Method for preparing low carbon cement clinker by treating phosphogypsum with dry kiln
By using conventional raw materials in the new dry kiln to reduce, decompose and desulfurize the phosphogypsum in the rotary kiln, the melting crust problem caused by desulfurization of phosphogypsum in the new dry kiln is solved, and high-efficiency desulfurization and high-strength low-carb cement are achieved The preparation of clinker has improved the resource utilization rate of phosphogypsum.
Patent Information
- Application Number
- CN202310339893.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-29
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2043-03-29
AI Technical Summary
Desulfurization of phosphogypsum in the decomposition furnace of the existing new dry kiln will lead to melt crust problems and it is difficult to achieve a high desulfurization rate, which will affect the resource utilization of phosphogypsum and the strength of cement clinker.
Using low-cost conventional raw materials, in the new dry kiln production line in the existing cement factory, the phosphogypsum after drying, crushing and grinding is mixed with silicon-aluminum-ferrous raw materials, and is carried out in the rotary kiln under a reducing atmosphere. The desulfurization of CaSO4 and the calcination of clinker are controlled to control the calcination temperature between 1150-1300℃ to prepare low-carbohydrate cement clinker to ensure that the sum of C2S and low-calcium mineral C3S2 content is ≥50%, and the SO3 content is ≤1%.
The high-efficiency desulfurization of phosphogypsum is achieved, with a desulfurization rate of more than 99%, avoiding the problem of melt crust, improving the utilization rate of phosphogypsum, and reducing the calcination temperature. The low-carb cement clinker produced has higher strength and stability sex.
Smart Images

Figure CN116462426B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of building materials, and in particular relates to a method for preparing low-carbon cement clinker by utilizing phosphogypsum. Background Art
[0002] Phosphogypsum is a solid waste produced in the wet phosphoric acid process. The composition of phosphogypsum is relatively complex. In addition to hydrated calcium sulfate, there are also incompletely decomposed phosphate ore, residual phosphoric acid, fluoride, acid insoluble matter, organic matter, etc. Among them, the presence of fluorine and organic matter has the greatest impact on the resource utilization of phosphogypsum. Stacking will occupy a large amount of land and cause pollution to water and land resources. According to statistics from the China Phosphate Fertilizer Industry Association, the total annual emission of phosphogypsum in 2020 was about 75-80 million tons. Although many industries have tried to use phosphogypsum, the utilization rate is low. The domestic stockpile has reached more than 600 million tons, and the world has reached more than 6 billion tons. The resource utilization and safe and efficient utilization of phosphogypsum are of great significance to solving the environmental pollution and resource waste caused by stacking treatment.
[0003] Using phosphogypsum instead of limestone as a source of CaO to produce cement clinker is a challenging and meaningful direction to solve the resource utilization of phosphogypsum. CaO in the clinker can be provided by phosphogypsum, which can improve the utilization rate of solid waste phosphogypsum and reduce the mining of natural limestone mines. Both active admixtures and clinkers have strict requirements on the SO3 content, but CaSO4 requires a higher temperature to completely decompose and desulfurize compared to CaCO3, which will increase the difficulty and cost of the process operation. It can even still exist in large quantities under high-temperature calcination, which undoubtedly restricts the difficulty of applying phosphogypsum.
[0004] In 1969, the Austrian Linz Company completed and put into operation a plant for producing cement from phosphogypsum and sulfuric acid. In the 1980s, my country also built 7 sets of equipment. The main method is to dry and dehydrate the phosphogypsum, mix it with coke, clay, sandstone, etc. according to the clinker ratio, and calcine it in a hollow rotary kiln to produce clinker. The SO2 in the kiln gas is converted and absorbed to produce sulfuric acid. However, the strength of cement produced from phosphogypsum is generally low, and it even fails to reach the strength grade of 42.5 ordinary Portland cement. At present, most of the co-production units have been shut down.
[0005] There have been many literature reports on the research on the decomposition of phosphogypsum using carbonaceous raw materials, carbon monoxide atmosphere, elemental sulfur, etc., but it is difficult to achieve a desulfurization rate of more than 95% for phosphogypsum by relying solely on the reduction of carbon and sulfur. If the desulfurization rate does not meet this requirement, it will have many adverse effects on the production and application of clinker.
[0006] The applicant has made a breakthrough in the decomposition and desulfurization of phosphogypsum in recent research and applied for an invention patent for "a process for desulfurization of phosphogypsum and co-production of cement". The method mainly adopts a mixed desulfurization method with low KH value ingredients, with a KH value of 0.6-0.7, so that the desulfurization rate reaches more than 95%. The SO3 content in the obtained silicate cement clinker does not exceed 3%, but it is very difficult to continue to reduce the SO3 content to below 1%.
[0007] Secondly, the KH value required for preparing conventional cement clinker is relatively high. If a lower KH value is used for desulfurization, the utilization rate of phosphogypsum will be reduced. Furthermore, since the temperature for the best desulfurization effect of phosphogypsum is above 1100°C, desulfurization of phosphogypsum in the decomposition furnace of the new dry kiln will lead to problems such as melt crusting.
[0008] How to use low-cost conventional raw materials, without increasing the cost of equipment transformation, and utilize the new dry kiln production line in the existing cement plant to process phosphogypsum, solve the problem of molten crust caused by desulfurization of phosphogypsum in the decomposition furnace of the existing new dry kiln, and achieve better desulfurization effect of phosphogypsum, has become a technical problem that needs to be solved urgently. Summary of the invention
[0009] The purpose of the present invention is to provide a method for treating phosphogypsum and preparing low-carbon cement clinker by using a new dry kiln, using low-cost conventional raw materials, without increasing the cost of equipment modification, and using the new dry kiln production line in an existing cement plant to treat phosphogypsum, thereby solving the problem of molten crusting caused by desulfurization of phosphogypsum in a decomposition furnace of an existing new dry kiln, and achieving a better desulfurization effect for phosphogypsum, and producing low-carbon cement clinker with a sum of the contents of C2S and low-calcium mineral C3S2 ≥50%.
[0010] In order to achieve the above purpose, the technical solutions adopted are as follows:
[0011] A method for treating phosphogypsum and preparing low-carbon cement clinker using a dry kiln comprises the following steps:
[0012] (1) obtaining phosphogypsum, drying, crushing, grinding, and mixing with silicon-aluminum-iron raw materials and grinding;
[0013] (2) the obtained mixed material is preheated in a preheater and a decomposition furnace;
[0014] (3) The preheated mixture directly enters the rotary kiln for desulfurization of CaSO4 and calcination of clinker under a reducing atmosphere, and low-carbon cement clinker is obtained after cooling.
[0015] According to the above scheme, the silicon-aluminum-iron raw material in step (1) is one or more of sandstone, coal gangue, silica, clay, fly ash, and various types of waste residues.
[0016] According to the above scheme, the ingredients in step (1) are KH=0.4-0.5 and SM=2-7.
[0017] In the optimized solution, the ingredients in step (1) are KH=0.4-0.5 and SM=4-7.
[0018] According to the above scheme, the reducing atmosphere in step (3) is controlled by incomplete combustion of the carbonaceous raw material so that the volume concentration of CO in the rotary kiln is 2%-10%.
[0019] According to the above scheme, the calcination temperature of the rotary kiln in step (3) is 1150-1300°C.
[0020] In the optimized solution, the calcination temperature of the rotary kiln in step (3) is 1200-1250°C.
[0021] According to the above scheme, the sum of the contents of C2S and low-calcium mineral C3S2 in the mineral composition of the low-carbon cement clinker obtained in step (3) is ≥50%, and the content of SO3 in the clinker is ≤1%.
[0022] Compared with the prior art, the present invention has the following beneficial effects:
[0023] The present invention does not need to increase the cost of equipment modification. It utilizes the new dry kiln in the existing cement plant to process phosphogypsum, transfers the reduction decomposition and desulfurization of the phosphogypsum to the rotary kiln, and prepares low-carbon cement clinker that can also be obtained under a reducing atmosphere, thereby solving the problem that the desulfurization of phosphogypsum in the decomposition furnace of the existing new dry kiln will cause melt crusting.
[0024] A large amount of phosphogypsum can be processed, and the utilization rate of phosphogypsum in the ingredients is above 80%.
[0025] The calcination temperature is lower than that of silicate cement clinker, and the obtained calcination product is low-carbon cement clinker, the sum of the contents of C2S and low-calcium mineral C3S2 of which is ≥50%.
[0026] The raw materials used are all low-priced conventional raw materials in cement clinker production and can be obtained locally. After scientific formulation, the desulfurization effect of phosphogypsum is good and stable, the desulfurization rate reaches more than 99%, and the SO3 content in the calcined product is ≤1%. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 : XRD pattern of the calcined product of Example 1. DETAILED DESCRIPTION
[0028] The following examples further illustrate the technical solution of the present invention, but are not intended to limit the scope of protection of the present invention.
[0029] A specific embodiment provides a method for treating phosphogypsum and preparing low-carbon cement clinker using a dry kiln, comprising the following steps:
[0030] (1) obtaining phosphogypsum, drying, crushing, grinding, and mixing with silicon-aluminum-iron raw materials and grinding;
[0031] (2) The obtained mixture is preheated by a preheater and a decomposition furnace; the decomposition furnace here only serves to further preheat the mixture;
[0032] (3) The preheated mixture enters the rotary kiln for desulfurization of CaSO4 and calcination of clinker under a reducing atmosphere, and low-carbon cement clinker is obtained after cooling.
[0033] Specifically, the ferroaluminum-silicon raw material in step (1) is one or more of sandstone, coal gangue, silica, clay, fly ash, and various waste residues. The raw materials of the present invention are all low-priced conventional raw materials in cement clinker production, which can be obtained locally. After scientific formulation, the desulfurization effect of phosphogypsum is good and stable, the desulfurization rate reaches more than 99%, and the content of SO3 in the calcined product is ≤1%.
[0034] Specifically, in step (1), KH=0.4-0.5 and SM=2-7 are used as the ingredients. In the optimized solution, SM=4-7 is used, and a higher SM value can ensure a higher and more stable desulfurization rate.
[0035] Specifically, the reducing atmosphere in step (3) is controlled by incomplete combustion of the carbonaceous raw material so that the volume concentration of CO in the rotary kiln is 2%-10%.
[0036] Specifically, the carbonaceous raw material is one or more of ordinary coal, high-sulfur coal, and coke.
[0037] Specifically, the calcination temperature of the rotary kiln in step (3) is 1150-1300° C. The optimized calcination temperature is 1200-1250° C.
[0038] Specifically, the sum of the contents of C2S and low-calcium mineral C3S2 in the mineral composition of the low-carbon cement clinker obtained in step (3) is ≥50%, and the content of SO3 in the clinker is ≤1%. The existing new dry kiln can be used to process phosphogypsum and prepare clinker, the utilization rate of phosphogypsum in the ingredients is above 80%, the calcination temperature is lower than that of silicate cement clinker, and the calcined product is low-carbon cement clinker, the sum of the contents of C2S and low-calcium mineral C3S2 is ≥50%, avoiding the problem of incomplete decomposition of phosphogypsum in the decomposition furnace of the new dry kiln and resulting in molten crust.
[0039] The acquisition and detection of raw materials in the following specific examples:
[0040] Obtain phosphogypsum and silicon-aluminum-iron raw materials, dry, crush and grind them for chemical composition analysis. For example, the chemical composition of a batch of phosphogypsum, coal gangue, iron ore soil and fly ash obtained randomly is shown in Table 1:
[0041] Table 1 Chemical composition analysis
[0042] name Loss on ignition <![CDATA[SiO2]]> <![CDATA[Al2O3]]> <![CDATA[Fe2O3]]> CaO MgO <![CDATA[SO3]]> <![CDATA[K2O]]> <![CDATA[Na2O]]> Phosphogypsum 19.27 6.6 0.23 0.52 29.66 0.03 42.46 0.37 0.08 Coal Gangue 4.63 76.3 6.62 4.64 1.91 2.35 0.48 1.34 0.55 Iron Ore Soil 3.27 48.9 15.55 15.9 7.56 4.41 0.01 0.78 2.79
[0043] The carbonaceous raw material used was subjected to conventional analysis and chemical composition analysis of the ash, which is high-sulfur coal. The results are shown in Table 2 and Table 3 respectively:
[0044] Table 2 Conventional analysis of high sulfur coal
[0045] name Moisture Ash Volatile Matter Fixed carbon content Total sulfur Qnet,ad Qnet,d High sulfur coal 1.42 23.48 10.25 64.85 2.99 25.25 26.33
[0046] Table 3 Chemical composition analysis of high sulfur coal ash
[0047] name Loss on ignition <![CDATA[SiO2]]> <![CDATA[Al2O3]]> <![CDATA[Fe2O3]]> CaO MgO <![CDATA[SO3]]> <![CDATA[K2O]]> <![CDATA[Na2O]]> Coal ash 0 47.36 26.12 15.21 4.16 1.55 2.11 1.03 0.40
[0048] Example 1
[0049] 1. Ratio design
[0050] The SO3 in the chemical composition of phosphogypsum is calculated into its own ignition loss, and the remaining chemical composition is measured according to the ignition loss 19.27% + 42.46% = 61.73%, and the remaining chemical composition corresponds to the material mainly composed of CaO. The ash of the ferro-aluminum raw material and the carbon raw material (taking into account the ash introduced by the combustion of high-sulfur coal) is designed according to the KH value of 0.469, the SM value of 5.935, and the total CaO to SiO2 mass ratio of 1.494 in the chemical composition. The proportions and corresponding indicators are shown in Tables 4 and 5 respectively:
[0051] Table 4 Proportions
[0052] name Loss on ignition <![CDATA[SiO2]]> <![CDATA[Al2O3]]> <![CDATA[Fe2O3]]> CaO MgO <![CDATA[SO3]]> <![CDATA[K2O]]> <![CDATA[Na2O]]> Ratio Phosphogypsum 19.27 6.6 0.23 0.52 29.66 0.03 42.46 0.37 0.08 85.8 Coal Gangue 4.63 76.3 6.62 4.64 1.91 2.35 0.48 1.34 0.55 14.2 Coal ash 0 47.36 26.12 15.21 4.16 1.55 2.11 1.03 0.40 1.61
[0053] Table 5 Indicators corresponding to the ratio
[0054] KH SM IM <![CDATA[Total CaO:SiO2]]> 0.469 5.935 1.154 1.494
[0055] 2. Preheating
[0056] The phosphogypsum and coal gangue measured in the above ratio are mixed and ground, and the obtained mixture enters the decomposition furnace through the preheater. The decomposition furnace here only plays the role of further preheating and does not decompose CaSO4.
[0057] 3. Calcination
[0058] The preheated mixture directly enters the rotary kiln, where CaSO4 desulfurization and clinker calcination are carried out in a reducing atmosphere created by partial incomplete combustion of high-sulfur coal in the blown air. After cooling, low-carbon cement clinker is obtained. The volume concentration of CO in the rotary kiln is 6% and the calcination temperature is 1200℃.
[0059] Example 2
[0060] 1. Ratio design
[0061] The SO3 in the chemical composition of phosphogypsum is calculated into its own ignition loss, and the remaining chemical composition is measured according to the ignition loss 19.27% + 42.46% = 61.73%, and the remaining chemical composition corresponds to the material mainly composed of CaO. The ash of the ferro-aluminum raw material and the carbon raw material (taking into account the ash introduced by the combustion of high-sulfur coal) is designed according to the KH value of 0.469, the SM value of 3.735, and the total CaO to SiO2 mass ratio of 1.587 in the chemical composition. The proportions and corresponding indicators are shown in Tables 6 and 7 respectively:
[0062] Table 6 Proportion
[0063] name Loss on ignition <![CDATA[SiO2]]> <![CDATA[Al2O3]]> <![CDATA[Fe2O3]]> CaO MgO <![CDATA[SO3]]> <![CDATA[K2O]]> <![CDATA[Na2O]]> Ratio Phosphogypsum 19.27 6.6 0.23 0.52 29.66 0.03 42.46 0.37 0.08 84.6 Iron Ore Soil 3.27 48.9 15.55 15.9 7.56 4.41 0.01 0.78 2.79 6.6 Coal Gangue 4.63 76.3 6.62 4.64 1.91 2.35 0.48 1.34 0.55 8.8 Coal ash 0 47.36 26.12 15.21 4.16 1.55 2.11 1.03 0.40 1.59
[0064] Table 7 Indicators corresponding to the ratio
[0065] KH SM IM <![CDATA[Total CaO:SiO2]]> 0.469 3.735 1.037 1.587
[0066] 2. Preheating
[0067] The phosphogypsum, iron ore and coal gangue measured in the above ratio are mixed and ground, and the obtained mixture enters the decomposition furnace through the preheater. The decomposition furnace here only plays the role of further preheating and does not decompose CaSO4.
[0068] 3. Calcination
[0069] The preheated mixture directly enters the rotary kiln, where CaSO4 desulfurization and clinker calcination are carried out in a reducing atmosphere created by partial incomplete combustion of high-sulfur coal in the blown air. After cooling, low-carbon cement clinker is obtained. The volume concentration of CO in the rotary kiln is 5% and the calcination temperature is 1200℃.
[0070] Comparative Example 1
[0071] 1. Ratio design
[0072] The SO3 in the chemical composition of phosphogypsum is calculated into its own ignition loss, and the remaining chemical composition is measured according to the ignition loss 19.27% + 42.46% = 61.73%, and the remaining chemical composition corresponds to the CaO-based substance. The ash of the ferro-aluminum raw material and the carbon raw material (taking into account the ash introduced by the combustion of high-sulfur coal) is designed according to the KH value of 0.661, the SM value of 3.429, and the total CaO to SiO2 mass ratio of 2.145 in the chemical composition. The proportions and corresponding indicators are shown in Tables 8 and 9 respectively:
[0073] Table 8 Proportions
[0074] name Loss on ignition <![CDATA[SiO2]]> <![CDATA[Al2O3]]> <![CDATA[Fe2O3]]> CaO MgO <![CDATA[SO3]]> <![CDATA[K2O]]> <![CDATA[Na2O]]> Ratio Phosphogypsum 19.27 6.6 0.23 0.52 29.66 0.03 42.46 0.37 0.08 90 Iron Ore Soil 3.27 48.9 15.55 15.9 7.56 4.41 0.01 0.78 2.79 6 Coal Gangue 4.63 76.3 6.62 4.64 1.91 2.35 0.48 1.34 0.55 4 Coal ash 0 47.36 26.12 15.21 4.16 1.55 2.11 1.03 0.40 1.69
[0075] Table 9 Indicators corresponding to the ratio
[0076]
[0077] 2. Preheating
[0078] The phosphogypsum, iron ore and coal gangue measured in the above ratio are mixed and ground, and the obtained mixture enters the decomposition furnace through the preheater. The decomposition furnace here only plays the role of further preheating and does not decompose CaSO4.
[0079] 3. Calcination
[0080] The preheated mixture directly enters the rotary kiln, where CaSO4 desulfurization and clinker calcination are carried out in a reducing atmosphere created by partial incomplete combustion of high-sulfur coal in the blown air. After cooling, low-carbon cement clinker is obtained. The volume concentration of CO in the rotary kiln is 5% and the calcination temperature is 1200℃.
[0081] Comparative Example 2
[0082] 1. Ratio design
[0083] The SO3 in the chemical composition of phosphogypsum is calculated into its own ignition loss, and the remaining chemical composition is measured according to the ignition loss 19.27% + 42.46% = 61.73%, and the remaining chemical composition corresponds to the material mainly composed of CaO. The ash of the ferro-aluminum raw material and the carbon raw material (taking into account the ash introduced by the combustion of high-sulfur coal) is designed according to the KH value of 0.662, the SM value of 5.673, and the total CaO to SiO2 mass ratio of 2.040 in the chemical composition. The proportions and corresponding indicators are shown in Tables 10 and 11 respectively:
[0084] Table 10 Proportions
[0085] name Loss on ignition <![CDATA[SiO2]]> <![CDATA[Al2O3]]> <![CDATA[Fe2O3]]> CaO MgO <![CDATA[SO3]]> <![CDATA[K2O]]> <![CDATA[Na2O]]> Ratio Phosphogypsum 19.27 6.6 0.23 0.52 29.66 0.03 42.46 0.37 0.08 91.4 Coal Gangue 4.63 76.3 6.62 4.64 1.91 2.35 0.48 1.34 0.55 8.6 Coal ash 0 47.36 26.12 15.21 4.16 1.55 2.11 1.03 0.40 1.72
[0086] Table 11 Indicators corresponding to the ratio
[0087] KH SM IM <![CDATA[Total CaO:SiO2 <!-- 5 -->]]> 0.662 5.673 1.081 2.040
[0088] 2. Preheating
[0089] The phosphogypsum and coal gangue measured in the above ratio are mixed and ground, and the obtained mixture enters the decomposition furnace through the preheater. The decomposition furnace here only plays the role of further preheating and does not decompose CaSO4.
[0090] 3. Calcination
[0091] The preheated mixture directly enters the rotary kiln, where CaSO4 desulfurization and clinker calcination are carried out in a reducing atmosphere created by partial incomplete combustion of high-sulfur coal in the blown air. After cooling, low-carbon cement clinker is obtained. The volume concentration of CO in the rotary kiln is 6% and the calcination temperature is 1200℃.
[0092] In addition to the temperature of 1200°C, each embodiment and comparative example further set a calcination temperature of 1100°C. The SO3 content of the calcined product (clinker) is shown in Table 12, and the SO3 content is measured by total sulfur analysis. The main mineral content is shown in Table 13, and the main mineral content is obtained by analyzing the XRD spectrum of the calcined product (clinker) using jade software.
[0093] Table 12 SO3 content of calcined product (clinker)
[0094]
[0095] Table 13 Main mineral contents
[0096] project Calcination temperature <![CDATA[C3S2]]> <![CDATA[C2S]]> <![CDATA[SiO2]]> <![CDATA[Ca2Al2SiO7]]> CS <![CDATA[CaSO4]]> <![CDATA[C4A3S-]]> Unknown sulfur-containing mineral Example 1 1100℃ 0 68.9 5.8 16.4 7.2 0 0 0 Example 2 1100℃ 0 61.0 5.3 29.5 3.0 0 0 0 Comparative Example 1 1100℃ 0 83.7 0.8 9.2 0 1.6 1.2 2.6 Comparative Example 2 1100℃ 0 83.5 2.8 3.6 0 3.3 0.3 5.6 Example 1 1200℃ 57.8 17.7 0.9 23.6 0 0 0 0 Example 2 1200℃ 14.3 46.5 0.7 36.4 0.7 0 0 0 Comparative Example 1 1200℃ 0 85.5 0.3 9.7 0 0 3.6 0 Comparative Example 2 1200℃ 0 87.7 0.8 4.4 0 1.4 2.2 2.6
[0097] According to the research of our institute, when the KH is 0.66, the total CaO:SiO2 is 2.0-2.3:
[0098] (1) Formation of aluminum-iron phase mineral C in the ingredients 12 The part of CaSO4 in A7, C3A, C4AF and C2F relies on Fe2O3 and Al2O3 for desulfurization. The desulfurization effect of Fe2O3 and Al2O3 on CaSO4 is worse than that of SiO2.
[0099] (2) Al2O3 combines with CaO and CaSO4 to form by-product minerals, which inhibit further desulfurization;
[0100] (3) C4AF and C2F are also difficult to burn in a reducing atmosphere and cannot be formed well, resulting in a decrease in the direct desulfurization effect of Fe2O3 on CaSO4 (the part of CaSO4 required to form iron-phase minerals) and the indirect desulfurization effect (fluxing to promote the formation of C2S);
[0101] (4) The desulfurization of CaSO4 has reached the limit chemical equilibrium that can be adjusted under the KH at this time, and the SO3 content is between 1% and 3%. After using conventional raw materials, the SO3 content in the calcined product is 2%.
[0102] The present invention, under the condition of reducing atmosphere, is based on low KH (KH value is 0.66) ingredients, so that SiO2 promotes the desulfurization of CaSO4 to form a more stable and easier to generate mineral C2S. The method continues to optimize and improve, reduces KH to a total CaO:SiO2 ratio of less than 2, provides more SiO2 for desulfurization, makes all CaSO4 have SiO2 and excess SiO2 is matched to generate calcium silicate-containing minerals, allows the desulfurization chemical balance of SiO2 on CaSO4 to continue to move in the direction of desulfurization, and reduces the negative impact of Fe2O3 and Al2O3 that cannot further desulfurize CaSO4.
[0103] Compared with Example 1, Example 2 has a lower SM value and a higher total CaO:SiO2, which is equivalent to having more Al2O3 and Fe2O3 in the ingredients. Due to the negative impact of the presence of Al2O3 and Fe2O3 that cannot further desulfurize CaSO4, the SO3 content in the calcined product is slightly higher than that in Example 1. However, because the mixed material entering the rotary kiln is in powder form, the heating and atmosphere conditions are more uniform than those of a spherical material, and the SO3 content can still be reduced to less than 1%.
[0104] Compared with all the embodiments, Comparative Examples 1 and 2 mainly have higher KH values (higher total CaO:SiO2), that is, the company has made breakthrough progress in the decomposition and desulfurization of phosphogypsum in recent research, and applied for an invention patent for "a process for desulfurization and co-production of cement for phosphogypsum", which mainly adopts a method of mixing and desulfurization of ingredients with low KH values, with a KH value of 0.6-0.7, so that SiO2 promotes the desulfurization of CaSO4 to form a more stable and easier to generate mineral C2S, but the SO3 content after calcination at 1100°C is 1-3%, and cannot be reduced to below 1%; Comparative Example 2 has a higher SM value than Comparative Example 1. When KH is 0.66, the high SM value will aggravate the difficulty in burning due to insufficient liquid phase minerals, so the SO3 content is higher than that of Comparative Example 1; the SO3 content after calcination at 1200°C is 2-3%.
[0105] In the embodiment, based on the premise that SiO2 promotes CaSO4 desulfurization at low KH value to form a more stable and easier to generate mineral C2S, a lower KH value and total CaO:SiO2 are used to provide more SiO2 for desulfurization and reduce the eutectic temperature, thereby solving the problem of difficult burning and desulfurization at high KH value. The higher SM value reduces the negative impact of Fe2O3 and Al2O3 in not being able to further desulfurize CaSO4. The final SO3 content is successfully reduced to less than 1%. The XRD spectrum of Example 1 is shown in Figure 1 As shown, combined Figure 1 It can be seen from Table 12 and Table 13 that a high desulfurization rate has been achieved at 1100℃, and no CaSO4 peak can be seen. Desulfurization is based on the formation of C2S, and a large amount of C3S2 is not formed until 1200℃. The calcined product at 1100℃ has C2S ≥ 65%, which can be used as a highly active admixture or admixture; the calcined product at 1200℃ is a clinker with C3S2 ≥ 50% and C2S ≥ 15%, that is, low-carbon cement clinker.
[0106] The above-mentioned embodiments are only preferred embodiments of the present invention and cannot be used to limit the scope of protection of the present invention. Any non-substantial changes and substitutions made by technicians in this field on the basis of the present invention shall fall within the scope of protection required by the present invention.
Claims
1. A method for treating phosphogypsum and preparing low-carbon cement clinker using a dry kiln, Features The following steps are involved: (1) Obtain phosphogypsum, dry, crush and grind it, mix it with silicon, aluminum and iron raw materials and grind it; the ingredients are KH=0.4-0.5 and SM=2-7; (2) The obtained mixed material is preheated in a preheater and a decomposition furnace; (3) The preheated mixture directly enters the rotary kiln for CaSO 4 The desulfurization and clinker calcination are carried out to obtain low-carbon cement clinker after cooling; the reducing atmosphere is controlled by the incomplete combustion of the carbonaceous raw materials so that the volume concentration of CO in the rotary kiln is 2%-10%; the calcination temperature of the rotary kiln is 1150-1300℃.
2. The method for treating phosphogypsum and preparing low carbon cement clinker by using a dry kiln as claimed in claim 1, Features The ferro-aluminum raw material in step (1) is one or more of sandstone, coal gangue, silica, clay and fly ash.
3. The method for treating phosphogypsum and preparing low carbon cement clinker by using a dry kiln as claimed in claim 1, Features In step (1), the ingredients used are SM=4-7.
4. The method for treating phosphogypsum and preparing low carbon cement clinker by using a dry kiln as claimed in claim 1, Features The calcination temperature of the rotary kiln in step (3) is 1200-1250°C.
5. The method for treating phosphogypsum and preparing low carbon cement clinker by using a dry kiln as claimed in claim 1, Features The mineral composition of the low carbon cement clinker obtained in step (3) is C 2 S and low calcium mineral C 3 S 2 The sum of the contents of SO in clinker is ≥50%. 3 The content is ≤1%.