethylformamide containing 0.9 g of cyanamide, stir evenly, and heat to react at 115 °C for 8 h. After the reaction, collect the precipitate by centrifugation, wash with anhydrous ethanol, NaOH aqueous solution, and distilled water in sequence until neutral, and then wash with distilled water until neutral to obtain guanidine-functionalized graphene. Example 5
[0043] (1) 0.2 g of graphene oxide was added to distilled water, and after ultrasonic treatment, a graphene aqueous solution with a uniform dispersion concentration of 0.2% was obtained. 2 g of polyethyleneimine was uniformly dispersed in distilled water by ultrasonic treatment to obtain a polyethyleneimine aqueous solution with a concentration of 2%;
[0044] (3) The polyethyleneimine-grafted graphene in step (2) is mixed with a 14% hydrochloric acid solution, fully stirred, condensed and refluxed at a reaction temperature of 76°C and a reflux time of 6 h to obtain polyethyleneimine hydrochloride graphene.
[0045] (2) adding the polyethyleneimine aqueous solution of step (1) dropwise to the graphene aqueous solution to carry out the reaction at 40°C for 36 h, centrifuging, washing and drying to obtain polyethyleneimine grafted graphene;
[0046] (4) Add dropwise 0.3 g of polyethyleneimine hydrochloride graphene in step (3) into a solution of N,N-dimethylformamide containing 1.2 g of cyanamide, stir evenly, and heat to react at 95 °C for 9 h. After the reaction, collect the precipitate by centrifugation, wash with anhydrous ethanol, NaOH aqueous solution, and distilled water in sequence until neutral, and then wash with distilled water until neutral to obtain guanidine-functionalized graphene.
[0047] Take 0.5 mL of the solution with a concentration of 1.0×10 7 CFU / mL Escherichia coli liquid and 0.5 mL of dispersion containing guanidine-functionalized graphene were taken at different time periods, diluted 1000 times with physiological saline, and 80 μL of each was applied. The coated culture dish was placed in a constant temperature box, set at 37°C, and the culture time was 20 h. The concentration of the suspension after culture was measured to test the antibacterial rate.
[0048] The antibacterial rate of the guanidine-functionalized graphene prepared in each embodiment against Escherichia coli reached 93.51-99.92%, showing excellent antibacterial properties.
Claims
1. A method for preparing guanidine-functionalized graphene, characterized in that: The preparation method of the guanidine-functionalized graphene is as follows: (1) adding graphene oxide to distilled water, and obtaining a uniformly dispersed graphene aqueous solution after ultrasonic treatment, and uniformly dispersing polyethyleneimine in distilled water by ultrasonic treatment to obtain a polyethyleneimine aqueous solution; (2) adding the polyethyleneimine aqueous solution of step (1) dropwise to the graphene aqueous solution to carry out a reaction, and after the reaction, centrifuging, washing, and drying to obtain polyethyleneimine-grafted graphene; (3) The polyethyleneimine-grafted graphene in step (2) is mixed with a hydrochloric acid solution, fully stirred, condensed and refluxed to obtain polyethyleneimine hydrochloride graphene; (4) Add the polyethyleneimine hydrochloride graphene in step (3) dropwise into an N,N-dimethylformamide solution containing cyanamide, stir evenly, and heat to react. After the reaction, collect the precipitate by centrifugation, wash it with anhydrous ethanol, an aqueous NaOH solution, and distilled water in sequence until it is neutral, and then wash it with distilled water until it is neutral, to obtain guanidine-functionalized graphene.
2. The method for preparing guanidine-functionalized graphene according to claim 1, characterized in that: In the step (1), the concentration of the graphene aqueous solution is 0.05%-0.2%, the concentration of the polyethyleneimine aqueous solution is 0.5%-2%, and the ultrasonic time is 2-4 h.
3. The method for preparing guanidine-functionalized graphene according to claim 1, characterized in that: The reaction time in step (2) is 18-36 h and the temperature is 25-40 °C.
4. The method for preparing guanidine-functionalized graphene according to claim 1, characterized in that: In the step (2), the reaction weight ratio of polyethyleneimine to graphene is 3-10:
1.
5. The method for preparing guanidine-functionalized graphene according to claim 1, characterized in that: The concentration of the hydrochloric acid solution in step (3) is 6-20%.
6. The method for preparing guanidine-functionalized graphene according to claim 1, characterized in that: In the step (3), the reaction temperature is 60-80°C and the reaction time is 3-8 h.
7. The method for preparing guanidine-functionalized graphene according to claim 1, characterized in that: In the step (4), the reaction weight ratio of polyethyleneimine hydrochloride graphene and cyanamide is 1:2-6.
8. The method for preparing guanidine-functionalized graphene according to claim 1, characterized in that: In the step (4), the reaction temperature is 90-120°C and the reaction time is 6-12 h.