A smelting method for improving the yield of high-titanium steel metal titanium

By using new deoxidant and slag-making agents during the smelting of high-titanium steel, the oxygen and nitrogen content is controlled, and the problem of Ti reacting with N and O to form inclusions is solved, the yield of titanium and the quality of casting is improved, and the yield of titanium is increased, and the quality of casting is extended. High-titanium steel wear resistance.

CN116716447BActive Publication Date: 2024-12-03ANGANG STEEL CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202310585032.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-05-23
Publication Date
2024-12-03
Estimated Expiration
2043-05-23

AI Technical Summary

Technical Problem

When the existing smelting method produces high-titanium steel, Ti reacts with N and O in the steel to form inclusions, which affects the yield of metal titanium and the quality of casting billets. Especially when the N content in the molten steel reaches 0.0050%, the formation of TiN decreases. Received rate.

Method used

Using new deoxidant (aluminum slag balls) and slag-making agents (lime, bauxite, SD slag balls), the oxygen and nitrogen contents are controlled during the refining process of converter steel discharge and LF furnaces to prevent the formation of TiN, and Al2O3 and AlN are used. The adsorption effect reduces the amount of inclusions and increases the amount of slag in the LF furnace to prevent nitrogen inhalation.

Benefits of technology

The yield of metal titanium is improved to more than 90%, the inclusions in the casting billet is reduced, the wear resistance of high titanium steel is extended, and the N content in the molten steel is stabilized and the formation of TiN is avoided.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004242961240000051
    Figure BDA0004242961240000051
  • Figure BDA0004242961240000061
    Figure BDA0004242961240000061
Patent Text Reader

Abstract

The present invention relates to the technical field of high-titanium steel production, and in particular to a smelting method for improving the yield of titanium metal in high-titanium steel. The weight percentage content of Ti in the molten steel is 0.5% to 2.0%. The smelting method specifically comprises the following steps: step 1) converter tapping endpoint control, step 2) deoxidation alloying, adding alloy into the ladle, step 3) during LF furnace refining, the slag volume is increased to 9.5 to 12.5 kg / ton of steel, and step 4) after the refining is completed, the machine is cast, and after the casting is completed, the Ti content in the steel is measured and the inclusions in the ingot are detected. The yield of titanium metal reaches more than 90% without generating inclusions.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of high-titanium steel production, and in particular to a smelting method for improving the yield of metallic titanium in high-titanium steel. Background Art

[0002] Titanium (Ti) is a good deoxidizing and degassing agent and an effective element for fixing nitrogen and carbon in steel. The application of titanium in steel is mainly in the form of microalloying. Adding a certain amount of titanium (0.01% to 0.03%) to steel can achieve the effects of refining the structure of steel, improving the strength of steel, and improving the plasticity and impact toughness of steel. With the increase of titanium content in steel, the toughness, processing performance and wear resistance of the product are greatly improved, especially when Ti ≥ 0.15% in steel, a large amount of micron-level (1 to 5 μm) TIC (≥ 80%) and a small amount of TIN can be obtained. The wear resistance of the product is more than 10 times that of titanium microalloyed steel, and the service life of the product is significantly extended. Therefore, high-titanium steel has a very broad application prospect.

[0003] However, when producing high-titanium steel through existing smelting methods, when the weight percentage of Ti in molten steel is 0.5% to 2.0%, Ti in the steel often reacts with N and O to form inclusions, which not only affects the yield of metallic titanium, but also affects the quality of the ingot. According to relevant research, when the N content in molten steel reaches 0.0050%, Ti will react with N to form TiN inclusions, which will increase the burnout of Ti and reduce the yield. Summary of the invention

[0004] In order to overcome the shortcomings of the prior art, the present invention provides a smelting method for improving the yield of titanium metal in high-titanium steel, which not only makes the yield of titanium metal reach more than 90%, but also does not produce inclusions.

[0005] A smelting method for improving the yield of titanium metal in high-titanium steel, wherein the weight percentage of Ti in the molten steel is 0.5% to 2.0%, and the smelting method specifically comprises the following steps:

[0006] Step 1) Converter tapping endpoint control:

[0007] The weight percentage content of C in the steel is controlled at 0.04% to 0.06%, and steel tapping is prohibited above 0.07%. The weight percentage content of P is controlled at ≤0.006%, the steel tapping temperature is controlled at 1650 to 1680°C, and the temperature after argon blowing is controlled at 1595 to 1615°C.

[0008] Step 2) Deoxidation alloying:

[0009] The converter must be oxygenated before steel is tapped, and the amount of alloy added is adjusted according to the oxygen content in the steel.

[0010] The alloy components are calcium carbide powder (composite deoxidizing slag), high carbon ferromanganese, ferroaluminum, and aluminum slag balls (new deoxidizer).

[0011] By weight percentage:

[0012] The composition of calcium carbide powder is CaC2: 70% to 80%, CaO ≤ 20%, Si + Fe + C ≤ 6%;

[0013] The composition of high carbon ferromanganese is C ≥ 7%, Mn ≥ 70%, Fe ≤ 30%;

[0014] The composition of aluminum iron is Al: 45% to 57%, C ≤ 0.5%, Si ≤ 2%, and the balance is Fe;

[0015] The composition of aluminum slag balls is Al≥40%, Al2O3: 20%~25%, AlN: 10%~20%, SiO2≤6%, S+P≤0.05%, MgO: 3%~8%.

[0016] Adding alloy to the ladle:

[0017] Calcium carbide powder is added along with the steel flow by hand-throwing at the back of the furnace, and the added amount is 0.6-2.5kg / ton of steel; when the added amount of calcium carbide powder exceeds 100kg, the remaining part can be added to the bottom of the ladle before tapping.

[0018] The amount of high carbon ferromanganese added is 5 to 7 kg per ton of steel. Start adding when the molten steel reaches 1 / 4 to 1 / 3 of the total amount of molten steel, and add it in 3 to 6 times.

[0019] Aluminum iron and aluminum slag balls are added in sequence by hand at the back of the furnace. The amount of aluminum iron added is 2-3kg / ton of steel, and the amount of aluminum slag balls added is 1-1.5kg / ton of steel.

[0020] Finally, lime is added, with the amount of lime added being 1.0 to 2.0 kg per ton of steel.

[0021] All alloys added to the ladle must be added when the molten steel reaches 3 / 4 of the output.

[0022] Step 3) During LF furnace refining, the slag amount is increased to 9.5-12.5 kg / ton steel to prevent the molten steel from being exposed to the air and absorbing nitrogen, thereby generating TiN inclusions.

[0023] The slag-making agent components are lime, bauxite and SD slag balls.

[0024] Calculated by weight percentage, the chemical composition of SD slag ball is as follows: Al≥20%, Al2O3 is 40%~60%, CaO is 2%~10%, and AlN≤10%.

[0025] The chemical composition of lime is as follows: CaO ≥ 88%, Al2O3 ≤ 0.5%, SiO2 ≤ 1.2%.

[0026] The chemical composition of bauxite is as follows: CaO≤0.5%, Al2O3≥85%, MgO≤0.5%, H2O≤2.0%, TiO2≤5.0%.

[0027] The mass ratio of CaO to Al2O3 in the slag is 1.6 to 1.8.

[0028] Determine the O and N content in the molten steel. After meeting the composition requirements, add 5.6-22.4kg / ton of steel sponge titanium. After the sponge titanium is fully melted, keep it at 1515-1585℃ for 10-30min. In terms of weight percentage, the chemical composition of sponge titanium is as follows: Ti≥99.9%, and the balance is iron.

[0029] Step 4) After refining, the steel is put into casting machine. After casting, the Ti content in the steel is determined and the inclusions in the ingot are detected.

[0030] In order to achieve the above object, the present invention adopts the following technical solutions:

[0031] Compared with the prior art, the present invention has at least the following technical effects or advantages:

[0032] 1. Most traditional deoxidizers use aluminum for deoxidation, but aluminum and oxygen in steel generate Al2O3 inclusions. Large inclusions will enter the slag, while fine and dispersed micron-sized inclusions will remain in the molten steel, affecting the quality of the ingot. The novel deoxidizer (aluminum slag ball) adopted by the present invention has the following components: Al≥40%, Al2O3: 20%-25%, AlN: 10%-20%, SiO2≤6%, S+P≤0.05%, MgO: 3%-8%, and the metal Al and AlN in the novel deoxidizer react with O in steel to generate Al2O3; Al2O3 has strong clustering performance, so the Al2O3 in the novel deoxidizer can adsorb small particles of Al2O3 inclusions dispersed in the steel, so that the Al2O3 inclusions aggregate and grow, and are more likely to float, thereby playing a deoxidation role; at the same time, the AlN in the novel deoxidizer also reacts with MnO in the slag, reduces MnO to Mn and brings it back into the molten steel, reduces the burning loss of Mn, and improves the recovery rate of metal Mn.

[0033] 2. The present invention increases the amount of slag (9.5-12.5 kg / ton steel) during LF furnace refining to prevent molten steel from being exposed to the air and absorbing nitrogen to produce TiN inclusions, thereby stably controlling the N content in the molten steel to be less than 0.0050%, preventing Ti in the steel from reacting with N to produce excessive TiN precipitates, which affects the quality of subsequent castings. The new slag-making agent used in the present invention is composed of lime, bauxite, and SD slag balls, wherein the SD slag balls have Al≥20%, Al2O3 of 40%-60%, CaO of 2%-10%, and AlN≤10%. The Al2O3 in the slag-forming agent can further absorb fine inclusions in the steel, control the CaO / Al2O3 at 1.6-1.8, enhance the ability to absorb inclusions, and make them float more easily; the AlN in the slag-forming agent will react with the unstable oxides (FeO+MnO) in the refined slag, bring the reduced metal Fe and Mn back to the molten steel, and reduce the (FeO+MnO) content in the refined slag. When the (FeO+MnO) content is less than 1%, the reducibility of the refined slag is enhanced and the diffusion deoxidation ability is also enhanced, which is conducive to the desulfurization reaction, thereby further enhancing the desulfurization ability of the LF furnace.

[0034] 3. The present invention adopts a deoxidation method of a new deoxidizer (aluminum slag ball) converter steel deoxidation-LF furnace new slag-making agent (SD slag ball) deoxidation-titanium alloying, which fully reduces the oxygen content and the number of inclusions in the steel before titanium alloying, and utilizes the converter steel deoxidation method to prevent FeO (10%-15%) in the converter slag from being brought into the refined slag. The AlN in the new slag-making agent is used to reduce the content of unstable oxides (FeO+MnO) in the refined slag, prevent Ti from reacting with (FeO+MnO), enhance the reducibility of the refined slag, and reduce the burning oxidation of titanium, thereby increasing the titanium recovery rate to more than 90% and reducing the number of Al2O3 and TiO2 inclusions, reducing the inclusions in the ingot by 22%. At the same time, although the N generated by the AlN reaction will increase the N content of the molten steel, the N content in the steel does not exceed 0.0050%. Therefore, the TiN generated in the steel does not aggregate to form large particle inclusions. Instead, the generated micron- and nano-scale TiN precipitates improve the wear resistance of high titanium steel.

[0035] The recovery rate of titanium metal reaches more than 90% without generating inclusions. DETAILED DESCRIPTION

[0036] The present invention discloses a smelting method for improving the yield of titanium metal in high-titanium steel. Those skilled in the art can refer to the content of this article and appropriately improve the process parameters to achieve it. It is particularly important to point out that all similar substitutions and modifications are obvious to those skilled in the art, and they are all considered to be included in the present invention. The method and application of the present invention have been described through preferred embodiments, and relevant personnel can obviously modify or appropriately change and combine the methods and applications described herein without departing from the content, spirit and scope of the present invention to implement and apply the technology of the present invention.

[0037] A smelting method for improving the yield of titanium metal in high-titanium steel, wherein the weight percentage of Ti in the molten steel is 0.5% to 2.0%, and the smelting method specifically comprises the following steps:

[0038] 1. Control of converter tapping endpoint: The weight percentage of C in tapping is controlled at 0.04%-0.06% (tapping is prohibited if it is above 0.07%), the weight percentage of P is ≤0.006%, the tapping temperature is controlled at 1650-1680°C, and the temperature after argon blowing is guaranteed to be 1595-1615°C.

[0039] 2. Deoxidation and alloying: The converter must be oxygenated before steel is tapped. The amount of alloy added is adjusted according to the oxygen content in the steel. The alloy uses composite deoxidizing slag (calcium carbide powder), high carbon ferromanganese, aluminum iron, and a new deoxidizer (aluminum slag balls).

[0040] Among them, in terms of weight percentage, the composition of calcium carbide powder is CaC2: 70%~80%, CaO≤20%, Si+Fe+C≤6%; the composition of high carbon ferromanganese is C≥7%, Mn≥70%, Fe≤30%; the composition of ferroaluminum is Al: 45%~57%, C≤0.5%, Si≤2%, and the balance is Fe; the composition of aluminum slag balls is Al≥40%, Al2O3: 20%~25%, AlN: 10%~20%, SiO2≤6%, S+P≤0.05%, MgO: 3%~8%.

[0041] 3. Calcium carbide powder is added with the steel flow by hand-throwing at the back of the furnace, and the added amount is 0.6kg~2.5kg / ton of steel. When the added amount of calcium carbide powder exceeds 100kg, the remaining part can be added to the bottom of the ladle before tapping. High carbon ferromanganese (added amount is 5kg~7kg / ton of steel) starts to be added when the molten steel reaches 1 / 4~1 / 3 of the total amount of molten steel, and is added in 3~6 times. Aluminum iron (added amount is 2kg~3kg / ton of steel) and aluminum slag balls (added amount is 1kg~1.5kg / ton of steel) are added in sequence by hand-throwing at the back of the furnace, and finally 1.0kg~2.0kg / ton of lime is added. All alloys added to the ladle must be added when the molten steel reaches 3 / 4 of the tapping amount.

[0042] 4. Increase the amount of slag (9.5kg-12.5kg / ton steel) during LF furnace refining to prevent the molten steel from being exposed to the air and absorbing nitrogen to produce TiN inclusions. The slag-making agent is composed of lime, bauxite, and SD slag balls (Al≥20%, Al2O340%-60%, CaO2%-10%, AlN≤10%) by weight percentage. The lime and bauxite components are shown in Table 1. The mass ratio of CaO to Al2O3 in the slag is 1.6-1.8.

[0043] Table 1 Slag forming agent composition table (wt / %)

[0044]

[0045]

[0046] The O and N contents in the molten steel were determined. After the composition requirements were met, 5.6kg to 22.4kg / ton of steel sponge titanium was added. The composition of the sponge titanium is shown in Table 2. After full melting, the temperature was maintained at 1515 to 1585°C for 10 to 30 minutes.

[0047] Table 2 Titanium sponge composition (wt / %)

[0048] raw material Ti Fe N Titanium sponge ≥99.9 margin /

[0049] 5. After refining, the steel is put into casting machine. After casting, the Ti content in the steel is determined and the inclusions in the ingot are detected.

[0050] Embodiment 1:

[0051] Taking a 100-ton converter as an example, producing high-titanium steel with a Ti content of 0.5%:

[0052] 1. The weight percentage of C in the converter steel is 0.055%, the steel tapping temperature is 1665°C, and the weight percentage of O in the steel is 0.055%.

[0053] 2. Add 200kg of calcium carbide powder by hand-throwing at the back of the furnace along with the steel flow. 550kg of high carbon ferromanganese is added when the molten steel reaches 1 / 3 of the total amount of molten steel, and is added in 5 times. 250kg of ferroaluminum and 140kg of aluminum slag balls are added in sequence by hand-throwing at the back of the furnace, and finally 160kg of lime is added. All alloys added to the ladle are added when the molten steel reaches 3 / 4 of the amount of steel.

[0054] 3. LF furnace refining: add slag-making agent 630kg lime, 400kg bauxite, 20kg SD slag ball, slag amount is 1050kg, covering the steel liquid surface. The O content in the steel is less than 0.0005%, and the N content is less than 0.0050%. Add 560kg sponge titanium, and keep it at 1550℃ for 20 minutes after full melting.

[0055] 4. After refining, the steel was put into casting machine. After casting, the Ti content in the steel was measured to be 0.51%, and the titanium recovery rate was 92%.

[0056] Embodiment 2:

[0057] Taking a 100-ton converter as an example, producing high-titanium steel with a Ti content of 0.9%:

[0058] 1. The weight percentage of C in the converter steel is 0.034%, the steel tapping temperature is 1680°C, and the weight percentage of O in the steel is 0.081%.

[0059] 2. Add 290kg of calcium carbide powder by hand-throwing at the back of the furnace along with the steel flow. 650kg of high carbon ferromanganese is added when the molten steel reaches 1 / 4 of the total amount of molten steel, and is added in 6 times. 280kg of ferroaluminum and 170kg of aluminum slag balls are added in sequence by hand-throwing at the back of the furnace, and finally 180kg of lime is added. All alloys added to the ladle are added when the molten steel reaches 3 / 4 of the total amount of steel.

[0060] 3. LF furnace refining: add slag-making agent 650kg lime, 380kg bauxite, 30kg SD slag ball, slag amount is 1060kg, covering the steel liquid surface. The O content in the steel is less than 0.0005%, and the N content is 0.0020%. Add 1010kg sponge titanium, and keep it at 1570℃ for 15 minutes after full melting.

[0061] 4. After refining, the steel was put into casting machine. After casting, the Ti content in the steel was measured to be 0.91%, and the titanium recovery rate was 90%.

[0062] Embodiment 3:

[0063] Taking a 100-ton converter as an example, producing high-titanium steel with a Ti content of 1.4%:

[0064] 1. The weight percentage of C in the converter steel is 0.045%, the steel tapping temperature is 1675°C, and the weight percentage of O in the steel is 0.065%.

[0065] 2. Add 270kg of calcium carbide powder by hand-throwing at the back of the furnace along with the steel flow. 620kg of high carbon ferromanganese begins to be added when the molten steel reaches 1 / 4 of the total amount of molten steel, and is added in 6 times. 280kg of ferroaluminum and 140kg of aluminum slag balls are added in sequence by hand-throwing at the back of the furnace, and finally 180kg of lime is added. All alloys added to the ladle are added when the molten steel reaches 3 / 4 of the total amount of steel.

[0066] 3. LF furnace refining: add slag-making agent 730kg lime, 420kg bauxite, 50kg SD slag ball, 1200kg slag to cover the steel liquid surface. The O content in the steel is less than 0.0005%, and the N content is 0.0033%. Add 1600kg sponge titanium, and keep it at 1560℃ for 25 minutes after full melting.

[0067] 4. After refining, the steel was put into casting machine. After casting, the Ti content in the steel was measured to be 1.43%, and the titanium recovery rate was 90%.

[0068] Table 2 Effect of using new slag-making agent and deoxidizer on nitrogen addition in molten steel (wt%)

[0069]

[0070] Table 2 shows the effect of using new slag-forming agent and deoxidizer on nitrogen addition in molten steel. As shown in Table 2, the titanium recovery rate is increased from the original 70% to more than 90%. The new slag-forming agent and deoxidizer are selected to deoxidize during the steel tapping of the converter, which effectively reduces the inclusions in the ingot. The titanium recovery rate of the present invention is increased to more than 90%; the inclusions in the ingot are reduced by 22%; the N content in the molten steel is stably controlled to be less than 0.0050%, and no TiN inclusions are generated.

[0071] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.

Claims

1. A smelting method for improving the yield of titanium metal in high-titanium steel, characterized in that: The Ti weight percentage content in the molten steel is 0.5% to 2.0%. The smelting method specifically comprises the following steps: Step 1) Control of converter tapping endpoint: The weight percentage of C in the tapped steel is controlled at 0.04%~0.06%, the weight percentage of P is controlled at ≤0.006%, the tapping temperature is controlled at 1650~1680℃, and the temperature after argon blowing is controlled at 1595~1615℃; Step 2) Deoxidation alloying: The alloy components are calcium carbide powder, high carbon ferromanganese, aluminum iron, and aluminum slag balls; by weight percentage: the components of the aluminum slag balls are Al≥40%, Al2O3: 20%~25%, AlN: 10%~20%, SiO2≤6%, S+P≤0.05%, and MgO: 3%~8%; Adding alloy to the ladle: Calcium carbide powder is added with the steel flow, and the amount added is 0.6~2.5kg / ton of steel; The amount of high carbon ferromanganese added is 5~7kg / ton steel. Start adding when the molten steel reaches 1 / 4~1 / 3 of the total amount of molten steel, and add it in 3~6 times; Aluminum iron and aluminum slag balls are added in sequence, with the amount of aluminum iron added being 2~3kg / ton of steel and the amount of aluminum slag balls added being 1~1.5kg / ton of steel; Finally, lime is added, the amount of lime added is 1.0~2.0kg / ton of steel; All alloys are added when the molten steel reaches 3 / 4 of the output; Step 3) During LF furnace refining, the slag amount is increased to 9.5~12.5kg / ton steel; The slag-making agent components are lime, bauxite, and SD slag balls; In terms of weight percentage, the chemical composition of SD slag ball is as follows: Al ≥ 20%, Al2O3 40% to 60%, CaO 2% to 10%, AlN ≤ 10%; The mass ratio of CaO to Al2O3 in the slag is 1.6~1.8; Determine the O and N content in the molten steel. Once the composition requirements are met, add 5.6-22.4kg / ton of steel titanium sponge; Step 4) After refining, the steel is put into casting machine. After casting, the Ti content in the steel is determined and the inclusions in the ingot are detected.

2. A smelting method for improving the yield of titanium metal in high-titanium steel according to claim 1, characterized in that: Step 2) By weight percentage: The composition of calcium carbide powder is CaC2: 70%~80%, CaO≤20%, Si+Fe+C≤6%; The composition of high carbon ferromanganese is C≥7%, Mn≥70%, Fe≤30%; The composition of aluminum iron is Al: 45%~57%, C≤0.5%, Si≤2%, and the balance is Fe.

3. A smelting method for improving the yield of titanium metal in high-titanium steel according to claim 1, characterized in that: Step 2) When the amount of calcium carbide powder added exceeds 100kg, the remaining part is added to the bottom of the ladle before tapping.

4. A smelting method for improving the yield of titanium metal in high-titanium steel according to claim 1, characterized in that: Step 3) The chemical composition of lime is as follows by weight percentage: CaO ≥ 88%, Al2O3 ≤ 0.5%, SiO2 ≤ 1.2%.

5. The smelting method for improving the yield of titanium metal in high-titanium steel according to claim 1, characterized in that: Step 3) The chemical composition of bauxite is as follows by weight percentage: CaO≤0.5%, Al2O3≥85%, MgO≤0.5%, H2O≤2.0%, TiO2≤5.0%.

6. A smelting method for improving the yield of titanium metal in high-titanium steel according to claim 1, characterized in that: Step 3) The chemical composition of the titanium sponge is as follows by weight percentage: Ti ≥ 99.9%, and the balance is iron.

7. The smelting method for improving the yield of titanium metal in high-titanium steel according to claim 1, characterized in that: Step 3) After the titanium sponge is fully melted, keep it at 1515~1585℃ for 10~30min.

Citation Information

Patent Citations

  • Low-cost manufacturing method of deformed steel bar

    CN110512046A

  • Machining method for controlling titanium oxide of titanium-containing alloy steel and adopted tundish

    CN113275529A

  • Method for controlling inclusion of Ti2O3 and TiN during smelting of high-titanium steel in induction furnace

    CN114350899A

  • Method of melting titanium-containing steel

    JP2003293029A

  • Method for preparing titanium-containing ultra-low-carbon steel

    WO2023274223A1