A kind of adhesive for formaldehyde-free artificial board, preparation and application
The viscosity stabilizer is prepared by the reaction of polyvinyl alcohol and isocyanate curing agent, which solves the problems of poor initial viscosity and short active period of the aldehyde-free adhesive, and achieves free adjustment of viscosity and extended active period, satisfying the different artificial boards Production needs ensure safe, environmentally friendly and low-cost production.
Patent Information
- Application Number
- CN202310151711.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-02-22
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2043-02-22
AI Technical Summary
The existing adhesives for artificial-free artificial boards have shortcomings in the initial viscosity and active period, the viscosity is difficult to adjust, and the processing performance is poor, which cannot meet the production needs of different types of artificial boards.
The viscosity stabilizer is prepared by first reacting polyvinyl alcohol with isocyanate curing agent. By controlling the dosage and type of main glue and curing agent, the viscosity and activity period of the adhesive are adjusted, and the adhesive formula is formed to meet the needs of different applications to avoid The use of flour is to reduce production costs and improve glue strength.
It realizes free adjustment of adhesive viscosity, extends the active period to more than 72 hours, meets the production needs of different types of artificial boards, is safe and environmentally friendly, reduces process costs, and improves the bonding strength.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of formaldehyde-free adhesives for wood, and more specifically, to a formaldehyde-free adhesive for artificial boards, and its preparation and application. Background Art
[0002] About 90% of the formaldehyde-containing adhesives used in artificial boards are urea-formaldehyde resins. The advantages of using urea-formaldehyde resin to prepare artificial boards are mature production processes, water-resistant boards, and high bonding strength. The disadvantage is that they release formaldehyde over a long period of time. Studies have shown that artificial boards made from urea-formaldehyde resin can release formaldehyde for up to 15 years, and the release of formaldehyde is more obvious in high temperature and high humidity environments. my country stipulates that the formaldehyde content in the indoor environment of civil buildings cannot exceed 0.08 mg / m 3 Excessive formaldehyde may cause throat and eye discomfort at the least, or cause breathing difficulties and vomiting at the worst, and may even cause irreversible physiological diseases. People who are in an environment with excessive formaldehyde for a long time may induce leukemia, especially for young children, pregnant women and the elderly. In June 2004, the World Health Organization has classified formaldehyde as a Class I carcinogen. On May 1, 2018, the new version of the mandatory national standard GB 18580-2017 "Limits of formaldehyde emission in artificial boards and their products for indoor decoration and renovation materials" cancelled the E2 limit mark and only retained the E1 limit mark, which put forward higher requirements for the environmental performance of artificial boards. Starting from October 1, 2021, GB / T39598-2021 "Guidelines for indoor load limits of artificial boards based on limit formaldehyde emission" and GB / T39600-2021 "Grading of formaldehyde emission of artificial boards and their products" will be implemented. The E0 level in the new national standard is higher than the European standard and directly matches the US formaldehyde-free exemption level. The ENF level even exceeds the highest standard in Japan. my country's new national standard has become the most stringent standard in the world, which will inevitably bring more opportunities and challenges to my country's wood-based panel industry. Reducing the formaldehyde emission of wood-based panels has become a key issue related to national health and economic development.
[0003] Isocyanate compounds are a type of non-aldehyde adhesive, such as PMDI adhesive. Since they do not contain formaldehyde, they are green and environmentally friendly, and have good water resistance. They are a new direction for the development of formaldehyde-free adhesives in recent years. However, researchers have also found that directly using isocyanate as an adhesive to prepare artificial boards will result in poor initial adhesion, too fast glue penetration, and poor processing performance of artificial boards. For this reason, isocyanate is generally compounded with other adhesives. For example, water-based vinyl resins such as polyvinyl alcohol aqueous solution, polyvinyl acetate emulsion, and acrylic emulsion are used as the main emulsion, and isocyanate is added as a curing agent to form a water-based polymer-isocyanate adhesive, which provides a higher bonding strength. However, it is also found that the viscosity of the water-based polymer in this type of adhesive increases too fast after compounding with isocyanate, resulting in a short active period of the system, which needs to be ready for use, and the viscosity is not easy to adjust over a large range, all of which limit the application of such formaldehyde-free adhesives.
[0004] Therefore, it is necessary to develop a formaldehyde-free adhesive with freely adjustable viscosity and long activity period to overcome the problems existing in the prior art. Summary of the invention
[0005] In order to solve the above problems, the first object of the present invention is to provide an adhesive for formaldehyde-free artificial boards. The adhesive system does not contain formaldehyde, is safe and environmentally friendly to use, has a small amount of glue applied, good initial adhesion, can freely adjust the viscosity of the adhesive according to different usage requirements, and does not require the addition of flour when preparing multilayer boards. At the same time, the active period after the main glue and the curing agent are mixed is extended to a maximum of more than 72 hours, and can be widely used in the production of different types of artificial boards.
[0006] The second object of the present invention is to provide a method for preparing the formaldehyde-free adhesive for artificial panels as described above.
[0007] The third object of the present invention is to provide an application of the formaldehyde-free adhesive for artificial boards in the preparation of artificial boards. The prepared high-viscosity adhesive can be directly used to prepare plywood, etc., and the low-viscosity adhesive can be used to produce fiberboards and particleboards, etc. by atomization sizing.
[0008] In the present invention, the activity period refers to the time from the start of mixing of the main adhesive and the curing agent in a two-component adhesive to the time when the fluidity deteriorates and the adhesive cannot be applied.
[0009] In order to achieve the above first purpose, the technical solution provided by the present invention is:
[0010] The present invention discloses an adhesive for formaldehyde-free artificial panels, which is prepared from the following raw materials in parts by weight:
[0011] 36-375 parts of viscosity stabilizer, 100 parts of aqueous emulsion, 0.1-10 parts of filler and 2-25 parts of first curing agent;
[0012] The viscosity stabilizer is prepared from 100 parts of polyvinyl alcohol and 0.1-10 parts of a second curing agent under the action of a catalyst.
[0013] In the prior art, although mixing isocyanate with a water-based polymer with good initial viscosity can solve the problem of poor initial viscosity of isocyanate, it also leads to the problem of too fast viscosity growth and shortened activity period of the system. If other substances are introduced to inhibit the combination of isocyanate and water-based polymer, the binding strength between the two may be destroyed, and additional production considerations (such as high cost, matching of production equipment, process adjustment, etc.) will be brought about, which will also affect the continuous production of adhesives. In order to solve this technical problem and minimize the impact on production to the greatest extent, the inventors designed a new adhesive formula for formaldehyde-free artificial panels, using polyvinyl alcohol and a certain amount of isocyanate curing agent to react in advance to prepare a viscosity stabilizer, so that the isocyanate consumes a part of the hydroxyl groups on the polyvinyl alcohol molecules in advance. Then, the performance of the adhesive is controlled by controlling the main glue and the remaining amount of isocyanate curing agent. And through a large number of experimental screenings, we finally determined the dosage relationship between the two additions of curing agent and polyvinyl alcohol, so that the viscosity of the resulting adhesive meets the needs of different applications, while ensuring its activity period and bonding strength, providing technicians with adhesives with different formulas.
[0014] In the present invention, the viscosity stabilizer is used to adjust the viscosity and activity period of the adhesive, and the viscosity stabilizer is prepared by the following method:
[0015] Dissolve 100 parts of polyvinyl alcohol in 255-1550 parts of deionized water, add 0.1-10 parts of the second curing agent and 0.0005-0.05 parts of the catalyst, and stir and react at 30-60° C. for 0.5-6 hours to obtain the product.
[0016] Furthermore, polyvinyl alcohol can react with the second curing agent to achieve cross-linking to control the viscosity of the adhesive. Therefore, the viscosity of the adhesive can be freely adjusted from 50-80000 mPa.s by changing the type and amount of polyvinyl alcohol and the second curing agent to meet different application requirements; when a low-viscosity adhesive needs to be prepared, polyvinyl alcohol with a smaller degree of polymerization is selected, and when a high-viscosity adhesive needs to be prepared, polyvinyl alcohol with a larger degree of polymerization is replaced to participate in the reaction. In a specific embodiment, the degree of polymerization of the polyvinyl alcohol is 300-2400, and the degree of alcoholysis is 78-99%. For example: polyvinyl alcohol 2499, degree of polymerization 2400, alcoholysis degree (molar fraction) is 98%-99%; polyvinyl alcohol 1788, degree of polymerization 1700, alcoholysis degree (molar fraction) 87.0%~89.0%, etc.
[0017] Further, the first curing agent or the second curing agent includes but is not limited to one or more of aromatic polyisocyanate, aliphatic polyisocyanate, aromatic aliphatic polyisocyanate or alicyclic polyisocyanate, and the first curing agent and the second curing agent may be the same or different; illustratively, the aromatic polyisocyanate is selected from toluene diisocyanate or polymethylene polyphenyl polyisocyanate (PAPI), etc. The aliphatic polyisocyanate is selected from hexamethylene diisocyanate, etc. The aromatic aliphatic polyisocyanate is selected from xylylene diisocyanate, etc. The alicyclic polyisocyanate is selected from isophorone diisocyanate, etc.
[0018] Further, the catalyst includes but is not limited to one or more of N,N-dimethylcyclohexylamine, bismuth cycloalkaneate, bismuth octanoate, bismuth laurate, bismuth isooctanoate, dibutyltin dilaurate, stannous octoate, N,N'-lutidine, N,N-dimethylethanolamine, triethanolamine, N-2-hydroxypropyldimethylmorpholine, N,N'-bis-(α-hydroxypropyl)-2-methylpiperazine, N,N'-diethyl-2-methylpiperazine, N,N'-diethylpiperazine, N-methylmorpholine, N-ethylmorpholine, triethyleneimine, N,N-dimethylbutylamine, N,N-dimethylhexadecylamine, N,N-dimethylbenzylamine, triethylamine, triethylenediamine or N,N-dimethylcyclohexylamine.
[0019] Further, the aqueous emulsion is prepared by the following method:
[0020] (1) 40-85 parts of soft monomer and 15-60 parts of hard monomer are mixed, and 2-5 parts of emulsifier and 120-400 parts of deionized water are added for pre-emulsification to obtain a pre-emulsified liquid;
[0021] (2) Add 0.3-1.0 parts of initiator to the above pre-emulsifier and react at 70-80°C for 3-6 hours to obtain;
[0022] Further, the soft monomer includes but is not limited to one or more of vinyl acetate, allyl acetate, n-butyl acrylate, isobutyl acrylate, isooctyl acrylate, ethyl acrylate, sec-butyl acrylate, n-propyl acrylate, lauryl acrylate, 2-ethylhexyl acrylate, 2-ethylhexyl methacrylate, lauryl methacrylate, 2-hydroxyethyl acrylate, 2-hydroxypropyl acrylate or vinyl acetate;
[0023] Further, the hard monomer includes, but is not limited to, one or more of methyl methacrylate, styrene, ethyl methacrylate, acrylonitrile, acrylic acid, methacrylic acid, acrylamide, N-hydroxymethyl acrylamide, n-butyl methacrylate, isobutyl methacrylate, tert-butyl methacrylate, octadecyl methacrylate, cyclohexyl methacrylate, or isobornyl methacrylate;
[0024] Further, the emulsifier includes but is not limited to one or more of sodium dodecylbenzene sulfonate, sodium dodecyl sulfate, sodium ethoxylated alkyl sulfate, ammonium ethoxylated alkyl sulfate, alkylphenol polyoxyethylene ether formaldehyde condensate, phenylethylphenol polyoxyethylene ether formaldehyde condensate, isopropylphenylphenol polyoxyethylene ether formaldehyde condensate or benzylphenol polyoxyethylene ether formaldehyde condensate;
[0025] Furthermore, the initiator is ammonium persulfate or potassium persulfate.
[0026] Further, the filler includes but is not limited to one or more of montmorillonite, talc, bentonite, kaolin, diatomaceous earth, tannin, heavy calcium, barium sulfate or mica powder. It is particularly necessary to point out here that the type of filler does not include flour. The reason is that the introduction of flour will increase the production cost of the adhesive and waste flour resources. Another reason is that flour contains a large amount of hydroxyl groups, which will preferentially and quickly react with isocyanate curing agents, not only reducing the active period of the adhesive, but also consuming the effective addition amount of isocyanate curing agents, reducing the bonding strength. However, not introducing flour will inevitably cause a decrease in the viscosity of the adhesive. For this reason, the present application achieves the requirement for adhesive viscosity in the application without adding flour by adjusting the amount of the first curing agent and the control of the components and the amount of the viscosity stabilizer.
[0027] In order to achieve the above second purpose, the technical solution provided by the present invention is:
[0028] The present invention discloses a method for preparing the adhesive for the formaldehyde-free artificial board, comprising the following steps:
[0029] The viscosity stabilizer, aqueous emulsion and filler are mixed and stirred to obtain the main glue, and then the first curing agent is added and stirred until uniform.
[0030] In order to achieve the third object above, the technical solution provided by the present invention is:
[0031] The invention discloses a formaldehyde-free artificial board, wherein the formaldehyde-free artificial board comprises the adhesive as described above or the adhesive prepared by the method as described above.
[0032] Furthermore, the formaldehyde-free artificial board is a common type available on the market, including but not limited to particle board, fiberboard, blockboard, plywood or structural composite wood. The production processes of several artificial boards are listed below for illustration:
[0033] When preparing particleboard, the preparation steps may be:
[0034] 1) Select the required raw materials and control the required water content;
[0035] 2) Control the glue application amount to 90-160 kg / m3 The main glue and the first curing agent are applied to the raw materials by atomization, and then the raw materials after gluing are mixed and placed in a mold or on a carrier. After paving, pre-pressing, hot pressing, edge sealing and other operations are performed according to application requirements, the required particleboard is made.
[0036] Furthermore, the raw material can be conventional wood, including wood particles and shavings produced by crushing poplar, pine, eucalyptus, etc., or wood particles processed from non-wood units such as wheat, rice, flax, bagasse, cotton stalks, and reeds.
[0037] Furthermore, the hot pressing conditions can be adjusted according to actual requirements, for example, the hot pressing temperature is 100-250° C., the hot pressing pressure is 10-300 bar, and the hot pressing time is 5-10 minutes.
[0038] When preparing plywood, the steps may be:
[0039] (1) Apply the adhesive on the surface of the veneer, with the amount of adhesive applied being 90-150 g / m 2 ;
[0040] (2) The veneers with an odd number of glue layers are assembled in such a way that the wood grain directions of the adjacent veneers are perpendicular to each other to obtain slabs, which are then pre-pressed and hot-pressed to obtain formaldehyde-free artificial boards.
[0041] Furthermore, the pre-pressing pressure is 0.8-1.2 MPa, and the pre-pressing time is 20-60 min; the hot pressing temperature is 120-180° C., the hot pressing pressure is 10-300 bar, and the hot pressing time is 20-60 minutes, etc.
[0042] Furthermore, the veneer material is poplar, eucalyptus, pine, birch, basswood, crabapple, magnolia, maple, elm, oak or rubber wood, etc.
[0043] The beneficial effects of the present invention are as follows:
[0044] The present invention provides an adhesive for formaldehyde-free artificial panels, and its preparation and application have the following advantages compared with the prior art:
[0045] 1. The viscosity of the adhesive of the present invention can be freely adjusted according to application requirements, and the adjustment range is 50-80000mPa.s. When preparing plywood, a high-viscosity adhesive formula can be selected; when preparing fiberboard or particleboard, a low-viscosity adhesive formula can be selected, which overcomes the defect of the prior art that the viscosity of formaldehyde-free adhesive is single and cannot be adjusted.
[0046] 2. The adhesive of the present invention does not contain formaldehyde, is safe and environmentally friendly, and meets the current call for environmental safety; at the same time, the adhesive does not need to add flour when preparing plywood, which not only saves flour resources but also improves bonding strength.
[0047] 3. The adhesive of the present invention can replace urea-formaldehyde resin to produce formaldehyde-free artificial boards, has good process suitability, does not require adjustment of existing equipment and processes, and the prepared plywood can meet Class I bonding strength standards, and the prepared particleboard meets the national standard strength requirements. The amount of glue applied is low, and the comprehensive glue cost is about 25% lower than that of urea-formaldehyde resin.
[0048] 4. The adhesive of the present invention has a long active period, which can be up to 72 hours or more, and can still maintain a high bonding strength at the end of the active period. DETAILED DESCRIPTION
[0049] In order to explain the present invention more clearly, the present invention is further described below in conjunction with preferred embodiments. It should be understood by those skilled in the art that the following specific description is illustrative rather than restrictive, and should not be used to limit the scope of protection of the present invention.
[0050] Example 1
[0051] This embodiment prepares an adhesive for formaldehyde-free artificial panels, and the adhesive is composed of the following raw materials in parts by weight:
[0052] 200 parts of viscosity stabilizer, 100 parts of aqueous emulsion, filler: 4 parts of barium sulfate, first curing agent: 15 parts of polymethylene polyphenyl polyisocyanate;
[0053] Wherein, the second curing agent in the viscosity stabilizer is polymethylene polyphenyl polyisocyanate, and the catalyst is stannous octoate;
[0054] The viscosity stabilizer is prepared by the following method:
[0055] 100 parts of polyvinyl alcohol 2499 were dissolved in 900 parts of deionized water, and 0.3 parts of polymethylene polyphenyl polyisocyanate and 0.01 parts of stannous octoate were added, and the mixture was stirred and reacted at 40° C. for 2 hours.
[0056] The aqueous emulsion is prepared by the following method:
[0057] (1) 40 parts of isooctyl acrylate and 60 parts of methyl methacrylate were mixed, and 3 parts of sodium lauryl sulfate and 400 parts of deionized water were added for pre-emulsification to obtain a pre-emulsion;
[0058] (2) Add 0.5 parts of ammonium persulfate to the pre-emulsifier, and then react at 80° C. for 6 hours.
[0059] The viscosity stabilizer, aqueous emulsion and barium sulfate are mixed according to the formula, stirred evenly to obtain the main glue, and then polymethylene polyphenyl polyisocyanate is added to the main glue and stirred until uniform. The obtained performance data is shown in Table 1.
[0060] The adhesive is used to prepare plywood: the veneer with odd number of layers of glue (the amount of glue applied is 125 g / m 2 ) The veneers are assembled in a manner that the wood grain directions of adjacent veneers are perpendicular to each other to obtain slabs. After pre-pressing (60 minutes) and hot pressing (120°C, 35 minutes), formaldehyde-free plywood is obtained. The obtained performance data are shown in Table 2.
[0061] Example 2
[0062] This embodiment prepares an adhesive for formaldehyde-free artificial panels, and the adhesive is composed of the following raw materials in parts by weight:
[0063] 190 parts of viscosity stabilizer, 100 parts of aqueous emulsion, filler: 5 parts of talc, first curing agent: 20 parts of polymethylene polyphenyl polyisocyanate;
[0064] Wherein, the second curing agent in the viscosity stabilizer is polymethylene polyphenyl polyisocyanate, and the catalyst is stannous octoate;
[0065] The viscosity stabilizer is prepared by the following method:
[0066] 100 parts of polyvinyl alcohol 2099 were dissolved in 900 parts of deionized water, and 1 part of polymethylene polyphenyl polyisocyanate and 0.01 part of stannous octoate were added, and the mixture was stirred and reacted at 30° C. for 6 hours.
[0067] The aqueous emulsion is prepared by the following method:
[0068] (1) 45 parts of isooctyl acrylate, 50 parts of methyl methacrylate and 5 parts of acrylic acid are mixed, and 3 parts of sodium lauryl sulfate and 400 parts of deionized water are added for pre-emulsification to obtain a pre-emulsion;
[0069] (2) Add 0.5 parts of ammonium persulfate to the pre-emulsifier, and then react at 80° C. for 6 hours.
[0070] The viscosity stabilizer, aqueous emulsion and talcum powder are mixed according to the formula, stirred evenly to obtain the main adhesive, and then polymethylene polyphenyl polyisocyanate is added to the main adhesive and stirred until uniform. The obtained performance data is shown in Table 1.
[0071] The adhesive is used to prepare plywood: the veneer with odd number of layers of glue (the amount of glue applied is 125 g / m 2) The veneers are assembled in a manner that the wood grain directions of adjacent veneers are perpendicular to each other to obtain slabs. After pre-pressing (60 minutes) and hot pressing (120°C, 35 minutes), formaldehyde-free plywood is obtained. The obtained performance data are shown in Table 2.
[0072] Example 3
[0073] This embodiment prepares an adhesive for formaldehyde-free artificial panels, and the adhesive is composed of the following raw materials in parts by weight:
[0074] 250 parts of viscosity stabilizer, 100 parts of aqueous emulsion, filler: 5 parts of talcum powder, first curing agent: 20 parts of isophorone diisocyanate;
[0075] Wherein, the second curing agent in the viscosity stabilizer is isophorone diisocyanate, and the catalyst is stannous octoate;
[0076] The viscosity stabilizer is prepared by the following method:
[0077] 100 parts of polyvinyl alcohol 1799 were dissolved in 1150 parts of deionized water, 2 parts of isophorone diisocyanate and 0.01 parts of stannous octoate were added, and the mixture was stirred and reacted at 30°C for 6 hours.
[0078] The aqueous emulsion is prepared by the following method:
[0079] (1) 45 parts of isooctyl acrylate, 50 parts of methyl methacrylate and 5 parts of acrylic acid are mixed, and 3 parts of sodium lauryl sulfate and 150 parts of deionized water are added for pre-emulsification to obtain a pre-emulsion;
[0080] (2) Add 0.5 parts of ammonium persulfate to the pre-emulsifier, and then react at 80° C. for 6 hours.
[0081] The viscosity stabilizer, aqueous emulsion and talcum powder are mixed according to the formula, and stirred evenly to obtain the main adhesive. Then, isophorone diisocyanate is added to the main adhesive and stirred until uniform. The obtained performance data is shown in Table 1.
[0082] The adhesive is used to prepare plywood: the veneer with odd number of layers of glue (the amount of glue applied is 125 g / m 2 ) The veneers are assembled in a manner that the wood grain directions of adjacent veneers are perpendicular to each other to obtain slabs. After pre-pressing (60 minutes) and hot pressing (120°C, 35 minutes), formaldehyde-free plywood is obtained. The obtained performance data are shown in Table 2.
[0083] Example 4
[0084] This embodiment prepares an adhesive for formaldehyde-free artificial panels, and the adhesive is composed of the following raw materials in parts by weight:
[0085] 250 parts of viscosity stabilizer, 100 parts of aqueous emulsion, filler: 5 parts of talc, first curing agent: 20 parts of polymethylene polyphenyl polyisocyanate;
[0086] Wherein, the second curing agent in the viscosity stabilizer is polymethylene polyphenyl polyisocyanate, and the catalyst is stannous octoate;
[0087] The viscosity stabilizer is prepared by the following method:
[0088] 100 parts of polyvinyl alcohol 1799 were dissolved in 1150 parts of deionized water, 3 parts of polymethylene polyphenyl polyisocyanate and 0.01 parts of stannous octoate were added, and the mixture was stirred and reacted at 30°C for 6 hours.
[0089] The aqueous emulsion is prepared by the following method:
[0090] (1) 45 parts of isooctyl acrylate, 50 parts of methyl methacrylate and 5 parts of acrylic acid are mixed, and 3 parts of sodium lauryl sulfate and 150 parts of deionized water are added for pre-emulsification to obtain a pre-emulsion;
[0091] (2) Add 0.5 parts of ammonium persulfate to the pre-emulsifier, and then react at 80° C. for 6 hours.
[0092] The viscosity stabilizer, aqueous emulsion and talcum powder are mixed according to the formula, and stirred evenly to obtain the main adhesive. Then, isophorone diisocyanate is added to the main adhesive and stirred until uniform. The obtained performance data is shown in Table 1.
[0093] The adhesive is used to prepare plywood: the veneer with odd number of layers of glue (the amount of glue applied is 125 g / m 2 ) The veneers are assembled in a manner that the wood grain directions of adjacent veneers are perpendicular to each other to obtain slabs. After pre-pressing (60 minutes) and hot pressing (120°C, 35 minutes), formaldehyde-free plywood is obtained. The obtained performance data are shown in Table 2.
[0094] Example 5
[0095] This embodiment prepares an adhesive for formaldehyde-free artificial panels, and the adhesive is composed of the following raw materials in parts by weight:
[0096] 250 parts of viscosity stabilizer, 100 parts of aqueous emulsion, filler: 5 parts of talc, first curing agent: 20 parts of polymethylene polyphenyl polyisocyanate;
[0097] Wherein, the second curing agent in the viscosity stabilizer is polymethylene polyphenyl polyisocyanate, and the catalyst is stannous octoate;
[0098] The viscosity stabilizer is prepared by the following method:
[0099] 100 parts of polyvinyl alcohol 1799 were dissolved in 1150 parts of deionized water, 5 parts of polymethylene polyphenyl polyisocyanate and 0.01 parts of stannous octoate were added, and the mixture was stirred and reacted at 30°C for 6 hours.
[0100] The aqueous emulsion is prepared by the following method:
[0101] (1) 45 parts of isooctyl acrylate, 50 parts of methyl methacrylate and 5 parts of acrylic acid are mixed, and 3 parts of sodium lauryl sulfate and 150 parts of deionized water are added for pre-emulsification to obtain a pre-emulsion;
[0102] (2) Add 0.5 parts of ammonium persulfate to the pre-emulsifier, and then react at 80° C. for 6 hours.
[0103] The viscosity stabilizer, aqueous emulsion and talcum powder are mixed according to the formula, and stirred evenly to obtain the main adhesive. Then, isophorone diisocyanate is added to the main adhesive and stirred until uniform. The obtained performance data is shown in Table 1.
[0104] The adhesive is used to prepare plywood: the veneer with odd number of layers of glue (the amount of glue applied is 125 g / m 2 ) The veneers are assembled in a manner that the wood grain directions of adjacent veneers are perpendicular to each other to obtain slabs. After pre-pressing (60 minutes) and hot pressing (120°C, 35 minutes), formaldehyde-free plywood is obtained. The obtained performance data are shown in Table 2.
[0105] Example 6
[0106] This embodiment prepares an adhesive for formaldehyde-free artificial panels, and the adhesive is composed of the following raw materials in parts by weight:
[0107] 100 parts of viscosity stabilizer, 100 parts of water-based emulsion, filler: 5 parts of heavy calcium, first curing agent: 25 parts of isophorone diisocyanate;
[0108] The second curing agent in the viscosity stabilizer is isophorone diisocyanate, and the catalyst is dibutyltin dilaurate;
[0109] The viscosity stabilizer is prepared by the following method:
[0110] 100 parts of polyvinyl alcohol 0588 were dissolved in 1150 parts of deionized water, 0.1 parts of isophorone diisocyanate and 0.01 parts of dibutyltin dilaurate were added, and the mixture was stirred and reacted at 30° C. for 4 hours.
[0111] The aqueous emulsion is prepared by the following method:
[0112] (1) 40 parts of isooctyl acrylate, 10 parts of vinyl acetate, 45 parts of methyl methacrylate and 5 parts of acrylic acid are mixed, and 3 parts of sodium lauryl sulfate and 150 parts of deionized water are added for pre-emulsification to obtain a pre-emulsion;
[0113] (2) Add 0.8 parts of ammonium persulfate to the pre-emulsifier, and then react at 80° C. for 6 hours.
[0114] The viscosity stabilizer, aqueous emulsion and heavy calcium are mixed according to the formula, stirred evenly to obtain the main glue, and then isophorone diisocyanate is added to the main glue and stirred until it is uniform. The obtained performance data is shown in Table 1.
[0115] The adhesive is used in the preparation of particleboard: the amount of adhesive applied is controlled to be 150kg / m 3 The main glue and the first curing agent are applied to the raw materials by atomizing, and then the raw materials after gluing are mixed and placed in a mold or on a carrier. According to the application requirements, paving, pre-pressing, hot pressing (180°C, 5 minutes), edge sealing and other operations are performed to make formaldehyde-free particleboard. The obtained performance data are shown in Table 3.
[0116] Example 7
[0117] This embodiment prepares an adhesive for formaldehyde-free artificial panels, and the adhesive is composed of the following raw materials in parts by weight:
[0118] 100 parts of viscosity stabilizer, 100 parts of aqueous emulsion, filler: 0.1 parts of talc, first curing agent: 20 parts of polymethylene polyphenyl polyisocyanate;
[0119] The second curing agent in the viscosity stabilizer is polymethylene polyphenyl polyisocyanate, and the catalyst is dibutyltin dilaurate;
[0120] The viscosity stabilizer is prepared by the following method:
[0121] 100 parts of polyvinyl alcohol 0588 were dissolved in 1150 parts of deionized water, and 0.2 parts of polymethylene polyphenyl polyisocyanate and 0.02 parts of dibutyltin dilaurate were added, and the mixture was stirred and reacted at 30° C. for 4 hours.
[0122] The aqueous emulsion is prepared by the following method:
[0123] (1) 25 parts of isooctyl acrylate, 10 parts of vinyl acetate, 10 parts of butyl acrylate, 47 parts of methyl methacrylate and 8 parts of acrylic acid are mixed, and 4 parts of sodium dodecyl sulfate and 240 parts of deionized water are added for pre-emulsification to obtain a pre-emulsion;
[0124] (2) Add 0.8 parts of ammonium persulfate to the pre-emulsifier, and then react at 80° C. for 6 hours.
[0125] The viscosity stabilizer, aqueous emulsion and talcum powder are mixed according to the formula, stirred evenly to obtain the main adhesive, and then polymethylene polyphenyl polyisocyanate is added to the main adhesive and stirred until uniform. The obtained performance data is shown in Table 1.
[0126] The adhesive is used in the preparation of particleboard: the amount of adhesive applied is controlled to be 150kg / m 3 The main glue and the first curing agent are applied to the raw materials by atomizing, and then the raw materials after gluing are mixed and placed in a mold or on a carrier. According to the application requirements, paving, pre-pressing, hot pressing (180°C, 5 minutes), edge sealing and other operations are performed to make formaldehyde-free particleboard. The obtained performance data are shown in Table 3.
[0127] Example 8
[0128] This embodiment prepares an adhesive for formaldehyde-free artificial panels, and the adhesive is composed of the following raw materials in parts by weight:
[0129] 50 parts of viscosity stabilizer, 100 parts of aqueous emulsion, filler: 3 parts of talc, first curing agent: 5 parts of isophorone diisocyanate, 15 parts of polymethylene polyphenyl polyisocyanate;
[0130] The second curing agent in the viscosity stabilizer is isophorone diisocyanate, and the catalyst is dibutyltin dilaurate;
[0131] The viscosity stabilizer is prepared by the following method:
[0132] 100 parts of polyvinyl alcohol 1788 were dissolved in 1550 parts of deionized water, 0.2 parts of isophorone diisocyanate and 0.02 parts of dibutyltin dilaurate were added, and the mixture was stirred and reacted at 30° C. for 4 hours.
[0133] The aqueous emulsion is prepared by the following method:
[0134] (1) 40 parts of isooctyl acrylate, 10 parts of vinyl acetate, 10 parts of butyl acrylate and 40 parts of styrene were mixed, and 5 parts of sodium dodecyl sulfate and 240 parts of deionized water were added for pre-emulsification to obtain a pre-emulsion;
[0135] (2) Add 0.8 parts of ammonium persulfate to the pre-emulsifier, and then react at 80° C. for 6 hours.
[0136] The viscosity stabilizer, aqueous emulsion and talcum powder are mixed according to the formula, and stirred evenly to obtain a main adhesive. Then, isophorone diisocyanate and polymethylene polyphenyl polyisocyanate are added to the main adhesive and stirred until uniform. The obtained performance data is shown in Table 1.
[0137] The adhesive is used in the preparation of particleboard: the amount of adhesive applied is controlled to be 150kg / m 3 The main glue and the first curing agent are applied to the raw materials by atomizing, and then the raw materials after gluing are mixed and placed in a mold or on a carrier. According to the application requirements, paving, pre-pressing, hot pressing (180°C, 5 minutes), edge sealing and other operations are performed to make formaldehyde-free particleboard. The obtained performance data are shown in Table 3.
[0138] Table 1
[0139]
[0140] Table 2
[0141]
[0142] Note: The plywood performance test is carried out in accordance with the standard GB / T 9846-2015 "Ordinary Plywood".
[0143] Table 3
[0144]
[0145] Note: The performance test of particleboard is carried out in accordance with the standard GB / T 4895-2015.
[0146] Obviously, the above embodiments of the present invention are merely examples for clearly illustrating the present invention, and are not limitations on the implementation methods of the present invention. For ordinary technicians in the relevant field, other different forms of changes or modifications can be made based on the above description. It is impossible to list all the implementation methods here. All obvious changes or modifications derived from the technical solution of the present invention are still within the protection scope of the present invention.
Claims
1. An adhesive for formaldehyde-free artificial panels, characterized in that: It is prepared from the following raw materials in parts by weight: 36-375 parts of viscosity stabilizer, 100 parts of aqueous emulsion, 0.1-10 parts of filler and 2-25 parts of first curing agent; The viscosity stabilizer is prepared by the following method: Dissolve 100 parts of polyvinyl alcohol in 255-1550 parts of deionized water, add 0.1-10 parts of the second curing agent and 0.0005-0.05 parts of the catalyst, and stir and react at 30-60°C for 0.5-6 hours to obtain; The first curing agent and the second curing agent include one or more of aromatic polyisocyanate, aliphatic polyisocyanate, aromatic aliphatic polyisocyanate or alicyclic polyisocyanate; The filling does not contain flour.
2. The adhesive according to claim 1, characterized in that: The degree of polymerization of the polyvinyl alcohol is 300-2400, and the degree of alcoholysis is 78-99%.
3. The adhesive according to claim 1, characterized in that: The catalyst includes one or more of N,N-dimethylcyclohexylamine, bismuth cycloalkaneate, bismuth octanoate, bismuth laurate, bismuth isooctanoate, dibutyltin dilaurate, stannous octoate, N,N'-lutidine, N,N-dimethylethanolamine, triethanolamine, N-2-hydroxypropyldimethylmorpholine, N,N'-bis-(α-hydroxypropyl)-2-methylpiperazine, N,N'-diethyl-2-methylpiperazine, N,N'-diethylpiperazine, N-methylmorpholine, N-ethylmorpholine, triethyleneimine, N,N-dimethylbutylamine, N,N-dimethylhexadecylamine, N,N-dimethylbenzylamine, triethylamine, triethylenediamine or N,N-dimethylcyclohexylamine.
4. The adhesive according to claim 1, characterized in that: The aqueous emulsion is prepared by the following method: (1) 40-85 parts of soft monomer and 15-60 parts of hard monomer are mixed, and 2-5 parts of emulsifier and 120-400 parts of deionized water are added for pre-emulsification to obtain a pre-emulsified liquid; (2) Add 0.3-1.0 parts of initiator to the above pre-emulsifier and react at 70-80°C for 3-6 hours to obtain; The soft monomer includes one or more of vinyl acetate, allyl acetate, n-butyl acrylate, isobutyl acrylate, isooctyl acrylate, ethyl acrylate, sec-butyl acrylate, n-propyl acrylate, lauryl acrylate, 2-ethylhexyl acrylate, 2-ethylhexyl methacrylate, lauryl methacrylate, 2-hydroxyethyl acrylate, 2-hydroxypropyl acrylate or vinyl acetate; The hard monomer includes one or more of methyl methacrylate, styrene, ethyl methacrylate, acrylonitrile, acrylic acid, methacrylic acid, acrylamide, N-hydroxymethyl acrylamide, n-butyl methacrylate, isobutyl methacrylate, tert-butyl methacrylate, octadecyl methacrylate, cyclohexyl methacrylate or isobornyl methacrylate; The emulsifier includes one or more of sodium dodecylbenzene sulfonate, sodium dodecyl sulfate, sodium ethoxylated alkyl sulfate, ammonium ethoxylated alkyl sulfate, alkylphenol polyoxyethylene ether formaldehyde condensate, phenylethylphenol polyoxyethylene ether formaldehyde condensate, isopropylphenylphenol polyoxyethylene ether formaldehyde condensate or benzylphenol polyoxyethylene ether formaldehyde condensate; The initiator is ammonium persulfate or potassium persulfate.
5. The adhesive according to claim 1, characterized in that: The filler includes one or more of montmorillonite, talc, bentonite, kaolin, diatomaceous earth, tannin, heavy calcium, barium sulfate or mica powder.
6. The method for preparing the formaldehyde-free adhesive for artificial panels according to any one of claims 1 to 5, characterized in that: The steps include: The viscosity stabilizer, aqueous emulsion and filler are mixed and stirred to obtain the main glue, and then the first curing agent is added and stirred until uniform.
7. A formaldehyde-free artificial board, characterized in that: The formaldehyde-free artificial board contains the adhesive as described in any one of claims 1 to 5 or the adhesive prepared by the preparation method as described in claim 6.
8. The formaldehyde-free artificial board according to claim 7, characterized in that: The formaldehyde-free artificial board includes particle board, fiberboard, blockboard, plywood or structural composite wood.