A high temperature heat storage prefabricated component and preparation method thereof
By pressing and sintering the manganese-iron composite metal oxide heat storage material under high pressure in an inert atmosphere, the problems of low material density and poor mechanical strength in the existing technology are solved, and more efficient heat storage performance and stability are achieved.
Patent Information
- Application Number
- CN202310915792.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-07-25
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2043-07-25
AI Technical Summary
The preparation process of existing ferromanganese composite metal oxide heat storage materials is complicated, resulting in low density, many surface defects, poor mechanical strength, and easy cracking and disintegration during use, which limits its practical application.
Manganese carbonate and iron-based raw materials are pressed and formed under high pressure in an inert atmosphere, then sintered and densified, and activated at high temperature in an oxidizing atmosphere to form a high-temperature heat storage preform.
The thermal storage performance, mechanical properties and density are improved, surface defects are reduced, and the stability and service life of the thermal storage preforms are enhanced.
Smart Images

Figure FT_1 
Figure FT_2 
Figure FT_3
Abstract
Description
Technical Field
[0001] The invention relates to the field of energy storage, and in particular to a manganese-iron composite metal oxide heat storage preform and a preparation method thereof. Background Art
[0002] With the development of society, energy shortage has become an important issue faced by people. The development and utilization of renewable energy has important practical significance for energy conservation and environmental protection. Therefore, the development of thermal energy storage technology is particularly important. Thermal energy storage is to store the excess heat or waste heat that cannot be used temporarily or cannot be used in a certain way, and use it for other purposes at the right time. This technology has broad application prospects in the fields of solar energy utilization, "peak shifting and valley filling" of electricity, recycling of gas waste heat and waste heat, energy conservation in industrial and civil buildings and air conditioning, and has become a research hotspot worldwide.
[0003] Heat storage mainly includes three forms: sensible heat, latent heat of phase change and chemical reaction heat. Sensible heat storage (such as molten salt, thermal oil, water, etc.) mainly uses the rise and fall of the medium temperature to achieve heat storage and release. The process is relatively simple and the application is the most widely used, but its heat storage temperature generally does not exceed 570℃, and the heat storage energy density is relatively low, which is difficult to meet the needs of the next generation of high-temperature application technology (>700℃); latent heat storage uses the latent heat of the medium phase change process to achieve heat storage and release, but the thermal conductivity is low, the heat exchange during the phase change process is difficult to control, and the phase change material usually needs to be encapsulated, the process is complex, and the cost is high. Chemical heat storage uses the thermal effect of reversible chemical reactions to store and release energy. Depending on the application scenario and storage / release requirements, the range of optional reaction materials is relatively wide; in addition, the energy storage density can be one order of magnitude higher than sensible heat, which is convenient for long-term storage or long-distance transportation. High-temperature thermochemical energy storage technology based on metal oxides (such as cobalt / manganese / copper / iron, etc.) achieves energy storage / release through reduction / oxidation reactions between metal oxides of different valence states. The heat storage temperature can reach above 800°C, and the energy storage density can reach 1000kJ / kg within a small temperature change range.
[0004] Among them, manganese-based metal oxide heat storage systems have the advantages of low price, suitable reaction temperature range, non-toxicity and pollution. However, the reoxidation reaction kinetics of pure manganese oxide after high-temperature reduction is slow, and there is even a problem of inability to complete reoxidation.
[0005] In this regard, the prior art proposes to dope manganese-based metal oxides with Fe elements to generate manganese-iron composite metal oxide heat storage materials (Mn 1-x Fe x)2O3, which enhances the oxygen adsorption capacity of manganese-based composite metal oxide thermal storage materials and improves the oxygen ion diffusion rate. Furthermore, in the prior art, materials such as zirconium dioxide, aluminum oxide or silicon dioxide are often used as additives to modify manganese-iron composite metal oxide thermal storage materials to improve their structural strength and thermal shock resistance.
[0006] CN115477927A discloses a modified manganese-iron composite metal oxide heat storage material and its preparation method, wherein the main heat storage material is (Mn 1-x Fe x )2O3, and its preparation method is to first evenly mix a manganese source (reagent grade high-purity manganese dioxide) and an iron source to obtain a precursor, calcine the precursor at high temperature and then take it out and grind it to obtain manganese-iron composite metal oxide particles, and then mix the manganese-iron composite metal oxide particles with an anti-sintering additive powder, calcine it at high temperature, and obtain the main heat storage material manganese-iron composite metal oxide. The heat storage material prepared by this patent is actually an intermediate product. In practical applications, it is necessary to pressurize the obtained manganese-iron composite metal oxide and then sinter it to obtain a heat storage preform. The above-mentioned preparation process is a multi-step reaction process, which requires multiple steps of grinding and calcination, and the operation is cumbersome. The obtained heat storage preform has a low density, many surface defects, and poor mechanical strength. It is very easy to crack or even disintegrate during use, which seriously limits the practical application of metal oxide heat storage materials. In addition, the raw material used in the above scheme is reagent grade high-purity manganese dioxide, which is expensive. Summary of the invention
[0007] The present invention overcomes the deficiencies in the prior art and provides a high-temperature heat storage prefabricated component and a preparation method thereof.
[0008] The high-temperature heat storage preform comprises a heat storage main material and an active auxiliary agent, wherein the heat storage main material is a manganese-iron-based high-temperature metal oxide; the high-temperature heat storage preform is prepared by the following method:
[0009] Step 1: Mix manganese carbonate, iron-based raw materials and active additive powder in a certain proportion and press them under high pressure to obtain a green preform;
[0010] Step 2: Sintering and densifying the green preform obtained in step 1 under an inert atmosphere to obtain the high-temperature heat storage preform;
[0011] Step 3: Activate the high-temperature heat storage preform obtained in step 2 at high temperature in an oxidizing atmosphere.
[0012] Preferably, the sintering temperature in step 2 is 800-1000°C.
[0013] Preferably, the high temperature activation temperature of step three is 850-950°C.
[0014] Preferably, the compression molding method is a molding method.
[0015] Preferably, the iron-based raw material is: iron carbonate, iron oxide or a mixture thereof, most preferably ferric oxide.
[0016] Preferably, the active auxiliary agent is boron nitride.
[0017] Preferably, the density of the high temperature heat storage preform after densification is in the range of 3.5-4.8 g / cm 3 ;
[0018] Preferably, the inert gas is nitrogen, argon or a mixture thereof.
[0019] Preferably, the oxidizing atmosphere is air.
[0020] The present invention finds that by using cheap manganese carbonate as a raw material, the decomposition property of manganese carbonate in a high-temperature inert environment can be utilized, and the preform is first formed and then directly sintered into a phase, and the phase formation process does not require human intervention. The obtained preform has better heat storage performance, better mechanical properties, better density and lower surface defects than the prior art. Specifically:
[0021] Manganese carbonate can undergo the following reactions in air:
[0022] MnCO3+1 / 2O2→MnO2+CO2 Reaction I
[0023] MnCO3+1 / 4O2→1 / 2Mn2O3+CO2 Reaction II
[0024] MnCO3+1 / 6O2→1 / 3Mn3O4+CO2 Reaction III
[0025] According to the thermodynamic results of manganese carbonate decomposition under different conditions, reaction I occurs preferentially in air, and manganese carbonate decomposes into MnO2;
[0026] In an inert environment, manganese carbonate decomposes directly, namely:
[0027]
[0028] According to the thermodynamic calculation results of reaction I and reaction IV, reaction I is an exothermic reaction, while reaction IV is an endothermic reaction, and the reaction rate of reaction IV is significantly lower, so the stress generated is smaller, which is helpful to the stability of the heat storage preform.
[0029] The present invention uses manganese carbonate as the raw material of manganese-based heat storage material, and sinters it with iron-based raw material additives in an inert environment. Manganese carbonate will directly decompose into manganese monoxide in a high-temperature inert environment, and further react with iron-based raw materials, such as iron oxide, to generate the required manganese-iron composite metal oxide heat storage material. Under pressure and high temperature, the manganese-iron composite metal oxide heat storage material is sintered and densified in one step to form a heat storage preform with a suitable density. Thermodynamic calculation data show that the decomposition reaction of manganese carbonate in air is an exothermic reaction, while the decomposition reaction in an inert environment is an endothermic reaction. Therefore, unlike the decomposition in air, the decomposition reaction rate of manganese carbonate in an inert gas environment is low, the reaction stress generated is small, and the heat storage preform can still remain intact after sintering. The heat absorption and release of manganese-iron composite metal oxide heat storage material at high temperature is achieved through its own reduction and oxidation reaction, accompanied by the absorption and release of oxygen, and the material itself will produce huge stress. If the mechanical strength of the heat storage preform itself is insufficient, it is easy to crack and disintegrate, and it cannot continue to be used. Therefore, it is required that the sintered preform needs to have sufficient density and mechanical strength.
[0030] In the prior art, the calcined manganese-iron composite metal oxide is pressed into powder and then sintered. The sintering activity of the powder particle surface is reduced, and the bonding strength between particles is limited, so sufficient mechanical strength cannot be obtained.
[0031] If excessive high pressure pressing or high temperature sintering is used to improve mechanical strength, the heat storage preform is over-densified, which will cause the gas diffusion microchannels inside the heat storage preform to close, and the heat storage material cannot absorb and release oxygen, and the necessary reaction for heat absorption and release cannot occur, resulting in a serious decline in the overall heat storage performance. The present invention uses manganese carbonate as the raw material of manganese-based heat storage material, and presses it with iron-based raw materials, additives, etc. under high pressure, and forms a heat storage preform after reaction sintering in an inert environment. Molding and high-temperature sintering make the preform fully densified, and the decomposition of manganese carbonate during the sintering process will release a large amount of carbon dioxide, forming microchannels for gas diffusion inside the preform, so that it still has good heat storage performance while maintaining high mechanical strength.
[0032] Since manganese carbonate is used as the raw material in the present invention, the manganese-iron composite metal oxide material in the heat storage preform sintered in an inert environment is in a reduced state, that is, the main component is manganese monoxide, which does not have thermochemical heat storage performance. Therefore, it is necessary to activate the heat storage preform at high temperature in an oxidizing atmosphere and oxidize it into manganese trioxide with better heat storage performance to improve its initial heat storage performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] Figure 1 : Comparison diagram of the preforms of Examples 1-4 before and after 100 thermal cycles after sintering.
[0034] Figure 2 : Comparison diagram of the preform of Example 5 before and after 100 thermal cycles after sintering.
[0035] Figure 3 : Comparison diagram of the green preform of Example 6 before and after sintering.
[0036] Figure 4 : Comparison of ball impact strength tests of the green preform of Example 7 and the preform of Example 8 after sintering.
[0037] Figure 5 : Comparison diagram of the preform of Example 8 before and after 100 thermal cycles after sintering. DETAILED DESCRIPTION
[0038] The present invention can be implemented by the following specific implementation scheme:
[0039] Example 1
[0040] Use an electronic balance to weigh 37.1g of manganese carbonate and 12.9g of iron oxide powder, add 0.1g of boron nitride to the metal oxide powder and mix evenly, put it into a molding die, make the powder as evenly distributed as possible in the mold, then apply 80MPa of pressure to the powder to demold, and obtain a green preform after demolding. Place the green preform in a sintering furnace and sinter at 1000℃ for 4 hours in a nitrogen atmosphere to obtain a density range of 4.0g / cm 3 The metal oxide-based solid-state heat storage preform was placed in a muffle furnace for activation treatment at 850°C for 20 hours. After 100 thermal cycles, the heat storage preform had no new cracks and was in good structure. The reduction rate and oxidation rate of the heat storage preform material were greater than 89% before and after 100 cycles, and the thermochemical heat storage performance was stable.
[0041] Example 2
[0042] Use an electronic balance to weigh 37.1g of manganese carbonate and 12.9g of iron oxide powder, add 0.1g of boron nitride to the metal oxide powder and mix evenly, put it into a molding die, make the powder as evenly distributed as possible in the mold, then apply 80MPa of pressure to the powder to demold, and obtain a green preform after demolding. Place the green preform in a sintering furnace and sinter at 800℃ for 4 hours in a nitrogen atmosphere to obtain a density range of 3.5g / cm 3 The metal oxide-based solid-state heat storage preform was placed in a muffle furnace for activation treatment at 850°C for 20 hours. After 100 thermal cycles, the heat storage preform had no new cracks and was structurally intact. The reduction rate and oxidation rate of the heat storage preform material were greater than 88% before and after 100 cycles, and the thermochemical heat storage performance was stable.
[0043] Example 3
[0044] Use an electronic balance to weigh 37.1g of manganese carbonate and 12.9g of iron oxide powder, add 0.5g of boron nitride to the metal oxide powder and mix evenly, put it into a molding die, make the powder distribute as evenly as possible in the mold, then apply a pressure of 100MPa to the powder to demold, and obtain a green preform after demolding. Place the green preform in a sintering furnace and sinter at 1000℃ for 4 hours in a nitrogen atmosphere to obtain a density range of 4.8g / cm 3 The metal oxide-based solid-state heat storage preform was placed in a muffle furnace for activation treatment at 850°C for 20 hours. After 100 thermal cycles, the heat storage preform had no new cracks and was structurally intact. The reduction rate and oxidation rate of the heat storage preform material were greater than 85% before and after 100 cycles, and the thermochemical heat storage performance was stable.
[0045] Example 4
[0046] Use an electronic balance to weigh 37.1g of manganese carbonate and 12.9g of iron oxide powder, add 0.1g of boron nitride to the metal oxide powder and mix evenly, put it into a molding die, make the powder as evenly distributed as possible in the mold, then apply 80MPa of pressure to the powder to demold, and obtain a green preform after demolding. Place the green preform in a sintering furnace and sinter at 800℃ for 4 hours in a nitrogen atmosphere to obtain a density range of 4.0g / cm 3 Metal oxide-based solid-state heat storage preforms are not activated. After 100 thermal cycles, there are no new cracks on the thermal preforms, and the structure is intact. The initial reduction rate and oxidation rate are 25%. After 100 cycles, the reaction activity recovers and the reduction rate recovers to about 70%.
[0047] See Example 1-4 for comparison before and after 100 thermal cycles. Figure 1 The left picture shows the state before thermal cycle after sintering, and the right picture shows the state after 100 thermal cycles. In the picture, from left to right and from top to bottom are the preforms of Examples 1-4.
[0048] Example 5 (Comparative Example)
[0049] Use an electronic balance to weigh 37.1g of manganese carbonate and 12.9g of iron oxide powder, add 0.1g of boron nitride to the metal oxide powder and mix evenly, put it into a molding die, make the powder distribute as evenly as possible in the mold, then apply 80MPa of pressure to the powder to demold, and obtain a green preform after demolding. Place the green preform in a sintering furnace and sinter at 800℃ for 4 hours in an air atmosphere to obtain a density range of 3.6g / cm 3 The metal oxide-based solid-state heat storage preform was placed in a muffle furnace for activation treatment at 850°C for 20 hours. After sintering, obvious cracks and depressions appeared on the surface of the heat storage preform (see Figure 2), at which time the reduction rate and oxidation rate reach more than 92%. It can be seen that when sintering in air atmosphere, due to the violent reaction, the mechanical strength after sintering decreases.
[0050] Example 6 (Comparative Example)
[0051] Use an electronic balance to weigh 40.6g of manganese dioxide and 9.4g of iron oxide powder, add 0.1g of boron nitride to the metal oxide powder and mix evenly, then put it into a molding die to make the powder as evenly distributed as possible in the mold, then apply a pressure of 80MPa to the powder to demold it, and after demolding, a green preform is obtained. The green preform is placed in a sintering furnace and sintered at 1000℃ for 4 hours in an air atmosphere. After sintering, the preform disintegrates into powder as shown in the figure. Figure 3 As shown, the left picture is a green preform, and the right picture is after sintering. It can be seen that using manganese dioxide as the raw material, the process of first forming and then sintering cannot obtain a preform that can be formed and used.
[0052] Example 7 (Comparative Example)
[0053] Weigh 69.6g (0.8mol) of reagent-grade manganese dioxide and 16.0g (0.1mol) of reagent-grade iron oxide, place them in a ball mill, and mill them for 30 minutes to fully mix them. Then place the mixture in a muffle furnace and calcine it at 1000℃ for 8h. After cooling down, take it out and grind it to obtain a black powdery heat storage main material Z1 (Mn 0.8 Fe 0.2 )2.
[0054] 50g of the heat storage main material Z1 and 0.1g of boron nitride as an anti-sintering aid were weighed and placed in a ball mill for 30 minutes to fully mix. The mixture was then placed in a muffle furnace and calcined at 800°C for 4 hours to attach the aid to the surface of the heat storage main material, thereby obtaining a modified manganese-iron composite metal oxide heat storage material.
[0055] The modified manganese iron composite metal oxide heat storage material was loaded into a compression mold and distributed as evenly as possible in the mold. Then, a pressure of 100 MPa was applied to the powder until demolding. After demolding, a green preform was obtained. A 5g stainless steel ball was used to hit the surface of the preform from a height of 20 cm. It was observed that the impact force of the small steel ball caused obvious cracks on the surface of the preform, the powder scattered, and the preform disintegrated. It can be seen that the strength of the preform obtained by simple pressing is too low and cannot be used directly (see Figure 4 left).
[0056] Example 8 (Comparative Example)
[0057] The green preform was obtained by the same steps as in Example 7. The green preform was placed in a muffle furnace and calcined at 1000°C for 4 hours. A 5g stainless steel ball was used to hit the surface of the preform from a height of 20cm. The surface did not deform and the structure remained intact (see Figure 4 Right). At this time, the initial reduction rate and oxidation rate are 92%. After 100 cycles, the preform shows obvious expansion, delamination and cracking (see Figure 5 ), at which time the reduction rate and oxidation rate are still higher than 90%. It can be seen that the existing process, which first forms the phase, then shapes and then calcines, is cumbersome, and the mechanical strength is obviously inferior to the process of the present invention.
[0058] The sample activity data of Examples 1-5 and 8 are shown in Table 1
[0059]
[0060]
[0061] Table 1
[0062] The above embodiments are only the best embodiments of the present invention and have no limiting effect on the protection scope of the present invention. All non-substantial changes and adjustments made by technical practitioners in this professional field on the basis of the present invention are within the protection scope claimed by the present invention.
Claims
1. A method for preparing a high-temperature heat storage prefabricated component: It is characterized in that The method comprises the following steps: Step 1: Mix manganese carbonate, iron-based raw materials and active additive powder in a certain proportion and press them into a green preform; Step 2: Sintering and densifying the green preform obtained in step 1 under an inert atmosphere to obtain the high-temperature heat storage preform; Step 3: Activate the high-temperature heat storage preform obtained in step 2 at high temperature in an oxidizing atmosphere.
2. The preparation method according to claim 1, It is characterized in that The sintering temperature of step 2 is 800-1000°C.
3. The preparation method according to claim 1, It is characterized in that The high temperature activation temperature of step three is 850-950°C.
4. The preparation method according to claim 1, It is characterized in that The compression molding method is a molding method.
5. The preparation method according to claim 1, It is characterized in that The iron-based raw material is: iron carbonate, iron oxide or a mixture of the two.
6. The preparation method according to claim 5, It is characterized in that The iron oxide is ferric oxide.
7. The preparation method according to claim 1, It is characterized in that The active auxiliary agent is boron nitride.
8. The preparation method according to claim 1, It is characterized in that The density of the high temperature heat storage preform after densification is in the range of 3.5-4.8 g / cm 3 .
9. The preparation method according to claim 1, It is characterized in that The inert atmosphere is nitrogen, argon or a mixture of the two.
10. The preparation method according to claim 1, It is characterized in that The oxidizing atmosphere is air.
11. A high temperature heat storage prefabricated part, It is characterized in that The high-temperature heat storage preform comprises a heat storage main material and an active auxiliary agent. The heat storage main material is a manganese-iron-based high-temperature metal oxide, which is prepared by the method according to any one of claims 1 to 10.