A production method of enamel coil and the enamel coil produced by the same

Through specific base glaze and surface glaze formulas and multi-zone sintering technology, the problem of inconvenient separation and transportation between layers during the winding process is solved, and the stable winding and bending resistance is improved. It is suitable for small-diameter inner cylinders storage and transportation.

CN118307201BActive Publication Date: 2024-12-06FOSHAN HUANYU MODERN MATERIAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410541336.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-04-30
Publication Date
2024-12-06
Estimated Expiration
2044-04-30

AI Technical Summary

Technical Problem

The existing enamel plates have poor bending resistance, which leads to easy separation of the base material layer and the glaze layer during the winding process, and the block-like enamel plates are inconvenient to transport.

Method used

Use specific base glaze and surface glaze formulas, combined with roller coating technology and multi-zone sintering process, to control the thickness and sintering temperature of each layer to form a stable base glaze and surface glaze layer, and to enhance the base material layer, base glaze layer and base glaze layer. The bonding force between the layer and the surface glaze layer ensures that the enamel plate does not separate between layers when winding.

Benefits of technology

The enamel plate is stable in coiling and storage, avoiding interlayer separation and cracking problems, improving the bending resistance and transportation convenience of the enamel plate, and can be stably wound and stored on a smaller diameter inner cylinder.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118307201B_ABST
    Figure CN118307201B_ABST
Patent Text Reader

Abstract

The present application discloses a production method of an enamel coil and the enamel coil obtained, and relates to the field of new materials. The production method of the enamel coil comprises the following steps: rolling a base glaze on the surface of a substrate layer, sintering the base glaze, cooling once, and forming a base glaze layer on the substrate layer; rolling a top glaze on the surface of the base glaze layer, sintering the top glaze, cooling twice, and forming a top glaze layer on the surface of the base glaze layer; covering the surface of the top glaze layer away from the base glaze layer with a protective film to obtain an enamel plate, and then rolling up to obtain an enamel coil. The enamel coil in the present application uses a specific base glaze to make the base glaze layer, and uses a specific top glaze to make the top glaze layer. At the same time, with the combination of roller coating and the control of the thickness of each layer, it is possible to ensure that the enamel plate does not separate from the layers while realizing the rolling of the enamel plate, thereby solving the problem of inconvenience in transportation of enamel plates that are usually in block form in the related art and the problem of easy interlayer separation of conventional enamel plates during the rolling process.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of new materials, and in particular to a production method of an enamel coil and the enamel coil obtained therefrom. Background Art

[0002] Enamel plates usually include a substrate layer and an enamel surface layer formed by glaze, wherein the enamel surface layer is usually a hard material with poor flexibility and permeability, and the interlayer adhesion between the substrate layer and the enamel surface layer is also poor, so the existing enamel plates have poor bending resistance. When the enamel plates are rolled up, the substrate layer and the glaze layer are easily separated, resulting in the glaze layer falling off or cracking. Therefore, the existing enamel plates usually exist in block form. However, block enamel plates have the problem of inconvenient transportation. Summary of the invention

[0003] In order to improve the transportation inconvenience of enamel plates in the related art, which are usually in block form, and the problem of interlayer separation easily occurring during the winding process of conventional enamel plates, the present application provides a production method for an enamel roll and the enamel roll produced therefrom.

[0004] In the first aspect, the present application provides a method for producing an enamel coil using the following technical solution:

[0005] A method for producing an enamel coil comprises the following steps:

[0006] Rolling a base glaze on the surface of the substrate layer, then sintering the base glaze and cooling it once to form a base glaze layer on the substrate layer; the base glaze is made of 3-4wt% boric acid, 2.5-3.5% clay, 0.8-1.2wt% oxidant, 0.8-1.2wt% leveling agent and the balance base glaze frit; the base glaze frit is made of 4-5wt% Al2O3, 13-15wt% B2O3, 15-19wt% Na2O, 0-3.6wt% PbO, 0-2.8wt% ZrO2, 0-1.45wt% SrO and the balance SiO2;

[0007] Roll-coat the surface glaze on the side of the base glaze layer away from the substrate layer, then sinter the surface glaze and perform secondary cooling to form the surface glaze layer on the surface of the base glaze layer; the surface glaze is made of 2.5-3.5wt% boric acid, 2.5-3.5wt% clay, 0.8-1.2wt% oxidant, 0.8-1.2wt% leveling agent and the remainder of the surface glaze frit; the surface glaze frit is made of 5-6wt% Al2O3, 18-20wt% B2O3, 7-9wt% Na2O, 18-20wt% TiO2, 0-4.4wt% PbO, 0-3.9wt% ZrO2, 0-1.86wt% SrO and the remainder of SiO2;

[0008] A protective film is covered on the surface of the top glaze layer away from the bottom glaze layer to obtain an enamel plate, which is then rolled up to obtain an enamel roll; wherein the thickness of the substrate layer is 0.3-0.6 mm, the thickness of the bottom glaze layer is 20-50 μm, and the thickness of the top glaze layer is 50-100 μm.

[0009] In the present application, a base glaze frit is added to the base glaze of the enamel coil. The Al2O3 in the base glaze frit within the above range can improve the physical and mechanical properties and chemical durability of the base glaze layer; B2O3 can reduce the thermal expansion coefficient of the base glaze layer, reduce the difference between the thermal expansion coefficients of the substrate layer and the base glaze layer, and improve the stability of the base glaze layer and the substrate layer; Na2O can adjust the sintering temperature of the base glaze and improve the glossiness of the base glaze layer; SiO2 can react with other metal oxides to improve the smoothness of the glaze surface, improve the anti-fouling property of the glaze surface, and stabilize the glaze color. In addition, the coordination between the above raw materials is conducive to obtaining a base glaze layer with strong penetration and diffusion capabilities to the substrate layer, dense structure, and good anti-bending performance, which is conducive to the stable adhesion of the base glaze layer and the substrate layer.

[0010] The glaze of the enamel coil is added with glaze frit. Among the raw materials in the glaze frit, except for Na2O and TiO2, the other raw materials are similar to the raw materials of the base glaze. However, the glaze of the present application also adds TiO2, which can improve the whiteness and UV discoloration resistance of the glaze, and improve the overall aesthetics and durability of the enamel coil. The changes in the amount of Na2O in the glaze and other glaze frits are adjustments made by the inventor based on the addition of TiO2 to the glaze to obtain a glaze layer with a thermal expansion coefficient similar to that of the base glaze, and to obtain a glaze layer that penetrates the base glaze layer, has strong diffusion power and a tight structure.

[0011] In summary, the above-mentioned base glaze has strong penetration and diffusion capabilities on the substrate layer, the base glaze layer and the substrate layer are stably attached, the surface glaze has strong penetration and diffusion capabilities on the base glaze layer, the base glaze layer and the surface glaze layer are stably attached, and at the same time, combined with roller coating and control of the thickness of each layer, the present application can ensure that the enamel plate does not undergo interlayer separation while achieving the winding of the enamel plate, thereby solving the problem of inconvenience in transportation of enamel plates that are usually in block form in related technologies and the problem that conventional enamel plates are prone to interlayer separation during the winding process.

[0012] Preferably, the base glaze sintering and the surface glaze sintering are divided into five zones for sintering, wherein the temperature of the base glaze sintering zone 1 and the surface glaze sintering zone 1 is set to 295-305°C, and the sintering time is controlled to 20-25s; the temperature of the base glaze sintering zone 2 and the surface glaze sintering zone 2 is set to 545-555°C, and the sintering time is controlled to 20-25s; the temperature of the base glaze sintering zone 3 and the surface glaze sintering zone 3 is set to 790-810°C, and the sintering time is controlled to 20-25s; the temperature of the base glaze sintering zone 4 and the surface glaze sintering zone 4 is set to 790-810°C, and the sintering time is controlled to 20-25s; the temperature of the base glaze sintering zone 5 and the surface glaze sintering zone 5 is set to 600-605°C, and the sintering time is controlled to 20-25s.

[0013] In the present application, the base glaze and the surface glaze are sintered in five zones respectively. Among them, the base glaze sintering zone 1 and the surface glaze sintering zone 1 are used to remove free water in the base glaze and the surface glaze and decompose small molecular organic matter to prevent free water and some organic matter from affecting the solid phase reaction in the next stage. The base glaze sintering zone 2 and the surface glaze sintering zone 2 are used to remove the structural water of the raw materials in the base glaze and the surface glaze respectively. At the same time, the base glaze and the surface glaze begin to undergo solid phase reaction in this process. In the base glaze sintering zone 3 and the surface glaze sintering zone 3, the low melting point compounds gradually melt to achieve layered sintering. During this process, the base glaze or the surface glaze and the substrate layer begin to diffuse and penetrate each other. In the four sintering zones of the bottom glaze and the four sintering zones of the surface glaze, the glaze in the bottom glaze or the surface glaze has melted, and at the same time, the bubbles in the substrate layer can be discharged, which is beneficial to obtaining a glaze surface with good surface quality and no shrinkage holes; and in this process, the permeability of the bottom glaze and the substrate layer in the four sintering zones is increased, and the permeability of the surface glaze and the bottom glaze layer is increased, and gradually a stable middle layer is formed between the substrate layer and the bottom glaze layer, and between the bottom glaze layer and the surface glaze layer. The middle layer is a stable layer structure formed by the mutual penetration of the bottom glaze and the substrate layer, and the mutual penetration of the surface glaze and the bottom glaze layer. After the sintering of the bottom glaze sintering zone four and the surface glaze sintering zone four is completed, the enamel surface of the bottom glaze layer or the surface glaze layer is formed but unstable. The bottom glaze sintering zone five and the surface glaze sintering zone five are mainly stabilized by appropriate cooling to stabilize the enamel surface structure of the bottom glaze layer and the enamel surface structure of the surface glaze layer respectively obtained in the bottom glaze sintering zone four and the surface glaze sintering zone four, which is beneficial to improve the adhesion stability of each layer of the enamel coil, so that the enamel coil can be stably wound and stored on the inner cylinder with a diameter of 40cm. At the same time, it can also prevent the problem of cracks in the bottom glaze layer or the surface glaze layer after long-term winding and storage.

[0014] The present application effectively improves the bonding strength between the base layer and the base glaze layer, and between the base glaze layer and the top glaze layer by controlling the sintering temperature and sintering time of the base glaze layer and the top glaze layer, which is beneficial to further improve the stability of the enamel coil when being rolled and stored on an inner cylinder with a diameter of 40 cm.

[0015] Preferably, the base glaze frit is made of 4-5wt% Al2O3, 13-15wt% B2O3, 15-19wt% Na2O, 2.4-3.6wt% PbO, 2.2-2.8wt% ZrO2, 1.25-1.45wt% SrO and the balance SiO2;

[0016] The glaze frit is prepared from 5-6wt% Al2O3, 18-20wt% B2O3, 7-9wt% Na2O, 18-20wt% TiO2, 3.8-4.4wt% PbO, 3.3-3.9wt% ZrO2, 1.55-1.86wt% SrO and the balance SiO2.

[0017] In this application, the addition of PbO can increase the viscosity of the glaze layer, making the structure of the bottom glaze layer and the surface glaze layer more compact and firm, and further improving the ability of the bottom glaze layer and the surface glaze layer to resist bending cracking or delamination. The enamel coil can adapt to the winding of the inner tube with a minimum diameter of 250mm, which is conducive to saving storage space and reducing transportation costs. At the same time, adding ZrO2 and SrO within a specific ratio range on the basis of other raw materials can solve the glaze quality problems such as fish scale shrinkage holes and pitting introduced by the addition of PbO without changing the sintering temperature, which is conducive to improving the anti-fouling performance of the enamel coil.

[0018] Preferably, the method for preparing the base glaze frit comprises the following steps:

[0019] Al2O3, B2O3, Na2O, PbO, ZrO2, SrO and SiO2 are mixed according to proportions, melted, cooled and crushed at 1050-1080°C to obtain base glaze frit.

[0020] Preferably, the preparation method of the base glaze is as follows:

[0021] After mixing the raw materials of the base glaze according to the proportion, add 45-55% of water of the total weight of the base glaze raw materials, ball-mill until the slurry fineness is 20-25 μm, and then filter to obtain the base glaze.

[0022] The present application controls the fineness of the base glaze to be 20-25 μm, which is conducive to forming a flat, smooth, and densely structured base glaze layer, which can improve the ability of the base glaze layer to resist bending cracking or delamination. At the same time, it is also conducive to the rapid penetration and diffusion of the base glaze into the substrate layer, so as to further improve the bonding stability between the substrate layer and the base glaze layer.

[0023] Preferably, the method for preparing the glaze frit comprises the following steps:

[0024] After Al2O3, B2O3, Na2O, TiO2, PbO, ZrO2, SrO and SiO2 are mixed according to the proportion,

[0025] It is melted, cooled and crushed at 1125-1155℃ to obtain glaze frit.

[0026] Preferably, the preparation method of the glaze is as follows:

[0027] After mixing the raw materials of the glaze according to the proportion, add 55-60% of the total weight of the glaze raw materials into water.

[0028] The slurry is ball-milled to a fineness of 15-20 μm, and then filtered to obtain the glaze.

[0029] The present application controls the fineness of the base glaze to be 15-20 μm, which is conducive to forming a flat, smooth, and densely structured surface glaze layer, which can improve the ability of the surface glaze layer to resist bending cracking or delamination. At the same time, it is also conducive to the rapid penetration and diffusion of the surface glaze into the base glaze layer, so as to further improve the bonding stability between the surface glaze layer and the base glaze layer.

[0030] Optionally, in the base glaze and the top glaze, the leveling agent is sodium carboxymethyl cellulose, and the oxidant is at least one of zinc oxide and magnesium oxide.

[0031] Optionally, when roller coating the base glaze and the surface glaze, the base glaze and the surface glaze are coated by reverse coating, and the coating process is carried out by the cooperation of the belt roller and the coating roller, the belt roller brings the base glaze to the coating roller, and then the coating roller brings the base glaze to the substrate layer; wherein the conveying speed of the substrate layer is controlled at 5-20m / min, the speed of the belt roller is controlled to be 1.2-1.8 times the conveying speed of the substrate layer, and the speed of the coating roller is controlled to be 2.0-2.5 times the conveying speed of the substrate layer.

[0032] In the present application, when roller coating the base glaze and the top glaze, the speed of the material roller is controlled to be 1.2-1.8 times the conveying speed of the substrate layer, and the speed of the coating roller is controlled to be 2.0-2.5 times the conveying speed of the substrate layer, which is beneficial to improve the coating uniformity of the base glaze layer and the top glaze layer.

[0033] Optionally, the substrate layer is made of any one of enameled steel plate, nickel-plated plate, aluminum-plated plate, martensitic stainless steel, and ferritic stainless steel.

[0034] When the base layer is made of enameled steel plate, at least one of the base glaze or top glaze needs to be roller-coated on both the upper and lower surfaces of the enameled steel plate to prevent the enameled steel plate from rusting. When the base layer is made of nickel-plated plate, aluminum-plated plate, martensitic stainless steel, or ferritic stainless steel, the base layer can be roller-coated on only one surface.

[0035] In the second aspect, the enamel coil provided in the present application adopts the following technical solution:

[0036] An enamel roll plate comprises a substrate layer, a bottom glaze layer, a surface glaze layer and a protective film which are arranged in sequence, and is produced by any one of the above-mentioned enamel roll plate production methods.

[0037] In summary, this application at least includes the following beneficial technical effects:

[0038] (1) The enamel rolled plate in the present application adopts a specific base glaze to make a base glaze layer, and adopts a specific top glaze to make a top glaze layer. At the same time, with the combination of roller coating and control of the thickness of each layer, it is possible to ensure that the enamel plate does not separate between layers while realizing the rolling of the enamel plate, thereby solving the problem of the inconvenience of transportation of enamel plates that are usually in block form in the related art and the problem that conventional enamel plates are prone to separation between layers during the rolling process.

[0039] (2) Conventionally, the sintering of the base glaze and the surface glaze is carried out in four steps. The present application adds the sintering of the fifth sintering zone after the conventional fourth sintering step. The sintering of the fifth sintering zone is mainly carried out by appropriately cooling down the enamel surface structure of the base glaze layer and the enamel surface structure of the surface glaze layer respectively obtained in the fourth sintering zone of the base glaze and the fourth sintering zone of the surface glaze. This is beneficial to improving the adhesion stability of each layer of the enamel coil, so that the enamel coil can be stably wound and stored on an inner cylinder with a diameter of 40 cm. At the same time, it can also prevent the problem of cracks in the base glaze layer or the surface glaze layer after long-term winding and storage.

[0040] (3) The present application adds specific proportions of PbO, ZrO2 and SrO to the basic base glaze and top glaze formulas, respectively. The combination of PbO, ZrO2 and SrO can effectively improve the enamel plate's ability to resist bending cracking or delamination and storage stability, so that the enamel plate can be wound on an inner cylinder with a minimum diameter of 250 mm and can be stored stably for a long time without interlayer separation or cracking. At the same time, the surface of the top glaze layer of the enamel rolled plate is smooth and flat, without fish-scale shrinkage holes or pitting. BRIEF DESCRIPTION OF THE DRAWINGS

[0041] Figure 1 It is a structural schematic diagram of an enamel roll plate of the present application.

[0042] Description of reference numerals:

[0043] 1. Base material layer; 2. Base glaze layer; 3. Top glaze layer; 4. Protective film. DETAILED DESCRIPTION

[0044] The present application is further described below in conjunction with specific experiments.

[0045] Example of base glaze preparation

[0046] [Preparation Example 1-1]

[0047] A base glaze is prepared from 3wt% boric acid, 3.5wt% clay, 0.8wt% magnesium oxide, 1.2wt% sodium carboxymethyl cellulose and the balance base glaze frit, wherein the base glaze frit is prepared from 4wt% Al2O3, 15wt% B2O3, 19wt% Na2O and the balance SiO2.

[0048] The preparation method of the base glaze in this preparation example comprises the following steps:

[0049] Al2O3, B2O3, Na2O and SiO2 are mixed according to the proportion, melted, cooled and crushed at 1050°C to obtain the base glaze frit;

[0050] After mixing the base glaze frit, boric acid, clay, magnesium oxide and sodium carboxymethyl cellulose in the base glaze according to the proportion, adding 45% water of the total weight of the base glaze raw materials, ball milling to a slurry fineness of 20-25 μm, and then filtering to obtain the base glaze.

[0051] [Preparation Example 1-2]

[0052] A base glaze is prepared from 4wt% boric acid, 2.5wt% clay, 1.2wt% zinc oxide, 0.8wt% sodium carboxymethyl cellulose and the balance base glaze frit, wherein the base glaze frit is prepared from 5wt% Al2O3, 13wt% B2O3, 15wt% Na2O and the balance SiO2.

[0053] The preparation method of the base glaze in this preparation example comprises the following steps:

[0054] Al2O3, B2O3, Na2O and SiO2 are mixed in proportion, melted, cooled and crushed at 1080°C to obtain a base glaze frit;

[0055] After mixing the base glaze frit, boric acid, clay, zinc oxide and sodium carboxymethyl cellulose in the base glaze according to the proportion, adding 55% water of the total weight of the base glaze raw materials, ball milling to a slurry fineness of 20-25 μm, and then filtering to obtain the base glaze.

[0056] [Preparation Example 1-3]

[0057] A base glaze, which differs from [Preparation Example 1-1] in that the base glaze frit is different.

[0058] In this preparation example, the base glaze frit is made of 4wt% Al2O3, 15wt% B2O3, 19wt% Na2O, 3.0wt% PbO, 2.5wt% ZrO2, 1.35wt% SrO and the balance SiO2.

[0059] [Preparation Example 1-4]

[0060] A base glaze, which differs from [Preparation Example 1-3] in that the base glaze frit is different.

[0061] In this preparation example, the base glaze frit is prepared from 4wt% Al2O3, 15wt% B2O3, 19wt% Na2O, 3.0wt% PbO, 3.85wt% SrO and the balance SiO2.

[0062] [Preparation Example 1-5]

[0063] A base glaze, which differs from [Preparation Example 1-3] in that the base glaze frit is different.

[0064] In this preparation example, the base glaze frit is prepared from 4wt% Al2O3, 15wt% B2O3, 19wt% Na2O, 3.0wt% PbO, 3.85wt% ZrO2 and the balance SiO2.

[0065] [Preparation Example 1-6]

[0066] A base glaze, which differs from [Preparation Example 1-3] in that the base glaze frit is different.

[0067] In this preparation example, the base glaze frit is prepared from 4wt% Al2O3, 15wt% B2O3, 19wt% Na2O, 1.2wt% PbO, 1.8wt% ZrO2, 1.0wt% SrO and the balance SiO2.

[0068] Glaze Preparation Example

[0069] [Preparation Example 2-1]

[0070] A glaze is prepared from 2.5wt% boric acid, 3.5wt% clay, 0.8wt% magnesium oxide, 1.2wt% sodium carboxymethyl cellulose and the remainder of glaze frit; wherein the glaze frit is prepared from 5wt% Al2O3, 20wt% B2O3, 9wt% Na2O, 18wt% TiO2 and the remainder SiO2.

[0071] The preparation method of the glaze in this preparation example comprises the following steps:

[0072] Al2O3, B2O3, Na2O, TiO2 and SiO2 are mixed according to the proportion, melted, cooled and crushed at 1125°C to obtain glaze frit;

[0073] After mixing the glaze frit, boric acid, clay, magnesium oxide and sodium carboxymethyl cellulose according to the proportion,

[0074] Add 55% of the total weight of the glaze raw materials with water, ball-mill until the slurry fineness is 15-20 μm, and then filter to obtain the glaze.

[0075] [Preparation Example 2-2]

[0076] A glaze is prepared from 3.5wt% boric acid, 2.5wt% clay, 1.2wt% zinc oxide, 0.8wt% sodium carboxymethyl cellulose and the remainder of glaze frit; wherein the glaze frit is prepared from 6wt% Al2O3, 18wt% B2O3, 7wt% Na2O, 20wt% TiO2 and the remainder SiO2.

[0077] The preparation method of the glaze in this preparation example comprises the following steps:

[0078] Al2O3, B2O3, Na2O, TiO2 and SiO2 are mixed according to the proportion, melted, cooled and crushed at 1155°C to obtain glaze frit;

[0079] After mixing the glaze frit, boric acid, clay, zinc oxide and sodium carboxymethyl cellulose according to the proportion,

[0080] Add 60% water of the total weight of the glaze raw materials, ball-mill until the slurry fineness is 15-20 μm, and then filter to obtain the glaze.

[0081] [Preparation Example 2-3]

[0082] A glaze, which differs from [Preparation Example 2-1] in that the glaze frit is different.

[0083] In this preparation example, the glaze frit is made of 5wt% Al2O3, 20wt% B2O3, 9wt% Na2O, 18wt% TiO2, 4.0wt% PbO, 3.5wt% ZrO2, 1.72wt% SrO and the balance SiO2.

[0084] [Preparation Example 2-4]

[0085] A glaze, which differs from [Preparation Example 2-3] in that the glaze frit is different.

[0086] In this preparation example, the glaze frit is made of 5wt% Al2O3, 20wt% B2O3, 9wt% Na2O, 18wt% TiO2, 4.0wt% PbO, 5.22wt% ZrO2 and the balance SiO2.

[0087] [Preparation Example 2-5]

[0088] A glaze, which differs from [Preparation Example 2-3] in that the glaze frit is different.

[0089] In this preparation example, the glaze frit is prepared from 5wt% Al2O3, 20wt% B2O3, 9wt% Na2O, 18wt% TiO2, 4.0wt% PbO, 5.22wt% SrO and the balance SiO2.

[0090] [Preparation Example 2-6]

[0091] A glaze, which differs from [Preparation Example 2-3] in that the glaze frit is different.

[0092] In this preparation example, the glaze frit is made of 5wt% Al2O3, 20wt% B2O3, 9wt% Na2O, 18wt% TiO2, 2.8wt% PbO, 1.5wt% ZrO2, 1.12wt% SrO and the balance SiO2.

[0093] Example

[0094] [Example 1]

[0095] An enamel roll comprises a base glaze layer 2, a substrate layer 1, a base glaze layer 2, a surface glaze layer 3 and a protective film 4 which are arranged in sequence. The thickness of the substrate layer 1 is 0.3 mm, the thickness of the base glaze layer 2 is 20 μm, the thickness of the surface glaze layer 3 is 50 μm, and the thickness of the protective film 4 is 5 μm.

[0096] The production method of enamel coil comprises the following steps:

[0097] S1. In continuous production, two raw coils of enameled steel sheets are sequentially transferred to the process section by using uncoiler A and uncoiler B, and then the coil tail of uncoiler A is welded with the coil head and tail of uncoiler B to obtain substrate layer 1; wherein, the raw coil of enameled steel sheets shall meet the requirements of GB / T 13790-2008 Cold-rolled low-carbon steel sheets and steel strips for enameling. In this embodiment, the grade of the raw coil of enameled steel sheets is DC05EK;

[0098] S2, coating the base glaze prepared in [Preparation Example 1-1] on the upper and lower surfaces of the substrate layer 1 with a roller, then sintering the base glaze and cooling it once, and forming base glaze layers 2 on the upper and lower surfaces of the substrate layer 1 respectively;

[0099] The bottom glaze is coated by reverse coating. During the coating process, the material roller and the coating roller cooperate with each other to bring the bottom glaze to the coating roller, and then the coating roller brings the bottom glaze to the substrate layer 1. The conveying speed of the substrate layer 1 is controlled at 10m / min, the speed control range of the material roller is 1.2 times the conveying speed of the substrate layer 1, and the speed of the coating roller is controlled to be 2.0 times the conveying speed of the substrate layer 1.

[0100] The bottom glaze sintering is divided into five zones for sintering. The temperature of the bottom glaze sintering zone 1 is set to 300℃, and the sintering time is controlled to 20s; the temperature of the bottom glaze sintering zone 2 is set to 550℃, and the sintering time is controlled to 20s; the temperature of the bottom glaze sintering zone 3 is set to 800℃, and the sintering time is controlled to 20s; the temperature of the bottom glaze sintering zone 4 is set to 800℃, and the sintering time is controlled to 20s; the temperature of the bottom glaze sintering zone 5 is set to 600℃, and the sintering time is controlled to 20s;

[0101] During the primary cooling, the cooling rate of the furnace temperature is controlled at 5°C / min, and the primary cooling is completed when the temperature of the plate drops below 50°C;

[0102] S3, coating the surface glaze prepared in [Preparation Example 2-1] on the surface of one of the base glaze layers 2 with a roller, then sintering the surface glaze and performing secondary cooling to form a surface glaze layer 3 on the substrate layer 1;

[0103] The roller coating of the top glaze is carried out in a reverse coating manner. During the coating process, the material roller and the coating roller cooperate with each other to bring the top glaze to the coating roller, and then the coating roller brings the top glaze to the substrate layer 1. The conveying speed of the substrate layer 1 is controlled at 10m / min, the speed control range of the material roller is 1.2 times the conveying speed of the substrate layer 1, and the speed of the coating roller is controlled to be 2.0 times the conveying speed of the substrate layer 1.

[0104] The glaze sintering is divided into five zones. The temperature of the glaze sintering zone 1 is set to 300℃, and the sintering time is controlled to 20s; the temperature of the glaze sintering zone 2 is set to 550℃, and the sintering time is controlled to 20s; the temperature of the glaze sintering zone 3 is set to 800℃, and the sintering time is controlled to 20s; the temperature of the glaze sintering zone 4 is set to 800℃, and the sintering time is controlled to 20s; the temperature of the glaze sintering zone 5 is set to 600℃, and the sintering time is controlled to 20s;

[0105] During secondary cooling, the cooling rate of the furnace temperature is controlled at 5°C / min, and the secondary cooling is completed when the temperature of the plate drops below 50°C;

[0106] S4, covering the surface of the top glaze layer 3 away from the bottom glaze layer 2 with a protective film 4 to obtain an enamel plate, and then rolling it up to obtain an enamel roll plate.

[0107] [Example 2]

[0108] An enamel roll comprises a base glaze layer 2, a substrate layer 1, a base glaze layer 2, a surface glaze layer 3 and a protective film 4 which are arranged in sequence, wherein the thickness of the substrate layer 1 is 0.6 mm, the thickness of the base glaze layer 2 is 50 μm, the thickness of the surface glaze layer 3 is 100 μm, and the thickness of the protective film 4 is 5 μm.

[0109] The production method of enamel coil comprises the following steps:

[0110] S1. In continuous production, two raw coils of enameled steel sheets are sequentially transferred to the process section by using uncoiler A and uncoiler B, and then the coil tail of uncoiler A is welded with the coil head and tail of uncoiler B to obtain substrate layer 1; wherein, the raw coil of enameled steel sheets shall meet the requirements of GB / T 13790-2008 Cold-rolled low-carbon steel sheets and steel strips for enameling. In this embodiment, the grade of the raw coil of enameled steel sheets is DC03EK;

[0111] S2, coating the base glaze prepared in [Preparation Example 1-2] on the upper and lower surfaces of the substrate layer 1 with a roller, then sintering the base glaze and cooling it once, and forming base glaze layers 2 on the upper and lower surfaces of the substrate layer 1 respectively;

[0112] The bottom glaze is coated by reverse coating. During the coating process, the material roller and the coating roller cooperate with each other to bring the bottom glaze to the coating roller, and then the coating roller brings the bottom glaze to the substrate layer 1. The conveying speed of the substrate layer 1 is controlled at 10m / min, the speed control range of the material roller is 1.8 times the conveying speed of the substrate layer 1, and the speed of the coating roller is controlled to be 2.5 times the conveying speed of the substrate layer 1.

[0113] The bottom glaze sintering is divided into five zones. The temperature of the bottom glaze sintering zone 1 is set at 300℃, and the sintering time is controlled to 25s; the temperature of the bottom glaze sintering zone 2 is set at 550℃, and the sintering time is controlled to 25s; the temperature of the bottom glaze sintering zone 3 is set at 800℃, and the sintering time is controlled to 25s; the temperature of the bottom glaze sintering zone 4 is set at 800℃, and the sintering time is controlled to 25s; the temperature of the bottom glaze sintering zone 5 is set at 600℃, and the sintering time is controlled to 25s;

[0114] During the primary cooling, the cooling rate of the furnace temperature is controlled at 5°C / min, and the primary cooling is completed when the temperature of the plate drops below 50°C;

[0115] S3, coating the surface glaze prepared in [Preparation Example 2-2] on the surface of one of the base glaze layers 2 with a roller, then sintering the surface glaze and performing secondary cooling to form a surface glaze layer 3 on the substrate layer 1;

[0116] The roller coating of the top glaze is carried out in a reverse coating manner. During the coating process, the material roller and the coating roller cooperate with each other to bring the top glaze to the coating roller, and then the coating roller brings the top glaze to the substrate layer 1. The conveying speed of the substrate layer 1 is controlled at 10m / min, the speed control range of the material roller is 1.8 times the conveying speed of the substrate layer 1, and the speed of the coating roller is controlled to be 2.5 times the conveying speed of the substrate layer 1.

[0117] The glaze sintering is divided into five zones. The temperature of the glaze sintering zone 1 is set to 300℃, and the sintering time is controlled to 25s; the temperature of the glaze sintering zone 2 is set to 550℃, and the sintering time is controlled to 25s; the temperature of the glaze sintering zone 3 is set to 800℃, and the sintering time is controlled to 25s; the temperature of the glaze sintering zone 4 is set to 800℃, and the sintering time is controlled to 25s; the temperature of the glaze sintering zone 5 is set to 600℃, and the sintering time is controlled to 25s.

[0118] During secondary cooling, the cooling rate of the furnace temperature is controlled at 5°C / min, and the secondary cooling is completed when the temperature of the plate drops below 50°C;

[0119] S4, covering the surface of the top glaze layer 3 away from the bottom glaze layer 2 with a protective film 4 to obtain an enamel plate, and then rolling it up to obtain an enamel roll plate.

[0120] [Example 3]

[0121] An enamel coil, which differs from [Example 1] in that: in step S2, the base glaze is sintered in four zones, the temperature of the base glaze sintering zone 1 is set to 300°C, and the sintering time is controlled to 20s; the temperature of the base glaze sintering zone 2 is set to 550°C, and the sintering time is controlled to 20s; the temperature of the base glaze sintering zone 3 is set to 800°C, and the sintering time is controlled to 20s; the temperature of the base glaze sintering zone 4 is set to 800°C, and the sintering time is controlled to 20s.

[0122] [Example 4]

[0123] An enamel coil, which differs from [Example 1] in that: in step S3, the glaze sintering is divided into four zones, the temperature of the glaze sintering zone 1 is set to 300°C, and the sintering time is controlled to 20s; the temperature of the glaze sintering zone 2 is set to 550°C, and the sintering time is controlled to 20s; the temperature of the glaze sintering zone 3 is set to 800°C, and the sintering time is controlled to 20s; the temperature of the glaze sintering zone 4 is set to 800°C, and the sintering time is controlled to 20s.

[0124] [Example 5]

[0125] An enamel roll plate, which differs from [Example 1] in that: the base glaze in step S2 adopts the base glaze prepared in [Preparation Example 1-3], and the surface glaze in step S3 adopts the surface glaze prepared in [Preparation Example 2-3].

[0126] [Example 6]

[0127] An enamel roll plate, which differs from [Example 5] in that: the base glaze in step S2 adopts the base glaze prepared in [Preparation Example 1-4], and the surface glaze in step S3 adopts the surface glaze prepared in [Preparation Example 2-4].

[0128] [Example 7]

[0129] An enamel roll plate, which differs from [Example 5] in that: the base glaze in step S2 adopts the base glaze prepared in [Preparation Example 1-5], and the surface glaze in step S3 adopts the surface glaze prepared in [Preparation Example 2-5].

[0130] [Example 8]

[0131] An enamel roll plate, which differs from [Example 5] in that: the base glaze in step S2 adopts the base glaze prepared in [Preparation Example 1-6], and the surface glaze in step S3 adopts the surface glaze prepared in [Preparation Example 2-6].

[0132] Comparative Example

[0133] [Comparative Example 1]

[0134] An enamel coil, which differs from [Example 1] in that: in step S2, the composition of the base glaze frit used for the base glaze is different.

[0135] The base glaze frit is made of 7wt% Al2O3, 5wt% B2O3, 19wt% Na2O and the balance SiO2.

[0136] [Comparative Example 2]

[0137] An enamel coil, which differs from [Example 1] in that: in step S3, the composition of the glaze frit used for the glaze is different.

[0138] The glaze frit is made of 3wt% Al2O3, 15wt% B2O3, 15wt% Na2O, 10wt% TiO2 and the balance SiO2.

[0139] [Comparative Example 3]

[0140] An enamel coil, which differs from [Example 1] in that: in steps S2 and S3, roller coating is replaced by spraying.

[0141] [Comparative Example 4]

[0142] An enamel roll plate, which differs from [Example 1] in that: the thickness of the base material layer 1 is 3 mm, the thickness of the bottom glaze layer 2 is 100 μm, and the thickness of the top glaze layer 3 is 250 μm.

[0143] Performance testing

[0144] 1. Surface quality of the glaze layer: Observe whether the surface of the glaze layer is smooth and flat, and whether there are any quality problems such as fish-scale shrinkage holes and pitting.

[0145] 2. Windability: The enamel coils prepared in the embodiments and comparative examples were respectively rolled up using inner cylinders with different diameters to observe whether the enamel coils could be rolled up smoothly without interlayer separation and cracks.

[0146] 3. Winding stability: If the winding can be carried out smoothly without interlayer separation, 20 rolls of enamel coils wound by inner cylinders with different diameters are randomly selected from each embodiment and comparative example, and after being stored in an environment of 40°C for 180 days, observe whether interlayer separation occurs in the enamel coils, and then calculate the percentage of the number of enamel coils with interlayer separation.

[0147] 4. Stability of the surface glaze layer: If the enamel coils can be rolled smoothly without interlayer separation and cracks, 20 rolls of enamel coils rolled by inner cylinders of different diameters are randomly selected from each embodiment and comparative example, and after being stored in an environment of 40°C for 180 days, the surface glaze layer of the enamel coils is observed to see whether stress cracks occur, and then the proportion of enamel coils with stress cracks in the surface glaze layer is calculated.

[0148] Table 1

[0149] Sample Glaze surface quality Example 1 The surface of the glaze layer is smooth and flat without fish-scale shrinkage holes and pitting problems Example 2 The surface of the glaze layer is smooth and flat without fish-scale shrinkage holes and pitting problems Example 3 The surface of the glaze layer is smooth and flat without fish-scale shrinkage holes and pitting problems Example 4 The surface of the glaze layer is smooth and flat without fish-scale shrinkage holes and pitting problems Example 5 The surface of the glaze layer is smooth and flat without fish-scale shrinkage holes and pitting problems Example 6 There are scattered fish-scale shrinkage holes on the surface of the glaze layer Example 7 There are scattered fish-scale shrinkage holes on the surface of the glaze layer Example 8 The surface of the glaze layer is smooth and flat without fish-scale shrinkage holes and pitting problems Comparative Example 1 The surface of the glaze layer is smooth and flat without fish-scale shrinkage holes and pitting problems Comparative Example 2 There are a lot of fish-scale shrinkage holes or pitting on the surface of the glaze layer, and the surface is not smooth and flat Comparative Example 3 There are a lot of fish-scale shrinkage holes or pitting on the surface of the glaze layer, and the surface is not smooth and flat Comparative Example 4 The surface of the glaze layer is smooth and flat without fish-scale shrinkage holes and pitting problems

[0150] Table 2

[0151]

[0152]

[0153] Table 3

[0154]

[0155]

[0156] Table 4

[0157]

[0158] The difference between Comparative Example 1 and Example 1 is that in step S2, the composition of the bottom glaze frit used for the bottom glaze is different. Among them, the content of Al2O3 and B2O3 in the bottom glaze frit used in Comparative Example 1 is not within the scope of the present application. Combined with the test results in Tables 1 to 4, it can be seen that when the content of Al2O3 and B2O3 in the bottom glaze frit is not within the scope of the present application, the bending resistance of the enamel plate is poor. During the bending process, the bottom glaze layer 2 of the enamel plate is easily separated from the substrate layer 1 and the surface glaze layer 3, and the problem of easy interlayer separation of the existing enamel plate during the winding process cannot be solved.

[0159] The difference between Comparative Example 2 and Example 1 is that in step S3, the composition of the glaze frit used for the glaze is different. Among them, the contents of Al2O3, B2O3, Na2O, and TiO2 of the glaze frit used in Comparative Example 2 are all outside the scope of the present application. Combined with the test results in Tables 1 to 4, it can be seen that when the contents of Al2O3, B2O3, Na2O, and TiO2 of the glaze frit are all outside the scope of the present application, the surface of the glaze layer 3 is prone to surface defects, and the enamel plate will be interlayer separated between the top glaze layer 3 and the bottom glaze layer 2 during the winding process, and the problem of the existing enamel plate being prone to interlayer separation during the winding process cannot be solved.

[0160] The difference between Comparative Example 3 and Example 1 is that in steps S2 and S3, roller coating is replaced by spray coating. Combining the test results in Tables 1 to 4, it can be seen that when spray coating is used instead of roller coating, surface defects are easily generated on the surface of the top glaze layer 3, and interlayer separation is easily generated between the substrate layer 1 and the bottom glaze layer 2, and between the top glaze layer 3 and the bottom glaze layer 2 during the winding process of the enamel plate, and the problem of interlayer separation easily occurring during the winding process of the existing enamel plate cannot be solved.

[0161] The difference between Comparative Example 4 and Example 1 is that the thicknesses of the substrate layer 1, the bottom glaze layer 2 and the top glaze layer 3 are different. In particular, in combination with the test results in Tables 1 to 4, it can be seen that when the thicknesses of the substrate layer 1, the bottom glaze layer 2 and the top glaze layer 3 are not within the scope of the present application, the substrate layer 1 and the bottom glaze layer 2, and the top glaze layer 3 and the bottom glaze layer 2 are easily separated during the winding process of the enamel plate, and the problem of the easy occurrence of interlayer separation in the winding process of the existing enamel plate cannot be solved.

[0162] The difference between Example 3-4 and Example 1 is that the sintering of the bottom glaze layer 2 in Example 3 omits the sintering of the five zones of the bottom glaze sintering, and the sintering of the top glaze layer 3 in Example 4 omits the sintering of the five zones of the top glaze sintering. Combined with the test results in Tables 1-4, it can be seen that after the sintering of the bottom glaze layer 2 and the top glaze layer 3 omits the sintering of the five zones, although the bottom glaze layer 2 and the top glaze layer 3 can be smoothly wound in the initial stage, during the storage process, the enamel coil part will experience interlayer separation, and cracks will appear in the top glaze layer 3 of some enamel coils. To solve this problem, when sintering the bottom glaze and the top glaze, it is preferred to add five-zone sintering after four-zone sintering to form a stable enamel surface structure, improve the interlayer bonding strength of the enamel coil and the stable top glaze layer 3 structure.

[0163] The difference between Examples 5-8 and Example 1 is that: compared with Example 1, ZrO2 and SrO are added to the base glaze and surface glaze in Examples 5 and 8 at the same time as PbO, but the ratios of PbO, ZrO2 and SrO added to the base glaze and surface glaze in Examples 5 and 8 are different; SrO is added to the base glaze and surface glaze in Example 6 at the same time as PbO, and ZrO2 is added to the base glaze and surface glaze in Example 7 at the same time as PbO. Combined with the test results in Tables 1 to 4, it can be seen that: adding ZrO2 and SrO at the same time as PbO, while ensuring that the PbO content in the base glaze is in the range of 2.4-3.6wt%, the ZrO2 content is in the range of 2.2-2.8wt%, and the SrO content is in the range of 1.25-1.45wt%, and the PbO content in the surface glaze is in the range of 3.8-4.4wt%, the ZrO2 content is in the range of 3.3-3.9wt%, and the SrO content is in the range of 1.55-1.86wt%. The bending resistance and stability of the enamel coil can be effectively improved, so that the enamel plate can be wound on an inner cylinder with a diameter of 250mm, and can be stably stored for a long time without interlayer separation or cracks. At the same time, the surface glaze layer 3 of the enamel coil is smooth and flat, without fish-scale shrinkage holes or pitting.

[0164] The embodiments of this specific implementation are all preferred embodiments of the present application, and are not intended to limit the protection scope of the present application. The same components are represented by the same figure marks. Therefore, any equivalent changes made based on the structure, shape, and principle of the present application should be included in the protection scope of the present application.

Claims

1. A method for producing an enamel coil, characterized in that: The following steps are involved: A base glaze is rolled on the surface of a substrate layer (1), and then the base glaze is sintered and cooled once, thereby forming a base glaze layer (2) on the substrate layer (1); the base glaze is made of 3-4wt% boric acid, 2.5-3.5wt% clay, 0.8-1.2wt% oxidant, 0.8-1.2wt% leveling agent and the remainder of base glaze frit; the base glaze frit is made of 4-5wt% Al2O3, 13-15wt% B2O3, 15-19wt% Na2O, 0-3.6wt% PbO, 0-2.8wt% ZrO2, 0-1.45wt% SrO and the remainder of SiO2; A top glaze is applied by roller coating on the surface of the base glaze layer (2) on the side facing away from the substrate layer (1), followed by sintering and secondary cooling of the top glaze, and forming a top glaze layer (3) on the surface of the base glaze layer (2); the top glaze is made of 2.5-3.5wt% boric acid, 2.5-3.5wt% clay, 0.8-1.2wt% oxidant, 0.8-1.2wt% leveling agent and the remainder of the top glaze frit; the top glaze frit is made of 5-6wt% Al2O3, 18-20wt% B2O3, 7-9wt% Na2O, 18-20wt% TiO2, 0-4.4wt% PbO, 0-3.9wt% ZrO2, 0-1.86wt% SrO and the remainder of SiO2; A protective film (4) is covered on the surface of the top glaze layer (3) facing away from the bottom glaze layer (2) to obtain an enamel plate, which is then rolled up to obtain an enamel roll plate; The bottom glaze sintering and the top glaze sintering are divided into five zones for sintering. The temperature of the bottom glaze sintering zone 1 and the top glaze sintering zone 1 is set to 295-305°C, and the sintering time is controlled to 20-25s; the temperature of the bottom glaze sintering zone 2 and the top glaze sintering zone 2 is set to 545-555°C, and the sintering time is controlled to 20-25s; the temperature of the bottom glaze sintering zone 3 and the top glaze sintering zone 3 is set to 790-810°C, and the sintering time is controlled to 20-2 5s; the temperature of the fourth sintering zone of the bottom glaze and the fourth sintering zone of the surface glaze is set to 790-810°C, and the sintering time is controlled to be 20-25s; the temperature of the fifth sintering zone of the bottom glaze and the fifth sintering zone of the surface glaze is set to 600-605°C, and the sintering time is controlled to be 20-25s; the thickness of the substrate layer (1) is 0.3-0.6mm, the thickness of the bottom glaze layer (2) is 20-50μm, and the thickness of the surface glaze layer (3) is 50-100μm.

2. The method for producing an enamel coil according to claim 1, characterized in that: The bottom glaze frit is made of 4-5wt% Al2O3, 13-15wt% B2O3, 15-19wt% Na2O, 2.4-3.6wt% PbO, 2.2-2.8wt% ZrO2, 1.25-1.45wt% SrO and the balance SiO2; The glaze frit is prepared from 5-6wt% Al2O3, 18-20wt% B2O3, 7-9wt% Na2O, 18-20wt% TiO2, 3.8-4.4wt% PbO, 3.3-3.9wt% ZrO2, 1.55-1.86wt% SrO and the balance SiO2.

3. A method for producing an enamel coil according to any one of claims 1 to 2, characterized in that: The method for preparing the bottom glaze frit comprises the following steps: Al2O3, B2O3, Na2O, PbO, ZrO2, SrO and SiO2 are mixed according to proportions, melted, cooled and crushed at 1050-1080°C to obtain base glaze frit.

4. A method for producing an enamel coil according to any one of claims 1 to 2, characterized in that: The preparation method of the bottom glaze is as follows: After mixing the raw materials of the base glaze according to the proportion, add 45-55% of water by the total weight of the base glaze raw materials, ball-mill until the slurry fineness is 20-25 μm, and then filter to obtain the base glaze.

5. A method for producing an enamel coil according to any one of claims 1 to 2, characterized in that: The method for preparing the glaze frit comprises the following steps: Al2O3, B2O3, Na2O, TiO2, PbO, ZrO2, SrO and SiO2 are mixed according to proportion, melted, cooled and crushed at 1125-1155℃ to obtain glaze frit.

6. A method for producing an enamel coil according to any one of claims 1 to 2, characterized in that: The preparation method of the glaze is as follows: After mixing the raw materials of the glaze according to the proportion, add 55-60% of water by the total weight of the glaze raw materials, ball-mill until the slurry fineness is 15-20 μm, and then filter to obtain the glaze.

7. A method for producing an enamel coil according to any one of claims 1 to 2, characterized in that: When the base glaze and the top glaze are roller-coated, the base glaze and the top glaze are roller-coated in a reverse coating manner, and the coating process is carried out by the cooperation of a belt roller and a coating roller, the belt roller carries the base glaze to the coating roller, and the coating roller then carries the base glaze to the substrate layer (1); wherein the conveying speed of the substrate layer (1) is controlled at 5-20 m / min, the speed of the belt roller is controlled at 1.2-1.8 times the conveying speed of the substrate layer (1), and the speed of the coating roller is controlled at 2.0-2.5 times the conveying speed of the substrate layer (1).

8. A method for producing an enamel coil according to any one of claims 1 to 2, characterized in that: The substrate layer (1) is made of any one of enameled steel plate, nickel-plated plate, aluminum-plated plate, martensitic stainless steel, and ferritic stainless steel; in the base glaze and the top glaze, the leveling agent is sodium carboxymethyl cellulose, and the oxidant is at least one of zinc oxide and magnesium oxide.

9. An enamel coil, characterized in that: The enamel rolled plate is produced by the production method of any one of claims 1 to 8.