Electrolyte additives, electrolytes, and lithium-ion batteries

By using electrolyte additives containing S, N heteroatoms and S=O double bonds in lithium-ion batteries, a dense interfacial film is formed, which solves the problem of side reactions in lithium-ion batteries at high temperatures and improves the safety and cycle performance of the batteries.

CN116417666BActive Publication Date: 2026-11-10BYD CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111637928.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-12-29
Publication Date
2026-11-10
Estimated Expiration
2041-12-29

AI Technical Summary

Technical Problem

Existing lithium-ion batteries are prone to side reactions under high temperature conditions, which can cause the batteries to swell, degrade cycle performance, and pose safety hazards.

Method used

Electrolyte additives containing S, N heteroatoms and S=O double bonds are used to form a dense interfacial film, which inhibits the high-temperature reaction between the positive and negative electrode materials and the electrolyte, thereby improving the high-temperature resistance of lithium-ion batteries.

Benefits of technology

It effectively suppresses positive and negative electrode side reactions under high temperature conditions, improves the safety and cycle performance of lithium-ion batteries, and extends their service life.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116417666B_ABST
    Figure CN116417666B_ABST
Patent Text Reader

Abstract

This application provides an electrolyte additive, an electrolyte, and a lithium-ion battery. The electrolyte additive includes S and N heteroatoms and S=O double bonds. The electrolyte additive has the following structural formula shown in chemical formula a: Chemical formula a, wherein R1, R2, R3, and R4 are selected from any one of alkyl, haloalkyl, alkenylalkyl, alkynylalkyl, aryl, haloaryl, alkylaryl, and haloalkylaryl.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application belongs to the field of lithium-ion battery technology, specifically, this application relates to an electrolyte additive, an electrolyte, and a lithium-ion battery. Background Technology

[0002] In recent years, with my country's increasing efforts to promote new energy vehicles, pure electric vehicles, with their green and environmentally friendly characteristics, have become an inevitable trend in the future development of the automotive industry. They will gradually replace traditional fuel-powered buses as the daily transportation tool for ordinary people. As the power source for electric vehicles, the improvement of various performance aspects of lithium-ion batteries has always been a key focus of the industry; therefore, lithium-ion batteries with high energy density, good cycle performance, long service life, and high safety performance have become the current development trend pursued by the industry.

[0003] However, in existing lithium-ion batteries, when the ambient temperature reaches above 60°C, a series of side reactions occur between the electrolyte and the positive and negative electrode materials. As the side reactions intensify, the battery will swell, leading to a decline in the battery's cycle performance and even causing safety issues.

[0004] In view of this, in order to solve the above-mentioned technical problems, it is necessary to develop a high-temperature resistant electrolyte system to improve the safety performance of lithium-ion batteries.

[0005] It is necessary to propose an electrolyte additive to improve the performance of the electrolyte, thereby enhancing the cycle performance of lithium-ion batteries. Summary of the Invention

[0006] One objective of this application is to provide a new technical solution for electrolyte additives, electrolytes, and lithium-ion batteries.

[0007] According to a first aspect of the embodiments of this application, an electrolyte additive is provided, the electrolyte additive comprising S, N heteroatoms and S=O double bonds, and the electrolyte additive having the structural formula shown in the following chemical formula a: Chemical formula a R1, R2, R3 and R4 are selected from any one of alkyl, haloalkyl, alkenylalkyl, alkynylalkyl, aryl, haloaryl, alkylaryl and haloalkylaryl.

[0008] Optionally, the alkyl group is any one of methyl, ethyl, n-propyl, isopropyl, n-butyl, sec-butyl, isobutyl, tert-butyl, n-pentyl, neopentyl, n-hexyl, cyclopropyl, and cyclobutyl.

[0009] Optionally, the alkenyl alkyl group is any one of allyl, olefinic, isobutyl, enylpentyl, and isopentyl.

[0010] Optionally, the alkynyl group is any one of propynyl, butyl, isobutyl, pentyl, and isopentyl.

[0011] Optionally, the haloalkyl group is any one of trifluoromethyl, trifluoroethyl, trifluoropropyl, pentafluoropropyl, trifluorobutyl, and pentafluorobutyl.

[0012] Optionally, the haloalkylaryl group is any one of p-trifluoromethylphenyl, trifluoroethyl, p-fluorophenyl, p-chlorophenyl, o-trifluoromethylphenyl, and p-fluorobenzyl.

[0013] According to a second aspect of the embodiments of this application, an electrolyte is provided, the electrolyte comprising the electrolyte additives as described in the first aspect.

[0014] Optionally, the electrolyte additive has a mass percentage content of 1%-5% in the electrolyte.

[0015] Optionally, the electrolyte additive has a mass percentage content of 1.5%-3% in the electrolyte.

[0016] Optionally, the electrolyte may further include lithium salt, solvent, and film-forming additives.

[0017] Optionally, the lithium salt includes at least one of lithium hexafluorophosphate, lithium difluoroflamimide, lithium difluoromethanesulfonylimide, lithium tetrafluoroborate, lithium hexafluoroarsenate, lithium hexafluoroantimonyate, lithium perchlorate, lithium difluoromethanesulfonylimide, lithium dioxalateborate, lithium difluorooxalateborate, lithium trifluoromethanesulfonate, lithium perfluorobutylsulfonate, lithium di(trifluoromethanesulfonyl)imide, and lithium di(perfluoroethylsulfonyl)imide.

[0018] Optionally, the solvent includes carbonate solvents and / or carboxylic acid ester solvents.

[0019] Optionally, the film-forming additive includes at least one of vinylene carbonate, fluoroethylene carbonate, propylene sulfite, vinyl sulfate, methanedisulfonate, 1,3-propane sulpholone, and tripropylene phosphate.

[0020] Optionally, the film-forming additive has a mass percentage content of 0.5%-3% in the electrolyte.

[0021] According to a third aspect of the embodiments of this application, a lithium-ion battery is provided, the lithium-ion battery comprising the electrolyte as described in the second aspect.

[0022] One technical advantage of the embodiments of this application is that: This application provides an electrolyte additive that can form a relatively dense interface film on both the positive and negative electrode surfaces of the battery. The interface film has good thermal stability and can inhibit the reaction between the electrolyte and the positive and negative electrode materials under high temperature conditions, thereby improving the high temperature resistance of the lithium-ion battery and giving the lithium-ion battery a high safety factor. Detailed Implementation

[0023] It should be noted that, unless otherwise specifically stated, the relative arrangement, numerical expressions, and values ​​of the components and steps described in these embodiments do not limit the scope of this application.

[0024] The following description of at least one exemplary embodiment is merely illustrative and is in no way intended to limit the scope of this application and its application or use.

[0025] Techniques, methods, and equipment known to those skilled in the art may not be discussed in detail, but where appropriate, they should be considered part of the specification.

[0026] In all the examples shown and discussed herein, any specific values ​​should be interpreted as merely exemplary and not as limitations. Therefore, other examples of exemplary embodiments may have different values.

[0027] This application provides an electrolyte additive comprising S and N heteroatoms and an S=O double bond, and having the structural formula shown in chemical formula a: Chemical formula a R1, R2, R3 and R4 are selected from any one of alkyl, haloalkyl, alkenylalkyl, alkynylalkyl, aryl, haloaryl, alkylaryl and haloalkylaryl.

[0028] The electrolyte additive in this embodiment is a tetraazine containing a sulfur-oxygen double bond. This additive contains S and N heteroatoms and an S=O double bond. Both the N and S atoms in this structure contain lone pairs of electrons, possessing a certain electron-donating ability, and can coordinate with lithium ions. Furthermore, due to the close spatial positions of the heteroatoms, a chelating effect can be formed, thereby enhancing the binding ability with lithium ions. During the charging and discharging process of the battery, this electrolyte additive can move closer to the positive and negative electrodes along with the migration of lithium ions. This electrolyte additive can form a relatively dense interfacial film on both the positive and negative electrode surfaces of the battery. This interfacial film has good thermal stability and can inhibit the reaction between the electrolyte and the positive and negative electrode materials under high-temperature conditions, thereby improving the high-temperature resistance of the lithium-ion battery and giving it a high safety factor. Simultaneously, the four nitrogen atoms in the additive structure are respectively connected to carboxylic acid ester functional groups. These carboxylic acid esters can undergo complexation on the positive electrode surface, thereby inhibiting the dissolution of positive electrode metal ions, reducing polarization side reactions in the cell during high-rate charging and discharging, and significantly improving the battery's cycle performance.

[0029] Lithium-ion batteries using electrolytes containing this additive exhibit improved high-temperature performance and cycle performance, and the additive also suppresses gas generation in lithium-ion batteries. This is because the electrolyte additive in this embodiment is dioxydithiotetraazine tetracarboxylic acid ester, which can form a uniform and dense CEI film on the positive electrode surface and a uniform and dense SEI film on the negative electrode surface of the lithium-ion battery. The N and S heteroatoms in this electrolyte additive can significantly improve the thermal stability of the CEI and SEI films, thereby suppressing the occurrence of positive and negative electrode side reactions under high-temperature conditions and ensuring good high-temperature resistance of the lithium-ion battery. Secondly, this additive readily forms substances such as LiS2O3 and lithium alkyl sulfonate in the CEI film formed at the positive electrode. These substances not only protect the positive electrode but also suppress gas generation at the positive electrode. Furthermore, the carboxylic acid ester compounds contained in this additive can undergo complexation on the positive electrode surface, thereby inhibiting the dissolution of positive electrode metal ions and preventing damage to the negative electrode, thus improving the battery's cycle performance. The electrolyte additive in this embodiment is dioxydithiotetraazine tetracarboxylate, which has more nitrogen atoms than triazine, thereby increasing the lithium nitride content in the SEI film and increasing ionic conductivity.

[0030] In one embodiment, the alkyl group is any one of methyl, ethyl, n-propyl, isopropyl, n-butyl, sec-butyl, isobutyl, tert-butyl, n-pentyl, neopentyl, n-hexyl, cyclopropyl, and cyclobutyl.

[0031] In one embodiment, the alkenyl alkyl group is any one of allyl, olefinic, isobutyl, enylpentyl, and isopentyl.

[0032] In one embodiment, the alkynyl group is any one of propynyl, butyl, isobutyl, pentyl, and isopentyl.

[0033] In one embodiment, the haloalkyl group is any one of trifluoromethyl, trifluoroethyl, trifluoropropyl, pentafluoropropyl, trifluorobutyl, and pentafluorobutyl.

[0034] In one embodiment, the haloalkylaryl group is any one of p-trifluoromethylphenyl, trifluoroethyl, p-fluorophenyl, p-chlorophenyl, o-trifluoromethylphenyl, and p-fluorobenzyl.

[0035] This application also provides an electrolyte comprising the electrolyte additives described above.

[0036] The advantages of adding the above-mentioned additives to the lithium-ion battery electrolyte of this application are as follows: The N and S atoms contained in the additives with the aforementioned specific structure both contain lone pairs of electrons, which have a certain electron-donating ability and can coordinate with lithium ions. Furthermore, due to the close spatial positions of the heteroatoms, a chelating effect can be formed, thereby enhancing the binding ability with lithium ions. During the charging and discharging process of the battery, the electrolyte additives can move closer to the positive and negative electrodes of the battery along with the migration of lithium ions, thereby forming a uniform and dense CEI film on the surface of the positive electrode and a uniform and dense SEI film on the surface of the negative electrode of the lithium-ion battery. The N and S heteroatoms in the electrolyte additives can greatly improve the thermal stability of the CEI and SEI films, thereby suppressing the occurrence of positive and negative electrode side reactions under high temperature conditions, ensuring that the lithium-ion battery has good high-temperature resistance, and thus improving the high-temperature cycle performance and high-temperature storage performance of the lithium-ion battery.

[0037] The electrolyte additives mentioned above contain S=O bonds and carboxylic acid esters, which can undergo complexation after the positive electrode film is formed, thereby inhibiting the damage to the negative electrode caused by the dissolution of the positive electrode transition metal, reducing the polarization side reactions in the cell during high-rate charge and discharge, and thus improving the cycle performance of lithium-ion batteries.

[0038] In one embodiment, the electrolyte additive further comprises 1%-5% by mass in the electrolyte.

[0039] In this specific example, the mass percentage content of electrolyte additives in the electrolyte is controlled within the range of 1%-5%. This is because: when the mass percentage content of electrolyte additives in the electrolyte is less than 1%, the film formation effect on the positive and negative electrode surfaces of the battery will be poor; when the mass percentage content of electrolyte additives in the electrolyte is higher than 5%, gas generation will be more serious, which will affect the high-temperature performance of the battery.

[0040] In one embodiment, the electrolyte additive further comprises 1.5%-3% by mass in the electrolyte.

[0041] In one embodiment, the solubility range of the electrolyte additive is 0.3M - 1M.

[0042] In one embodiment, the electrolyte further includes lithium salt, solvent, and film-forming additives.

[0043] In one embodiment, the lithium salt further comprises at least one of lithium hexafluorophosphate, lithium difluoroflamimide, lithium bis(trifluoromethanesulfonyl)imide, lithium tetrafluoroborate, lithium hexafluoroarsenate, lithium hexafluoroantimonyate, lithium perchlorate, lithium bis(trifluoromethanesulfonyl)imide, lithium dioxalateborate, lithium difluorooxalateborate, lithium trifluoromethanesulfonate, lithium perfluorobutylsulfonate, lithium bis(trifluoromethanesulfonyl)imide, and lithium bis(perfluoroethylsulfonyl)imide.

[0044] In one embodiment, the solvent further includes carbonate solvents and / or carboxylic acid ester solvents.

[0045] In one embodiment, the film-forming additive further includes at least one of vinylene carbonate, fluoroethylene carbonate, propylene sulfite, vinyl sulfate, methanedisulfonate, 1,3-propane sulpholone, and tripropylene phosphate.

[0046] In one embodiment, the film-forming additive has a mass percentage content of 0.5%-3% in the electrolyte.

[0047] In this specific example, the mass percentage content of the film-forming additive in the electrolyte is controlled within the range of 0.5%-3%. This is because: when the mass percentage content of the film-forming additive in the electrolyte is less than 0.5%, the film-forming effect is poor; when the mass percentage content of the film-forming additive in the electrolyte is greater than 3%, it will lead to an increase in the interfacial impedance of the battery during cycling.

[0048] In one embodiment, the concentration of lithium salt in the electrolyte is further 0.1 mol / L-5 mol / L, and further, the concentration of lithium salt in the electrolyte is 1 mol / L-1.5 mol / L.

[0049] In this specific example, the concentration of lithium salt in the electrolyte is controlled at 0.1 mol / L-5 mol / L. This is because: when the concentration of lithium salt in the electrolyte is below 0.1 mol / L, there are fewer charge carriers in the electrolyte; when the concentration of lithium salt in the electrolyte is above 5 mol / L, lithium salt is more likely to be deposited.

[0050] This application embodiment provides another lithium-ion battery, which includes the electrolyte as described above.

[0051] The present application will be further illustrated below through specific embodiments and comparative examples: Example 1 S101. Dissolve 5.6g of triethylamine with a concentration of 0.04mol / L in 300mL of dry diethyl ether to form the first solution; S102. Dissolve 0.02 mol of 1,2-diethylhydrazine dicarboxylate and 1.7 mL of 0.02 mol / L sulfoxide chloride in 700 mL of dry diethyl ether to form a second solution. Add the first solution dropwise to the second solution and stir for 3.5 hours. Then evaporate the solvent under reduced pressure until dry. Crystallize the obtained residue with methanol to obtain tetraethyl dioxydithiotetraazine tetracarboxylate electrolyte additive, the chemical structural formula of which is: ; S103. Mix 40 mL of ethylene carbonate (EC) and 60 mL of methyl ethyl carbonate (EMC) evenly to form a mixed solvent. Then, dissolve 7.6 g of lithium hexafluorophosphate (LiPF6) and 9.35 g of lithium difluorosulfonyl imide (LiFSI) in the above mixed solvent and stir evenly. Then, add tetraethyl dioxydithiotetraazine tetracarboxylate electrolyte additive to prepare the electrolyte. The molar concentration of LiPF6 and LiFSI is 0.5 mol / L, and the mass percentage content of the electrolyte additive is 2%.

[0052] Example 2 S101. Dissolve 5.6g of triethylamine with a concentration of 0.04mol / L in 300mL of dry diethyl ether to form the first solution; S102. Dissolve 0.02 mol of 1,2-diisopropylhydrazine dicarboxylate and 1.7 mL of 0.02 mol / L sulfoxide chloride in 700 mL of dry diethyl ether to form a second solution. Add the first solution dropwise to the second solution and stir for 3.5 hours. Then evaporate the solvent under reduced pressure until dry. Crystallize the obtained residue with methanol to obtain dioxydithiotetraazine tetracarboxylate tetraisopropyl ester electrolyte additive, whose chemical structural formula is: ; S103. Mix 40 mL of ethylene carbonate (EC) and 60 mL of methyl ethyl carbonate (EMC) evenly to form a mixed solvent. Then, dissolve 7.6 g of lithium hexafluorophosphate (LiPF6) and 9.35 g of lithium difluorosulfonyl imide (LiFSI) in the above mixed solvent and stir evenly. Then, add tetraethyl dioxydithiotetraazine tetracarboxylate electrolyte additive to prepare the electrolyte. The molar concentration of LiPF6 and LiFSI is 0.5 mol / L, and the mass percentage content of the electrolyte additive is 2%.

[0053] Example 3 S101. Dissolve 5.6g of triethylamine with a concentration of 0.04mol / L in 300mL of dry diethyl ether to form the first solution; S102. Dissolve 0.02 mol of 1,2-di-tert-butylhydrazine dicarboxylate and 1.7 mL of 0.02 mol / L sulfoxide chloride in 700 mL of dry diethyl ether to form a second solution. Add the first solution dropwise to the second solution and stir for 3.5 hours. Then evaporate the solvent under reduced pressure until dry. Crystallize the obtained residue with methanol to obtain dioxydithiotetraazine tetracarboxylate tetratert-butyl ester electrolyte additive, whose chemical structural formula is: ; S103. Mix 40 mL of ethylene carbonate (EC) and 60 mL of methyl ethyl carbonate (EMC) evenly to form a mixed solvent. Then, dissolve 7.6 g of lithium hexafluorophosphate (LiPF6) and 9.35 g of lithium difluorosulfonyl imide (LiFSI) in the above mixed solvent and stir evenly. Then, add tetraethyl dioxydithiotetraazine tetracarboxylate electrolyte additive to prepare the electrolyte. The molar concentration of LiPF6 and LiFSI is 0.5 mol / L, and the mass percentage content of the electrolyte additive is 2%.

[0054] Example 4 S101. Dissolve 5.6g of triethylamine with a concentration of 0.04mol / L in 300mL of dry diethyl ether to form the first solution; S102. Dissolve 0.02 mol of 1,2-trifluoroethylhydrazine dicarboxylate and 1.7 mL of 0.02 mol / L sulfoxide chloride in 700 mL of dry diethyl ether to form a second solution. Add the first solution dropwise to the second solution and stir for 3.5 hours. Then evaporate the solvent under reduced pressure until dry. Crystallize the obtained residue with methanol to obtain dioxydithiotetraazine tetracarboxylate tetra(trifluoroethyl) ester electrolyte additive, whose chemical structural formula is: ; S103. Mix 40 mL of ethylene carbonate (EC) and 60 mL of methyl ethyl carbonate (EMC) evenly to form a mixed solvent. Then, dissolve 7.6 g of lithium hexafluorophosphate (LiPF6) and 9.35 g of lithium difluorosulfonyl imide (LiFSI) in the above mixed solvent and stir evenly. Then, add tetraethyl dioxydithiotetraazine tetracarboxylate electrolyte additive to prepare the electrolyte. The molar concentration of LiPF6 and LiFSI is 0.5 mol / L, and the mass percentage content of the electrolyte additive is 2%.

[0055] Example 5 S101. Dissolve 5.6g of triethylamine with a concentration of 0.04mol / L in 300mL of dry diethyl ether to form the first solution; S102. Dissolve 0.02 mol of 1,2-diallylhydrazine dicarboxylate and 1.7 mL of 0.02 mol / L sulfoxide chloride in 700 mL of dry diethyl ether to form a second solution. Add the first solution dropwise to the second solution and stir for 3.5 hours. Then evaporate the solvent under reduced pressure until dry. Crystallize the obtained residue with methanol to obtain dioxydithiotetraazine tetracarboxylate tetra(allyl) ester electrolyte additive, whose chemical structural formula is: ; S103. Mix 40 mL of ethylene carbonate (EC) and 60 mL of methyl ethyl carbonate (EMC) evenly to form a mixed solvent. Then, dissolve 7.6 g of lithium hexafluorophosphate (LiPF6) and 9.35 g of lithium difluorosulfonyl imide (LiFSI) in the above mixed solvent and stir evenly. Then, add tetraethyl dioxydithiotetraazine tetracarboxylate electrolyte additive to prepare the electrolyte. The molar concentration of LiPF6 and LiFSI is 0.5 mol / L, and the mass percentage content of the electrolyte additive is 2%.

[0056] Example 6 S101. Dissolve 5.6g of triethylamine with a concentration of 0.04mol / L in 300mL of dry diethyl ether to form the first solution; S102. Dissolve 0.02 mol of 1,2-diphenylhydrazine dicarboxylate and 1.7 mL of 0.02 mol / L sulfoxide chloride in 700 mL of dry diethyl ether to form a second solution. Add the first solution dropwise to the second solution and stir for 3.5 hours. Then evaporate the solvent under reduced pressure until dry. Crystallize the residue with methanol to obtain dioxydithiotetraazine tetracarboxylate electrolyte additive, the chemical structural formula of which is: ; S103. Mix 40 mL of ethylene carbonate (EC) and 60 mL of methyl ethyl carbonate (EMC) evenly to form a mixed solvent. Then, dissolve 7.6 g of lithium hexafluorophosphate (LiPF6) and 9.35 g of lithium difluorosulfonyl imide (LiFSI) in the above mixed solvent and stir evenly. Then, add tetraethyl dioxydithiotetraazine tetracarboxylate electrolyte additive to prepare the electrolyte. The molar concentration of LiPF6 and LiFSI is 0.5 mol / L, and the mass percentage content of the electrolyte additive is 1.5%.

[0057] Example 7 S101. Dissolve 5.6g of triethylamine with a concentration of 0.04mol / L in 300mL of dry diethyl ether to form the first solution; S102. Dissolve 0.02 mol of 1,2-di-p-fluorophenylhydrazine dicarboxylate and 1.7 mL of 0.02 mol / L sulfoxide chloride in 700 mL of dry diethyl ether to form a second solution. Add the first solution dropwise to the second solution and stir for 3.5 hours. Then evaporate the solvent under reduced pressure until dry. Crystallize the obtained residue with methanol to obtain dioxydithiotetraazine tetracarboxylate tetra(p-fluorophenyl) ester electrolyte additive, whose chemical structural formula is: ; S103. Mix 40 mL of ethylene carbonate (EC) and 60 mL of methyl ethyl carbonate (EMC) evenly to form a mixed solvent. Then, dissolve 7.6 g of lithium hexafluorophosphate (LiPF6) and 9.35 g of lithium difluorosulfonyl imide (LiFSI) in the above mixed solvent and stir evenly. Then, add tetraethyl dioxydithiotetraazine tetracarboxylate electrolyte additive to prepare the electrolyte. The molar concentration of LiPF6 and LiFSI is 0.5 mol / L, and the mass percentage content of the electrolyte additive is 3%.

[0058] Example 8 S101. Dissolve 5.6g of triethylamine with a concentration of 0.04mol / L in 300mL of dry diethyl ether to form the first solution; S102. Dissolve 0.02 mol of 1,2-diethylhydrazine dicarboxylate and 1.7 mL of 0.02 mol / L sulfoxide chloride in 700 mL of dry diethyl ether to form a second solution. Add the first solution dropwise to the second solution and stir for 3.5 hours. Then evaporate the solvent under reduced pressure until dry. Crystallize the obtained residue with methanol to obtain tetraethyl dioxydithiotetraazine tetracarboxylate electrolyte additive, whose chemical structural formula is: ; S103. Mix 40 mL of ethylene carbonate (EC) and 60 mL of methyl ethyl carbonate (EMC) evenly to form a mixed solvent. Then, dissolve 7.6 g of lithium hexafluorophosphate (LiPF6) and 9.35 g of lithium difluorosulfonyl imide (LiFSI) in the above mixed solvent and stir evenly. Then, add tetraethyl dioxydithiotetraazine tetracarboxylate electrolyte additive to prepare the electrolyte. The molar concentration of LiPF6 and LiFSI is 0.5 mol / L, and the mass percentage content of the electrolyte additive is 1%.

[0059] Example 9 S101. Dissolve 5.6g of triethylamine with a concentration of 0.04mol / L in 300mL of dry diethyl ether to form the first solution; S102. Dissolve 0.02 mol of 1,2-diethylhydrazine dicarboxylate and 1.7 mL of 0.02 mol / L sulfoxide chloride in 700 mL of dry diethyl ether to form a second solution. Add the first solution dropwise to the second solution and stir for 3.5 hours. Then evaporate the solvent under reduced pressure until dry. Crystallize the obtained residue with methanol to obtain tetraethyl dioxydithiotetraazine tetracarboxylate electrolyte additive, whose chemical structural formula is: ; S103. Mix 40 mL of ethylene carbonate (EC) and 60 mL of methyl ethyl carbonate (EMC) evenly to form a mixed solvent. Then, dissolve 7.6 g of lithium hexafluorophosphate (LiPF6) and 9.35 g of lithium difluorosulfonyl imide (LiFSI) in the above mixed solvent and stir evenly. Then, add tetraethyl dioxydithiotetraazine tetracarboxylate electrolyte additive to prepare the electrolyte. The molar concentration of LiPF6 and LiFSI is 0.5 mol / L, and the mass percentage content of the electrolyte additive is 4%.

[0060] Comparative Example 1 40 mL of ethylene carbonate (EC) and 60 mL of methyl ethyl carbonate (EMC) were mixed evenly to form a mixed solvent. Then, 7.6 g of lithium hexafluorophosphate (LiPF6) and 9.35 g of lithium difluorosulfonyl imide (LiFSI) were dissolved in the above mixed solvent and stirred evenly. The molar concentration of LiPF6 and LiFSI was 0.5 mol / L.

[0061] Comparative Example 2 40 mL of ethylene carbonate (EC) and 60 mL of ethyl methyl carbonate (EMC) were mixed evenly to form a mixed solvent. Then, 7.6 g of lithium hexafluorophosphate (LiPF6) and 9.35 g of lithium bisfluorosulfonyl imide (LiFSI) were dissolved in the above mixed solvent and stirred evenly. Finally, ethylene carbonate (VC) was added to prepare the electrolyte. The molar concentrations of LiPF6 and LiFSI were both 0.5 mol / L, and the mass percentage content of VC was 2%.

[0062] Comparative Example 3 40 mL of ethylene carbonate (EC) and 60 mL of ethyl methyl carbonate (EMC) were mixed evenly to form a mixed solvent. Then, 7.6 g of lithium hexafluorophosphate (LiPF6) and 9.35 g of lithium bisfluorosulfonyl imide (LiFSI) were dissolved in the above mixed solvent and stirred evenly. Finally, ethylene difluorocarbonate (DFEC) was added to prepare the electrolyte. The molar concentrations of LiPF6 and LiFSI were both 0.5 mol / L, and the mass percentage content of DFEC was 2%.

[0063] Comparative Example 4 Compared with Example 1, the difference is that the mass percentage content of the electrolyte additive is 0.5%, while the other conditions are the same.

[0064] Comparative Example 5 Compared with Example 1, the difference is that the electrolyte additive has a mass percentage content of 5.5%, while the other conditions are the same.

[0065] Lithium-ion batteries were prepared using the electrolytes obtained in Examples 1-9 and Comparative Examples 1-5, respectively. The lithium-ion batteries prepared in Examples 1-9 were numbered S1, S2, S3, S4, S5, S6, S7, S8, and S9, respectively, and the lithium-ion batteries prepared in Comparative Examples 1-5 were numbered RS1, RS2, RS3, RS4, and RS5, respectively. Performance tests were performed on the above lithium-ion batteries. The specific test items and results are as follows: 1) Morphological characteristics After disassembling the lithium-ion battery S4, the battery electrodes were taken for morphological characterization. The surface of the negative electrode of the battery has a waxy deposited layer, which is the SEI film on the surface of the negative electrode; and the surface of the positive electrode of the battery has a dense accumulation of particles, which is the CEI film on the surface of the positive electrode.

[0066] The elemental analysis of the electrode of battery S4 was performed by scanning electron microscopy energy dispersive spectroscopy. The results are shown in Table 1 below. Table 1 is the elemental composition of the SEI film on the negative electrode surface of battery S4, where Wt% is the mass percentage and At% is the atomic percentage.

[0067] Table 1

[0068] As can be seen from Table 1, the SEI film on the negative electrode surface of battery S4 contains N and S elements from the electrolyte additive, which indicates that the electrolyte additive of this application can participate in the formation of the interface film on the surface of the battery electrode.

[0069] (2) High-temperature cycling performance test and high-temperature storage performance test High-temperature cycling performance tests were conducted on batteries S1-S9 and RS1-RS5. The specific test conditions were as follows: the domestic Blue Electric CT2001C test cabinet was used for testing. The batteries were cycled 500 times at 1000mA (1C) current between 2.75V and 4.35V at 60℃. The initial discharge capacity was recorded. After 500 charge-discharge cycles, the discharge capacity of the 500th cycle was recorded. The capacity retention rate of the batteries after high-temperature cycling was calculated using the formula: Capacity retention rate (%) = Discharge capacity after 500 cycles / Initial discharge capacity × 100%. Ten sets of batteries were set up for each example and comparative example. The average value of the test results was taken. The results of the high-temperature cycling performance tests of batteries S1-S9 and RS1-RS5 are shown in Table 2 below.

[0070] High-temperature storage performance tests were conducted on batteries S1-S9 and RS1-RS5. The specific test conditions were as follows: the batteries were fully charged at 1000mA (1C), maintained at a constant voltage of 4.35V to 50mA (0.05C), and then stored in a 60℃ constant temperature chamber for 28 days. The capacity retention rate of the batteries after high-temperature storage was calculated using the formula: Capacity retention rate (%) = Discharge capacity after 28 days of storage / Initial discharge capacity × 100%. Ten sets of batteries were used for each example and comparative example, and the average value of the test results was taken. The test results of the high-temperature storage performance of batteries S1-S9 and RS1-RS5 are shown in Table 2 below.

[0071] Table 2

[0072] As shown in Table 2, the addition of the electrolyte additive provided in this application to the battery electrolyte can significantly improve the high-temperature cycle performance of the battery. Table 2 also shows that the electrolyte additive dioxydithiotetraazine tetracarboxylate tetra(trifluoroethyl) ester (corresponding to battery S4) has better characteristics in improving the high-temperature cycle performance of the battery compared to other dioxydithiotetraazine tetracarboxylate esters; while Comparative Examples 1-3, due to the use of conventional additives, experienced faster capacity decay under high-temperature conditions. The capacity retention rate of the battery after 28 days of high-temperature storage is basically consistent with the high-temperature cycle capacity retention rate, indicating that the electrolyte additive of this application can effectively improve the high-temperature resistance of the battery.

[0073] (3) Nickel leaching test Batteries S1-S9 and RS1-RS5 were disassembled after 500 cycles at 45°C. The positive electrode material, negative electrode material, separator, and aluminum-plastic film of the batteries were repeatedly rinsed with 10 mL of dichloromethane. The rinsing solution was then tested using an inductively coupled plasma optical emission spectrometer (ICP-OES). The instrument used was a Thermo Fisher Scientific ICP-OES instrument, and the testing conditions were those familiar to most testers. Ten sets of batteries were used for each example and comparative example, and the test results were averaged. The test results are shown in Table 3 below.

[0074] Table 3

[0075] As shown in Table 3, the addition of the electrolyte additive provided in this application, with a mass percentage content of 1.5%-3% (S1-S7), significantly inhibited the dissolution of transition metal ions at the positive electrode compared to the absence of additives and the addition of conventional additives (RS1-RS3). Furthermore, when the mass percentage content of the electrolyte additive exceeded the 1.5%-3% range (S8, S9), the inhibitory effect on the dissolution of transition metal ions decreased; and when the mass percentage content of the electrolyte additive further exceeded the 1%-5% range (RS4, RS5), the inhibitory effect on the dissolution of transition metal ions further decreased. Among these, dioxydithiotetraazine tetracarboxylate tetra(trifluoroethyl) ester (S4) exhibited a better inhibitory effect on the dissolution of transition metal ions compared to other dioxydithiotetraazine tetracarboxylate esters.

[0076] While specific embodiments of this application have been described in detail by way of examples, those skilled in the art should understand that the above examples are for illustrative purposes only and are not intended to limit the scope of this application. Those skilled in the art should understand that modifications can be made to the above embodiments without departing from the scope and spirit of this application. The scope of this application is defined by the appended claims.

Claims

1. An electrolyte, characterized in that, The electrolyte includes an electrolyte additive, which comprises S and N heteroatoms and S=O double bonds, and the electrolyte additive has the structural formula shown in chemical formula a: Chemical formula a R1, R2, R3 and R4 are selected from any one of alkyl, haloalkyl, alkenylalkyl, alkynylalkyl, aryl, haloaryl, alkylaryl and haloalkylaryl.

2. The electrolyte according to claim 1, characterized in that, The alkyl group is any one of methyl, ethyl, n-propyl, isopropyl, n-butyl, sec-butyl, isobutyl, tert-butyl, n-pentyl, neopentyl, n-hexyl, cyclopropyl, and cyclobutyl.

3. The electrolyte according to claim 1, characterized in that, The alkenyl alkyl group is any one of allyl, olefin, isobutyl, pentyl, and isopentyl.

4. The electrolyte according to claim 1, characterized in that, The alkynyl group is any one of propynyl, butyl, isobutyl, pentyl, and isopentyl.

5. The electrolyte according to claim 1, characterized in that, The alkyl halogroup is any one of trifluoromethyl, trifluoroethyl, trifluoropropyl, pentafluoropropyl, trifluorobutyl, and pentafluorobutyl.

6. The electrolyte according to claim 1, characterized in that, The haloalkylaryl group is any one of p-trifluoromethylphenyl, trifluoroethyl, p-fluorophenyl, p-chlorophenyl, o-trifluoromethylphenyl, and p-fluorobenzyl.

7. The electrolyte according to claim 1, characterized in that, The electrolyte additive has a mass percentage content of 1%-5% in the electrolyte.

8. The electrolyte according to claim 7, characterized in that, The electrolyte additive has a mass percentage content of 1.5%-3% in the electrolyte.

9. The electrolyte according to claim 1, characterized in that, The electrolyte also includes lithium salt, solvent, and film-forming additives.

10. The electrolyte according to claim 9, characterized in that, The lithium salt includes at least one of lithium hexafluorophosphate, lithium difluoroflamimide, lithium bis(trifluoromethanesulfonyl)imide, lithium tetrafluoroborate, lithium hexafluoroarsenate, lithium hexafluoroantimonyate, lithium perchlorate, lithium bis(trifluoromethanesulfonyl)imide, lithium dioxalateborate, lithium difluorooxalateborate, lithium trifluoromethanesulfonate, lithium perfluorobutylsulfonate, lithium di(trifluoromethanesulfonyl)imide, and lithium di(perfluoroethylsulfonyl)imide; the solvent includes carbonate solvents and / or carboxylic acid ester solvents.

11. The electrolyte according to claim 9, characterized in that, The film-forming additive includes at least one of vinylene carbonate, fluoroethylene carbonate, propylene sulfite, vinyl sulfate, methanedisulfonate, 1,3-propane sulpholone, and tripropylene phosphate. The film-forming additive has a mass percentage content of 0.5%-3% in the electrolyte.

12. A lithium-ion battery, characterized in that, The lithium-ion battery includes the electrolyte as described in any one of claims 1-11.