Method for producing valuable metals

By adjusting the reduction degree based on the cobalt recovery rate and oxygen partial pressure in the recycling of waste lithium-ion batteries, using oxides containing nickel and cobalt as oxidants, the problem of adjusting the reduction degree of alloy is solved, and the recovery rate of valuable metals is improved and reduced. The impurity content achieves efficient metal recycling.

CN117222766BActive Publication Date: 2024-11-29SUMITOMO METAL MINING CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202280029502.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-03-28
Publication Date
2024-11-29
Estimated Expiration
2042-03-28

AI Technical Summary

Technical Problem

In the prior art, when recycling valuable metals in waste lithium-ion batteries, it is difficult to adjust the reduction degree of the alloy appropriately and efficiently, resulting in impurity residues or reduced recovery of the valuable metals.

Method used

The reduction degree is judged based on the cobalt recovery rate during the melting treatment, and if it is judged that it is excessive, the reduction degree is adjusted, and the cobalt grade in the slag and the oxygen partial pressure in the melt are measured. Control cobalt recovery to ensure high recovery and low impurity content of the alloy.

Benefits of technology

The reduction degree of alloy is adjusted appropriately and efficiently in the recycling of waste lithium-ion batteries, the recovery rate of valuable metals is improved, and the content of impurities such as phosphorus is effectively reduced, and the subsequent treatment process is simplified.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117222766B_ABST
    Figure CN117222766B_ABST
Patent Text Reader

Abstract

The present invention provides a method for appropriately and efficiently adjusting the reduction degree of an alloy obtained by melting treatment in a method for producing a valuable metal containing nickel and cobalt from a raw material containing an oxide containing nickel and cobalt. The present invention is a method for producing a valuable metal from a raw material containing an oxide containing nickel and cobalt, comprising: a melting step, in which the raw material is subjected to a melting treatment to obtain a melt; and a slag separation step, in which slag is separated from the melt and an alloy containing the valuable metal is recovered. In the melting step, the reduction degree in the melting treatment is determined based on the ratio of the amount of cobalt in the generated alloy to the amount of cobalt in the raw material (cobalt recovery rate), and when it is determined that the reduction degree is excessive, a raw material containing an oxide containing nickel and cobalt is added as an oxidant.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a method for producing valuable metals from a raw material containing oxides containing nickel and cobalt, such as waste lithium ion batteries. Background Art

[0002] In recent years, lithium-ion batteries have become popular as secondary batteries with light weight and high output. As lithium-ion batteries, a negative electrode material having a negative electrode active material such as graphite fixed to a negative electrode collector made of copper foil, a positive electrode material having a positive electrode active material such as lithium nickel oxide or lithium cobalt oxide fixed to a positive electrode collector made of aluminum foil, a separator made of a porous resin film of polypropylene, and a lithium hexafluorophosphate (LiPF4)-containing electrolyte are known. 6 ) or other electrolytes sealed in a lithium-ion battery.

[0003] One of the main uses of lithium-ion batteries is hybrid vehicles or electric vehicles. It is foreseeable that as the life cycle of the vehicle ends, the lithium-ion batteries carried by it will also be discarded in large quantities. Many proposals have been made to reuse such used batteries or defective products generated during manufacturing (hereinafter referred to as "wasted lithium-ion batteries") as resources. For example, as a method for recycling waste lithium-ion batteries, a dry smelting process has been proposed that uses a high-temperature furnace to melt all the waste lithium-ion batteries.

[0004] In addition to valuable metals such as nickel (Ni), cobalt (Co), and copper (Cu), waste lithium-ion batteries also contain impurities such as carbon (C), aluminum (Al), fluorine (F), and phosphorus (P). Therefore, when recovering valuable metals from waste lithium-ion batteries, these impurities need to be removed.

[0005] In the dry smelting process, raw materials including waste lithium-ion batteries are melted at a temperature of about 1500°C and then separated into metal and slag. In this process, valuable substances contained in the raw materials can be reduced and recovered in the form of metals, and impurities can be oxidized and separated into slag, thereby being removed.

[0006] However, if the reduction degree is adjusted to be too strong in order to increase the recovery rate of valuable metals such as cobalt, impurities such as phosphorus will not be oxidized and removed and will remain in the metal. On the other hand, if the reduction degree is adjusted to be too weak, the valuable metals will also be oxidized, reducing the recovery rate. In addition, for example, in the case of over-reduction, it is considered to adjust the reduction degree by blowing in oxygen or other gases for oxidation, but it is necessary to blow gas into the melt, which requires cost.

[0007] Therefore, in order to effectively remove impurities during the melt treatment and recover valuable metals at a high recovery rate, it is desired to appropriately and economically and efficiently adjust the reduction degree of the obtained alloy (metal).

[0008] It should be noted that Patent Document 1 discloses a technology for recovering valuable metals containing nickel and cobalt from waste lithium-ion batteries, etc., by performing dephosphorization without adversely affecting the recovery rate of the valuable metals, thereby recovering the valuable metals at a high recovery rate. However, the technology does not disclose the adjustment of the reduction degree of the obtained alloy.

[0009] Prior art literature

[0010] Patent Literature

[0011] Patent Document 1: Japanese Patent Application Publication No. 2013-091826. Summary of the invention

[0012] Problem that the invention aims to solve

[0013] The present invention is proposed based on the above-mentioned actual situation, and its purpose is to provide a method for appropriately and efficiently adjusting the reduction degree of the alloy obtained by melt treatment in a method for producing valuable metals containing nickel and cobalt from raw materials containing oxides containing nickel and cobalt such as the above-mentioned waste lithium-ion batteries.

[0014] Means used to solve problems

[0015] The inventors of the present invention have conducted intensive research to solve the above-mentioned problems. As a result, they have found that in the process of obtaining a melt by melting a raw material containing oxides containing nickel and cobalt, such as a waste lithium-ion battery, the degree of reduction in the melting process is determined based on the cobalt recovery rate. When it is determined that the degree of reduction is excessive, a raw material containing oxides containing nickel and cobalt is added as an oxidant, thereby appropriately and efficiently adjusting the degree of reduction. The present invention has been completed.

[0016] (1) The first invention of the present invention is a method for producing valuable metals from a raw material containing oxides containing nickel and cobalt, wherein the method comprises: a melting step of subjecting the raw material to a melting treatment to obtain a molten material; and a slag separation step of separating slag from the molten material and recovering an alloy containing valuable metals, wherein in the melting step, the degree of reduction in the melting treatment is determined based on the ratio of the amount of cobalt in the generated alloy to the amount of cobalt in the raw material (cobalt recovery rate), and when it is determined that the degree of reduction is excessive, the raw material containing oxides containing nickel and cobalt is added as an oxidant.

[0017] (2) A second aspect of the present invention is a method for producing valuable metals according to the first aspect, wherein in the melting step, the cobalt recovery rate is calculated based on an analysis result of the cobalt grade in the slag.

[0018] (3) A third aspect of the present invention is a method for producing valuable metals according to the first aspect, wherein in the melting step, the cobalt recovery rate is calculated based on a measurement result of an oxygen partial pressure in a melt generated by a melting treatment.

[0019] (4) A fourth invention of the present invention is a method for producing valuable metals according to any one of the first to third inventions, wherein in the melting step, when the cobalt recovery rate is 98% or more, it is determined that the reduction degree in the melting treatment is excessive.

[0020] (5) A fifth invention of the present invention is a method for producing a valuable metal, wherein in any one of the first to fourth inventions, the raw material containing an oxide containing nickel and cobalt is a raw material containing waste lithium-ion batteries.

[0021] (6) A sixth invention of the present invention is a method for producing valuable metals, wherein in any one of the first to fifth inventions, the raw material contains phosphorus, and the phosphorus content of the alloy recovered through the slag separation step is 0.1 mass % or less.

[0022] (7) A seventh invention of the present invention is a method for producing a valuable metal according to any one of the first to sixth inventions, wherein in the melting step, the raw material is melted at a heating temperature of 1300° C. or higher and 1600° C. or lower.

[0023] Effects of the Invention

[0024] According to the present invention, the reduction degree of the alloy obtained by the melt treatment can be appropriately and efficiently adjusted. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 This is a process diagram showing an example of the flow of a method for producing valuable metals.

[0026] Figure 2 This is a graph showing the relationship between the cobalt grade in the slag and the cobalt recovery rate.

[0027] Figure 3 This is a graph showing the relationship between the oxygen partial pressure in the melt and the cobalt recovery rate.

[0028] Figure 4 It is a graph showing the relationship between the cobalt recovery rate and the phosphorus grade in the metal, and is a graph for explaining the adjustment of the reduction degree in the smelting process. DETAILED DESCRIPTION

[0029] Hereinafter, an embodiment of the present invention (hereinafter referred to as "this embodiment") will be described. It should be noted that the present invention is not limited to the following embodiment, and various modifications can be made within the scope of the gist of the present invention.

[0030] 《1. Method for producing valuable metals》

[0031] The method for producing valuable metals of the present embodiment is a method for separating and recovering valuable metals from a raw material containing oxides containing at least nickel and cobalt. Therefore, it can also be called a method for recovering valuable metals. The method of the present embodiment is mainly based on a dry smelting process, but can also be composed of a dry smelting process and a wet smelting process.

[0032] As a “raw material containing oxides containing nickel and cobalt”, for example, there can be cited a raw material containing waste lithium-ion batteries. The positive electrode material constituting the lithium-ion battery contains oxides of nickel and cobalt. It should be noted that “waste lithium-ion batteries” refers to the concept of waste materials in the manufacturing process of lithium-ion batteries, including not only used lithium-ion batteries, but also defective products generated in the manufacturing process of the positive electrode material constituting the battery, residues within the manufacturing process, and waste generated. Therefore, waste lithium-ion batteries can also be referred to as lithium-ion battery waste.

[0033] In addition, "valuable metals" that can be recovered from raw materials containing oxides containing nickel and cobalt refer to at least nickel (Ni) and cobalt (Co). For example, when the raw material is a raw material containing waste lithium-ion batteries, as valuable metals, in addition to nickel and cobalt, copper (Cu) and the like can also be cited. Further, alloys composed of a combination of nickel, cobalt and copper can be cited. It should be noted that there is no particular limitation on the content of each valuable metal contained in the waste lithium-ion batteries. For example, it may also contain more than 10% by mass of copper.

[0034] Specifically, the method for producing valuable metals of the present embodiment comprises at least: a melting step, in which a raw material containing oxides containing nickel and cobalt is subjected to a melting treatment to obtain a melt; and a slag separation step, in which slag is separated from the melt and an alloy containing valuable metals is recovered. Moreover, in the method, it is characterized in that in the melting step, the degree of reduction in the melting treatment is judged based on the cobalt recovery rate, and when it is judged that the reduction is excessive, a raw material containing oxides containing nickel and cobalt is added as an oxidant. Here, the "cobalt recovery rate" refers to the ratio (percentage) of the amount of cobalt in the alloy generated and recovered by the treatment to the amount of cobalt in the raw material.

[0035] The cobalt recovery rate can be calculated based on, for example, the analysis results of the cobalt grade in the slag, or can also be calculated based on the measurement results of the oxygen partial pressure in the melt generated by melting the raw materials.

[0036] As described above, in the method of the present embodiment, the cobalt recovery rate is calculated from the slag, alloy, or melt containing them obtained by the melting treatment, and the degree of reduction is determined based on the cobalt recovery rate.

[0037] Furthermore, in this method, when it is determined that the degree of reduction that can be determined based on the cobalt grade in the slag is in an excessive state, that is, when it is over-reduced, an oxidant is added to adjust the degree of reduction, and as the reducing agent added at this time, a raw material containing an oxide containing nickel and cobalt as a raw material to be processed is used. Specifically, for example, when a raw material containing waste lithium ion batteries is used as a raw material for melting treatment, the raw material containing waste lithium ion batteries is used as the oxidant added when it is determined to be over-reduced.

[0038] According to this method, the degree of reduction can be properly grasped in the melt treatment, and an oxidant can be appropriately added based on the degree of reduction, so that the degree of reduction can be adjusted. Thus, valuable metals can be recovered at a high recovery rate, and metals with effectively reduced content of impurities such as phosphorus can be obtained. In addition, as an oxidant added when adjusting the degree of reduction, since a raw material containing an oxide containing nickel and cobalt (for example, a raw material containing waste lithium-ion batteries) is added, not only the degree of reduction can be effectively adjusted, but also the amount of metal recovery can be increased because it is an oxidant containing valuable metals as the recovery object.

[0039] Hereinafter, the method for producing valuable metals will be described in more detail by taking as an example the case where a raw material including waste lithium-ion batteries is used as the raw material containing an oxide containing nickel and cobalt.

[0040] 《2. About each step of the manufacturing method》

[0041] Figure 1 1 is a process diagram showing an example of the process of the method for producing valuable metals according to the present embodiment. Figure 1 As shown, the method for producing valuable metals is a method for producing valuable metals from raw materials containing waste lithium-ion batteries, comprising: a waste battery pretreatment step S1, removing the electrolyte and outer can of the waste lithium-ion batteries; a crushing step S2, crushing the contents of the battery to form a crushed material; a preheating step (also called an "oxidation roasting step") S3, preheating the crushed material as needed; a melting step (also called a "reduction melting step") S4, melting the crushed material to obtain a molten material; and a slag separation step S5, separating the slag from the molten material and recovering an alloy containing valuable metals.

[0042] [Waste battery pre-treatment process]

[0043] The waste battery pretreatment step S1 is performed for the purpose of preventing explosion of the waste lithium ion batteries, rendering them harmless, removing the outer cans, etc. when recovering valuable metals from the waste lithium ion batteries.

[0044] That is, waste lithium-ion batteries such as used lithium-ion batteries are closed systems and contain electrolytes, etc., so there is a risk of explosion when they are crushed in their original state. Therefore, it is necessary to implement discharge treatment and electrolyte removal treatment by some method. In this way, in the waste battery pre-treatment step S1, by removing the electrolyte and the outer can, safety can be improved, and the recovery productivity of valuable metals such as copper, nickel, and cobalt can be improved.

[0045] The specific method of pretreatment is not particularly limited, for example, the battery can be physically perforated with a needle-shaped knife tip to allow the electrolyte inside to flow out and be removed. Alternatively, the waste lithium-ion battery can be directly heated to burn the electrolyte for harmless treatment.

[0046] It should be noted that the outer cans constituting the battery are mostly composed of metal aluminum, iron, etc., and through such pre-treatment, the metal outer cans can be directly recycled as valuable metals relatively easily. For example, in the case of recycling aluminum and iron contained in the outer can, it is possible to use a vibrating screen machine to screen after the removed outer can is crushed. In the case of aluminum, even a slight crushing can easily become a powder, so that it can be effectively recovered. In addition, it is also possible to screen by magnetic force to recover the iron contained in the outer can.

[0047] [Crushing process]

[0048] In the crushing step S2, the battery contents obtained in the waste battery pretreatment step S1 are crushed to obtain a crushed product. The crushing step S2 is performed for the purpose of improving the reaction efficiency in the dry smelting process after the next step. By improving the reaction efficiency, the recovery rate of valuable metals such as copper, nickel, and cobalt can be improved.

[0049] The pulverization method is not particularly limited, and the contents of the battery can be pulverized using a conventionally known pulverizer such as a cutter mixer.

[0050] [Preheating process]

[0051] If necessary, a preheating step S3 can be provided to heat the pulverized waste lithium ion battery after the pulverizing step S2 (oxidative calcination). By performing the heating treatment in the preheating step S3, impurities contained in the battery contents can be volatilized or thermally decomposed and removed.

[0052] In the preheating step S3, for example, heating is preferably performed at a temperature (preheating temperature) of 700° C. or higher. By setting the preheating temperature to 700° C. or higher, the removal efficiency of impurities contained in the battery can be improved. On the other hand, the upper limit of the preheating temperature is preferably 900° C. or lower, thereby suppressing the thermal energy cost and improving the processing efficiency.

[0053] The heat treatment is preferably carried out in the presence of an oxidizing agent. Thus, carbon in the impurities contained in the contents of the battery can be oxidized and removed, and aluminum can also be oxidized. In particular, by removing carbon by oxidation, the molten particles of the valuable metals locally produced in the subsequent melting step S4 can agglomerate without physical obstacles caused by carbon, so the alloy obtained as a melt can be easily recovered in an integrated manner. It should be noted that, generally, due to differences in affinity with oxygen, the main elements constituting waste lithium-ion batteries are easily oxidized in the order of aluminum>lithium>carbon>manganese>phosphorus>iron>cobalt>nickel>copper.

[0054] There is no particular limitation on the oxidant, and from the aspect of easy handling, preferably oxygen-containing gases such as air, pure oxygen, and oxygen-enriched gas are used. In addition, the amount of the oxidant introduced, for example, can be set to about 1.2 times the chemical equivalent required for the oxidation of each substance as the oxidation treatment object.

[0055] [Melting process]

[0056] In the melting step (reduction melting step) S4, the crushed waste lithium ion battery is melted together with a flux to obtain a melt consisting of an alloy containing valuable metals and slag. As a result, impurity elements such as aluminum are contained in the slag as oxides, and phosphorus is also mixed in the flux and contained in the slag. On the other hand, valuable metals such as copper that are difficult to form oxides can be melted and recovered as an alloy integrated by the melt.

[0057] As the flux, it is preferred to include an element that can form a basic oxide with a low melting point by incorporating the impurity element. Among them, it is more preferred to include a calcium compound because it is inexpensive and stable at room temperature. Since phosphorus, which is an impurity element, turns into an acidic oxide when oxidized, the stronger the alkalinity of the slag formed by the melting treatment, the easier it is for phosphorus to be incorporated into the slag.

[0058] As the calcium compound, for example, calcium oxide or calcium carbonate can be added. In addition, as the amount of calcium added, Al 2 O 3 -CaO-Li 2 Since the O-based slag is a slag-based slag, it is preferable to add an appropriate amount of alumina in the sample to melt the alumina by eutecticization, that is, CaO / (Al 2 O 3 +CaO)=amount of 0.15 or more.

[0059] In order to appropriately adjust the degree of redox when melting the waste lithium ion batteries, the melting step S4 may be performed in the presence of an oxidizing agent or a reducing agent.

[0060] As the oxidant, a known oxidant can be used, a solid oxidant can be added, or a gaseous oxidant can be introduced into the furnace. In addition, as the reducing agent, a known reducing agent can also be used, preferably a reducing agent containing carbon atoms. By adding a reducing agent containing carbon atoms to the waste lithium ion battery, the oxides of valuable metals such as copper, nickel, and cobalt contained in the waste lithium ion battery as the recovery object can be easily reduced.

[0061] Specifically, as an example of a reducing agent containing carbon atoms, graphite can be cited, which can reduce 2 moles of oxides of valuable metals such as copper oxide or nickel oxide using 1 mole of carbon. In addition, hydrocarbons that can reduce 2 to 4 moles of valuable metal oxides per 1 mole of carbon or carbon monoxide that can reduce 1 mole of valuable metal oxides per 1 mole of carbon can also be added as a source of carbon. As described above, by performing a reduction melting treatment in the presence of carbon as a reducing agent, valuable metals can be efficiently reduced, and alloys containing valuable metals can be obtained more effectively. In addition, compared with the case of aluminothermic reaction in which metal powder such as aluminum is used as a reducing agent for reduction, the reduction treatment using carbon has the advantage of being very safe.

[0062] It should be noted that when carbon is added as a reducing agent, an excessive amount of carbon may be added. When the amount of carbon added is too much, in the case where the waste lithium ion battery contains a phosphorus compound, there is a possibility that phosphorus is reduced by the carbon and included in the alloy phase. However, by adding an oxidant as needed and melting the waste lithium ion battery in the presence of a flux, phosphorus can be removed by mixing it into the flux.

[0063] When heating in the melting process, at the stage of reaching the heating temperature, the fluidity of the melt is low and there is a molten residue, so, for example, it is necessary to keep the heating temperature for more than 30 minutes. It should be noted that it is preferred to finally observe the inside of the crucible and confirm whether it has completely become a melt with an iron measuring rod. After melting, the alloy in the molten state with high fluidity and the slag are separated in the crucible according to their specific gravity in a way that the lower layer is metal and the upper layer is slag. At this time, after collecting the supernatant slag using an iron measuring rod, it is cooled and crushed.

[0064] Here, in the manufacturing method of the valuable metal of the present embodiment, the reduction degree in the smelting treatment is determined based on the ratio of the amount of cobalt in the alloy generated and recovered by the treatment to the amount of cobalt in the raw material, that is, the cobalt recovery rate. And, for example, when the cobalt recovery rate is 98% or more, it can be determined that the reduction degree in the smelting treatment is excessive.

[0065] (First method related to calculation of cobalt recovery rate)

[0066] The cobalt recovery rate can be calculated based on the analysis results of the cobalt grade in the generated slag as a first aspect.

[0067] Figure 2 is a graph showing the relationship between the cobalt grade in the slag and the cobalt recovery rate. Figure 2 As shown in the figure, there is a proportional relationship between the cobalt grade in the slag and the cobalt recovery rate. The flux, such as the amount of calcium, added according to the composition of the waste lithium-ion battery as the raw material is determined to be an appropriate amount for melting. Therefore, if the composition of the waste lithium-ion battery as the raw material is determined, the amount of slag generated is determined, and the slope and intercept of the proportional relationship are also determined. Therefore, based on such a proportional relationship, the cobalt recovery rate can be effectively calculated according to the analysis results of the cobalt grade in the slag.

[0068] As described above, the slag generated by the melting process is used to rapidly (for example, within 8 minutes) analyze the cobalt grade in the slag using an analysis device such as a fluorescent X-ray analyzer. Thus, the cobalt recovery rate can be calculated.

[0069] Alternatively, the amount of cobalt in the metal can be calculated based on the amount of cobalt in the inputted waste lithium-ion batteries and the amount of cobalt in the slag obtained from the cobalt grade in the slag generated by the smelting process and the amount of slag generated, thereby calculating the cobalt recovery rate. It should be noted that the amount of slag is calculated by assuming that all nickel, cobalt, and copper allocated to the metal are subtracted from the amount of inputted waste lithium-ion batteries, and the remaining elements become oxides, and the added flux is added to the slag as calcium oxide.

[0070] (Second method related to calculation of cobalt recovery rate)

[0071] The cobalt recovery rate can be calculated based on the measurement result of the oxygen partial pressure of the melt (molten material) generated by the melt treatment as a second aspect.

[0072] Figure 3 Graph showing the relationship between oxygen partial pressure in the melt and cobalt recovery rate. Figure 3 As shown, there is a one-to-one correspondence between the oxygen partial pressure in the melt and the cobalt recovery rate. It can be seen that the cobalt recovery rate corresponding to the oxygen partial pressure can be obtained by measuring the oxygen partial pressure in the melt.

[0073] The method for measuring the oxygen partial pressure in the melt is not particularly limited as long as it is a method that can directly measure the oxygen partial pressure in the melt. For example, a method of measuring by inserting an oxygen analyzer in an oxygen sensor (oxygen probe) in such a way that the front end of the oxygen sensor is immersed in the melt can be cited. It should be noted that as the oxygen sensor, a known sensor such as a zirconium oxide solid electrolytic sensor can be used.

[0074] For example, refer to Figure 3 When the oxygen partial pressure in the melt is 10 -14 atm, the cobalt recovery rate is greater than 98%. When the oxygen partial pressure in the melt is 10 -12 Atm or above, the cobalt recovery rate is less than 95%.

[0075] Thus, the oxygen partial pressure in the melt is controlled to be greater than 10 -12 atm and less than 10 -14 Atm range is adjusted based on the cobalt recovery rate to adjust the reduction degree, thereby, as described later Figure 4 The relationship shown can effectively and efficiently remove phosphorus while recovering cobalt at a high recovery rate, and can recover a high-quality alloy with a reduced phosphorus content. It should be noted that according to the above relationship, the target metal can also be effectively obtained by controlling the oxygen partial pressure in the melt.

[0076] (Determination and control of reduction degree based on calculated cobalt recovery rate)

[0077] When the cobalt recovery rate is calculated based on the measurement results of the cobalt grade in the slag and the measurement results of the oxygen partial pressure of the melt in the above manner, the reduction degree in the smelting process is determined based on the cobalt recovery rate. Specifically, for example, the reduction degree is determined by confirming whether the cobalt recovery rate is in the range of 95% or more and 98% or less.

[0078] The present inventors have found that there is a relationship between the recovery rate of cobalt from raw materials including waste lithium-ion batteries and the grade of impurity phosphorus (P) contained in the recovered alloy (metal). Specifically, Figure 4 This is a graph showing the relationship between the cobalt recovery rate and the phosphorus grade in the metal (alloy). Figure 4 As shown in the figure, it can be seen that when the cobalt recovery rate exceeds 98%, the phosphorus grade in the recovered metal increases sharply. It should be noted that the recovery rate of cobalt as a valuable metal is preferably 95% or more.

[0079] Thus, it is confirmed whether the calculated cobalt recovery rate is within the range of 95% to 98%, and the melting process is terminated after confirming that it is within the range, so that the phosphorus content in the alloy (metal) recovered later can be 0.1% by mass or less. Thus, phosphorus can be effectively and efficiently removed while recovering cobalt at a high recovery rate, and a high-quality alloy with a reduced phosphorus content can be recovered without the need to set up a separate dephosphorization process after recovering the alloy.

[0080] On the other hand, when the calculated cobalt recovery rate is 98% or more, it can be judged that the degree of reduction in the smelting process is in an excessive state, that is, it is judged to be over-reduction. When the cobalt recovery rate is 98% or more, as shown in this value, although the effect is good in the recovery of cobalt, the distribution ratio of impurities such as phosphorus in the metal also increases.

[0081] In the method of the present embodiment, it is important to judge the reduction degree in the smelting process based on the obtained cobalt recovery rate. And, for example, when the calculated cobalt recovery rate is 98% or more, it can be judged that the reduction degree is excessive, and the reduction degree of the smelting process can be appropriately adjusted based on this judgment.

[0082] Specifically, when the calculated cobalt recovery rate deviates from the range of 95% to 98% or deviates from the specified target value even if it is within the range of 95% to 98%, if the cobalt grade in the slag is low, an oxidant is added as needed, and although a part of the cobalt in the metal is distributed to the slag, the phosphorus in the metal can be distributed to the slag. On the contrary, if the cobalt grade in the slag is high, a reducing agent is added, and although a part of the phosphorus in the slag is distributed to the metal, the cobalt in the slag can be distributed to the metal, thereby improving the recovery rate.

[0083] In this way, whether or not the reduction degree is appropriate can be effectively determined based on the cobalt recovery rate, and the oxidizing agent and the reducing agent can be added as necessary to control the melt treatment.

[0084] Here, when the calculated cobalt recovery rate is 98% or more, the reduction degree is excessive, that is, the obtained metal is over-reduced, and the phosphorus content in the metal increases. Therefore, it is necessary to add an oxidant to adjust the reduction degree. At this time, in the method of this embodiment, as the oxidant, a raw material containing oxides of nickel and cobalt is used as the oxidant. Specifically, as the raw material containing oxides of nickel and cobalt, a raw material containing waste lithium ion batteries is used as the oxidant.

[0085] Thus, the degree of reduction can be appropriately adjusted and impurities such as phosphorus in the metal can be effectively oxidized and removed into the slag, and nickel and cobalt in the raw materials used as oxidants (including raw materials of waste lithium-ion batteries) can be reduced to metal form for recovery.

[0086] Generally, in the melt treatment, since excessive carbon is added as described above, the frequency of adding an oxidant when adjusting the reduction degree increases. In this case, by using a raw material containing nickel and cobalt oxides as an oxidant, an appropriate reduction degree can be adjusted, and the nickel and cobalt contained in the oxidant can also be recovered together, thereby increasing the amount of metal recovered.

[0087] The amount of the oxidant used when adjusting the reduction degree may be set to an amount required to completely oxidize the phosphorus in the metal, for example, by estimating the phosphorus grade in the metal based on the cobalt recovery rate calculated from the cobalt grade in the slag.

[0088] Specifically, for example, when the metal amount is estimated to be 100 g and the phosphorus grade is 0.2 mass %, the amount of phosphorus in the metal is 0.2 g, and the oxidant is Ni 2 O 3 When the oxidation efficiency is 100%, P+5 / 6Ni 2 O 3 =1 / 2P 2 O 5 +5 / 3Ni reaction is established, so the oxidant Ni 2 O 3 The amount of addition is 0.89 g. In addition, assuming that the oxidant is Co 2 O 3 When the oxidation efficiency is 100%, P+5 / 6Co 2 O 3 =1 / 2P 2 O 5 +5 / 3Co reaction is established, so the oxidant Co 2 O 3 The added amount is 0.89 g. The added amount in the example is the amount when the reaction efficiency is set to 100%. However, since there is also an oxidation reaction of cobalt in the metal, it is preferred that the phosphorus in the metal is The reaction efficiency is set to be 30% or more and 90% or less, and the actual addition amount is set to keep the time for 5 minutes or more and 30 minutes or less. In addition, when using a reducing agent containing carbon atoms, there is also a reduction reaction of phosphorus in the slag. Therefore, it is preferred to set the addition amount of the reducing agent to 50%. +CO 2 The reaction efficiency was determined by setting it to 30% or more and 70% or less.

[0089] As described above, as the oxidant used when adjusting the reduction degree, a raw material containing oxides of nickel and cobalt, that is, a raw material containing waste lithium ion batteries, is used. In this case, an oxide (oxide from waste lithium ion batteries) obtained by oxidative roasting of waste lithium ion batteries at 700°C to 900°C is used. It should be noted that the Ni contained in the oxide from waste lithium ion batteries 2 O 3 0% or more and 85% or less, Co 2 O 3 In fact, it is preferred that the Ni content of the oxide be 0% or more and 85% or less. 2 O 3 and Co 2 O 3 The amount of oxide added is set based on the analytical value.

[0090] In addition, as the oxidant, not only waste lithium-ion batteries but also positive electrode materials separated from waste lithium-ion batteries (for example, NCA (nickel-cobalt-aluminum lithium-ion battery) waste) can be used. 2 O 3 0% or more and 85% or less, Co 2 O 3 In this case, the amount of impurities such as aluminum and phosphorus mixed from raw materials other than the positive electrode material can be suppressed, which is preferable.

[0091] It should be noted that when adjusting the reduction degree, it is not limited to using only an oxidant for adjustment as described above, and a reducing agent may also be added in combination. Specifically, as a reducing agent, a material with a high carbon grade (graphite powder, graphite particles, coal, coke, etc.) and carbon monoxide can be used for adjustment. In addition, as a reducing agent, a component with a high carbon grade in the raw material can also be used.

[0092] The heating temperature (melting temperature) in the melting treatment is not particularly limited, but is preferably set to be above 1300°C, and more preferably set to be above 1350°C. By performing the melting treatment at a temperature above 1300°C, valuable metals such as copper, cobalt, and nickel are efficiently melted, and alloys are formed in a state where the fluidity is sufficiently improved. Therefore, the separation efficiency of the valuable metals and impurity components in the slag separation step S5 described later can be improved. It should be noted that when the heating temperature is less than 1300°C, the separation efficiency of the valuable metals and impurities may be insufficient.

[0093] The upper limit of the heating temperature in the melting process is preferably 1600° C. or lower. When the heating temperature is higher than 1600° C., thermal energy is wasted, and refractory materials such as crucibles and furnace walls are consumed more intensively, which may reduce productivity.

[0094] During the melting process, dust, exhaust gas, etc. may be generated, but these can be rendered harmless by performing conventionally known exhaust gas treatment.

[0095] [Slag separation process]

[0096] In the slag separation step S5, after the melt obtained in the melting step S4 is solidified, slag is separated from the solidified melt and an alloy containing valuable metals is recovered. The slag and alloy contained in the solidified melt are separated due to the difference in specific gravity, so the slag and the alloy can be recovered separately.

[0097] Here, the treatment in the smelting process when each valuable metal is produced from an alloy containing valuable metals can be carried out by a known method such as a neutralization treatment and a solvent extraction treatment, without particular limitation. For example, in the case of an alloy composed of cobalt, nickel, and copper, after the valuable metals are leached with an acid such as sulfuric acid (leaching process), the residual nickel and cobalt solution can be discharged to the positive electrode active material production process in the battery manufacturing process for utilization by, for example, extracting copper by solvent extraction or the like (extraction process).

[0098] In the method of the present embodiment, as described above, in the melting step S4, the reduction degree of the melting treatment is confirmed based on the ratio of the amount of cobalt in the generated alloy to the amount of cobalt in the raw material (cobalt recovery rate). Then, for example, after confirming that the calculated cobalt recovery rate is 95% or more and 98% or less, the melting treatment is terminated, and then the alloy (metal) is separated from the slag in the slag separation step S5. Thus, the phosphorus content is effectively reduced, and specifically, an alloy with a phosphorus content of 0.1% by mass or less can be recovered.

[0099] On the other hand, when the smelting treatment is judged to be over-reduction based on the cobalt grade in the slag, for example, when the cobalt recovery rate calculated based on the cobalt grade is 98% or more and it is judged to be over-reduction, a raw material containing oxides of nickel and cobalt (including a raw material of waste lithium-ion batteries) is added as an oxidant to adjust the degree of reduction.

[0100] The cobalt recovery rate can be calculated based on the analysis results of the cobalt grade in the slag. Alternatively, the cobalt recovery rate can be calculated based on the measurement results of the oxygen partial pressure in the melt generated by the melt treatment.

[0101] According to the method of this embodiment, in the process of melting the waste lithium-ion battery, an alloy containing a valuable metal with phosphorus removed can be efficiently obtained, and the smelting process when each valuable metal is manufactured from the alloy containing the valuable metal can be simplified. That is, there is no need to set a process for dephosphorizing the obtained alloy containing the valuable metal. In addition, since the raw material is used as an oxidant added when the reduction degree is excessive, the valuable metal contained in the raw material can also be recovered together. That is, the valuable metal can be recovered with higher efficiency.

[0102] Example

[0103] Hereinafter, the present invention will be described in more detail with reference to examples, but the present invention is not limited to the following examples.

[0104] [Recycling of valuable metals]

[0105] (Waste battery pre-treatment process)

[0106] First, as waste lithium-ion batteries, used batteries of 18650 cylindrical batteries, vehicle-mounted square batteries, and defective batteries recovered in the battery manufacturing process were prepared. Then, the waste lithium-ion batteries were immersed in salt water and discharged, and the water was dispersed and roasted in the air at a temperature of 260°C to decompose and remove the electrolyte and the outer can to obtain the battery contents. The main element composition of the battery contents is shown in Table 1 below.

[0107] Table 1

[0108]

[0109] (Crushing process)

[0110] Then, the battery contents were pulverized using a pulverizer (trade name: GOOD CUTTER, manufactured by Ujiie Manufacturing Co., Ltd.) to obtain a pulverized product.

[0111] (Preheating process)

[0112] Then, the obtained pulverized product was placed in a rotary kiln and preheated at a preheating temperature of 800° C. for 180 minutes in the atmosphere.

[0113] (Melting process)

[0114] The oxide of the waste lithium ion battery was melted under the conditions shown in Table 2. Then, the cobalt recovery rate was estimated to be 99.9% based on the cobalt grade of 0.01 mass % in the slag obtained first, and the phosphorus grade in the metal was estimated to be 0.6 mass % based on the estimated cobalt recovery rate.

[0115] In addition, the oxygen partial pressure in the melt at this time was measured. As a result, the measured value of the oxygen partial pressure was 10 -15 atm, and the cobalt recovery rate can be estimated to be 99.9% based on the result of the oxygen partial pressure. It should be noted that in the measurement of the oxygen partial pressure, an oxygen analyzer having an oxygen probe (manufactured by Kawase Electric Industry Co., Ltd., OXT-O) at the front end is used, and the probe is inserted in a manner that the front end of the oxygen probe is directly immersed in the melt, and the measured value is read after the measured value is stabilized. The oxygen probe has a zirconium oxide solid electrolytic sensor.

[0116] According to the estimated phosphorus content in the metal, for every 100 g of metal, 0.89 g of Ni as an oxidant is required for every 0.2 mass% phosphorus content. 2 O 3 , 0.89 g of Co is required 2 O 3 Therefore, relative to the metal amount of 2120g, due to the Ni contained in the oxide from NCA (nickel cobalt aluminum lithium ion battery) waste 2 O3 77% by mass Co 2 O 3 The amount of oxide from NCA waste required to achieve a phosphorus oxidation efficiency of 100% is 8 mass %, so 66.6 g of oxide from NCA waste is required. Here, when the reduction degree is actually adjusted, the oxidation efficiency is taken into consideration, and in order to reliably remove phosphorus, 2.4 times the amount, that is, 160 g of oxide from NCA waste is added as an oxidant at a reaction efficiency of 42% to adjust the reduction degree.

[0117] (Slag separation process)

[0118] The melt after the melting treatment is poured into a mold using the difference in specific gravity, and is separated into metal and slag. The slag is separated from the solidified melt to recover the alloy.

[0119] The slag from which the alloy was recovered was subjected to elemental analysis using an ICP analyzer (Agilent Technologies, Inc., Agilent 5100SUDV)), and the amounts of cobalt and phosphorus were determined as ratios (mass %) relative to the total mass of the slag.

[0120] In addition, the alloy after separation of the slag was also subjected to elemental analysis using an ICP analyzer (Agilent Technologies, Inc., Agilent 5100SUDV)) to measure the amounts of cobalt and phosphorus, and to determine the cobalt recovery rate from the battery and the phosphorus grade in the alloy.

[0121] [result]

[0122] Table 2 below shows the recovery rate of cobalt from waste lithium-ion batteries relative to the total mass of slag and the measurement results of the phosphorus grade in the alloy.

[0123]

[0124] According to the results shown in Table 2, for the alloy obtained in the example, the recovery rate of cobalt as a valuable metal contained in the battery is 95% or more, and the phosphorus grade in the obtained alloy is 0.01 mass % or less, and a good result is obtained. That is, the reduction degree during reduction melting can be appropriately adjusted based on the cobalt recovery rate calculated from the results of the cobalt grade in the slag of the waste lithium ion battery in a molten state, so that the target metal can be obtained.

[0125] In addition, at an oxygen partial pressure of 10 -15 Atm, the cobalt recovery rate was 99.9%, and at an oxygen partial pressure of 10 -12.8 atm, the cobalt recovery rate was 96.4%, indicating that there is a relationship between oxygen partial pressure and cobalt recovery rate. Figure 3Therefore, it can be seen that the cobalt recovery rate can be calculated based on the oxygen partial pressure of the melt, and the target metal can be obtained based on the cobalt recovery rate. It should be noted that, according to such results, the target metal can also be obtained by controlling the oxygen partial pressure.

[0126] In addition, at this time, since the NCA scrap is used as an oxidant for adjusting the degree of reduction, the amount of metal recovered can also be increased.

Claims

1. A method for producing a valuable metal, which is a method for producing a valuable metal from a raw material containing an oxide containing nickel and cobalt, wherein: The method for producing the valuable metal comprises: a melting step of melting the raw materials to obtain a melt; and a slag separation step of separating slag from the melt and recovering an alloy containing valuable metals, In the melting step, the degree of reduction in the melting treatment is determined based on the mass percentage of the amount of cobalt in the generated alloy relative to the amount of cobalt in the raw material, that is, the cobalt recovery rate. When the cobalt recovery rate is 98 mass % or more, it is judged that the reduction degree in the smelting treatment is excessive. In this case, the raw material containing an oxide containing nickel and cobalt is added as an oxidant.

2. The method for producing a valuable metal according to claim 1, wherein: In the melting step, the cobalt recovery rate is calculated based on the analysis result of the cobalt grade in the slag.

3. The method for producing a valuable metal according to claim 1, wherein: In the melting step, the cobalt recovery rate is calculated based on the measurement result of the oxygen partial pressure in the melt generated by the melting treatment.

4. The method for producing a valuable metal according to any one of claims 1 to 3, wherein: The raw material containing nickel and cobalt oxides is a raw material containing waste lithium-ion batteries.

5. The method for producing a valuable metal according to any one of claims 1 to 3, wherein: The raw material contains phosphorus, The phosphorus content of the alloy recovered through the slag separation step is 0.1 mass % or less.

6. The method for producing a valuable metal according to claim 4, wherein: The raw material contains phosphorus, The phosphorus content of the alloy recovered through the slag separation step is 0.1 mass % or less.

7. The method for producing a valuable metal according to any one of claims 1 to 3 and 6, wherein: In the melting step, the raw material is melted at a heating temperature of 1300° C. or higher and 1600° C. or lower.

8. The method for producing a valuable metal according to claim 4, wherein: In the melting step, the raw material is melted at a heating temperature of 1300° C. or higher and 1600° C. or lower.

9. The method for producing a valuable metal according to claim 5, wherein: In the melting step, the raw material is melted at a heating temperature of 1300° C. or higher and 1600° C. or lower.

Citation Information

Patent Citations

  • Valuable metal recovery method

    JP2013091826A

  • Valuable metal recovery method

    CN103380220A

  • Method for recovering valuable metals from waste lithium ion batteries

    CN112424383A