A method for preparing nano lithium soapstone by microwave irradiation using clay as raw material
By utilizing highly active silicon sources after natural clay depolymerization and microwave irradiation technology, the problems of high production cost and unsatisfactory size distribution of hectorite were solved, low-cost, green preparation of nano-hectorite was achieved, and the synthesis efficiency was improved. Efficiency and product consistency.
Patent Information
- Application Number
- CN202410757432.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-13
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2044-06-13
AI Technical Summary
The production cost of hectorite is high, the efficiency of artificial synthesis is low, and the size distribution is not ideal. The existing process cannot get rid of the use of chemical raw materials, resulting in problems of synthesis cost and green process.
The highly active silicon source produced by the depolymerization of natural clay is used to prepare nanohectorite through microwave irradiation. A special depolymerization and synthesis process is adopted in stages, and acidic liquid and microwave irradiation are used to form acidic vapor for reaction, reducing chemical Pharmaceuticals use and increase silicon source activity.
The low-cost, green preparation of nanohectorite is achieved, which improves the synthesis efficiency and product size consistency, reduces the pollution of chemical raw materials, and is suitable for industrial large-scale production.
Smart Images

Figure CN118324153B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of preparation technology of hectorite, and in particular to a preparation method of nano hectorite by microwave irradiation using clay as a raw material. Background Art
[0002] Hectorite is a magnesium-lithium layered silicate mineral, a member of the saponite family in the smectite class. It is composed of two silicon-oxygen tetrahedral layers and a magnesium-oxygen trioctahedral layer in the middle, in which a part of the magnesium ions in the trioctahedral layer are replaced by monovalent lithium ions, and a part of the hydroxide ions are replaced by fluoride ions. Its crystal structure can usually be classified as a 2:1 type structure. Hectorite has excellent colloidal dispersibility, stability, thixotropy and suspension, and is therefore widely used in building materials, food, daily chemicals, nanomaterials, catalysis and other fields, and has high economic value.
[0003] The production of hectorite mainly depends on the purification of natural hectorite. However, due to the scarcity of natural hectorite resources (currently known long-term mining of hectorite is available in a few areas such as Hankto, California, USA) and the limitation of purification process, the production cost of high-purity hectorite is high, which greatly limits its application in some fields. In recent years, some researchers have successfully prepared hectorite to replace natural hectorite for scientific research by simulating the natural conditions of hectorite formation in the laboratory through corresponding processes, such as traditional hydrothermal synthesis methods, or microwave synthesis methods that replace traditional heating forms with microwaves. For example, Zhou Chunhui et al. used lithium fluoride, magnesium chloride, water glass, and ammonia water as raw materials, and successfully synthesized hectorite with LiF, Mg(OH)2, and SiO2 as raw materials (the molar ratio of LiF, Mg(OH)2, and SiO2 is 1.33:5.07:7.70) under hydrothermal conditions of crystallization temperature of 120℃ and crystallization time of 72h. Sun Hongjuan used a hydrothermal synthesis process, with LiOH, MgCl2, and SiO2 as raw materials (the molar ratio of LiOH, MgCl2, and SiO2 was 1:3:1.667), and successfully synthesized lithium soapstone with high crystallinity under the condition of a crystallization temperature of 120°C. These achievements provide valuable experience for the research on artificial synthesis of lithium soapstone. However, affected by the synthesis environment and synthesis method, the efficiency of preparing lithium soapstone is not only low, but also its size is not ideal, showing a chaotic state of morphological size distribution, which seriously affects its use. In addition, existing research cannot get rid of the use of chemical raw materials. For example, in terms of silicon sources, silica sol is usually used, which leads to problems in the artificial synthesis of lithium soapstone from the perspective of synthesis cost and process greening. If a low-cost, green and sustainable high-performance lithium soapstone preparation route can be found, it will be of great significance and practical value for its industrial large-scale production and utilization. Summary of the invention
[0004] In order to solve the problems of high cost of natural hectorite purification, poor performance of synthetic products (such as chaotic size distribution) and low yield of traditional synthesis process in the prior art, the present invention aims to replace the traditional silicon source with the highly active silicon source produced by the depolymerization of natural clay, and to prepare nano hectorite in a green and low-cost manner by taking advantage of the in-situ reconstruction of the elementary structure (i.e., the topological structure of natural clay) remaining after the depolymerization of natural clay. Furthermore, in order to efficiently depolymerize natural clay and synthetic hectorite, a special depolymerization and synthesis process with progressive stages is proposed, namely, the application technology of the present invention: a preparation method for preparing nano hectorite by microwave irradiation using clay as a raw material.
[0005] The present invention is achieved through the following technical solutions:
[0006] A method for preparing nano-hectorite by microwave irradiation using clay as a raw material, the specific steps are as follows:
[0007] S1, selecting natural clay ore, flotation separation and impurity removal, grinding into powder, and then sieving through a 100-mesh sieve to obtain natural clay powder;
[0008] S2, natural clay powder and acid solution are loaded into a microwave digestion tank according to a certain solid-liquid ratio, and the ratio range is natural clay (weight): acid solution (volume) = 1g: 2.5ml~5ml;
[0009] S3, the microwave digestion tank installed in step S2 is loaded into a microwave digestion instrument, and irradiated according to specific irradiation conditions, specifically, the irradiation temperature is 110-200 ℃, and the irradiation cycle is 30;
[0010] S4, take out the microwave digestion tank after microwave irradiation, filter the solid product until it is neutral, and place it in a constant temperature oven at 90°C to dry for 12 hours. The obtained solid powder is the clay-based active silicon source;
[0011] S5, the lithium source, magnesium source, clay-based active silicon source according to the amount of substance ratio of 1:3:1.7 mixed and stirred, transferred to a microwave digestion tank, dropwise addition of ammonia solution to maintain the PH of the reaction system at 9-12;
[0012] S6, the microwave digestion tank is loaded into the microwave digestion instrument, and the irradiation reaction is carried out. The reaction conditions are: the irradiation temperature is 110-180 ° C, and the irradiation cycle is 10-30;
[0013] S7, taking out the microwave digestion tank after microwave irradiation, filtering the solid product to neutrality, and placing it in a constant temperature oven at 90° C. to dry for 12 hours. The obtained solid powder is nano-lithium laponite.
[0014] The natural clay in step S1 is a mixture of one or more of kaolin, montmorillonite and rectorite.
[0015] The acid solution used in step S2 is hydrochloric acid, and its concentration is 2-4 mol / L.
[0016] In step S2, the natural clay and the acid solution are isolated from each other, that is, during the microwave irradiation process, only the acid solution is heated to form acidic steam as the reaction medium.
[0017] The irradiation cycle mentioned in step S3 is specifically that each cycle is 200W irradiation for 10s, 230W irradiation for 10s, 270W irradiation for 10s, 330W irradiation for 10s, 350W irradiation for 10s, and stop for 10s.
[0018] In step S5, the lithium source is one of lithium fluoride and lithium carbonate or a mixture of the two; the magnesium source is one of magnesium chloride and magnesium hydroxide or a mixture of the two.
[0019] The irradiation cycle mentioned in step S6 is as follows: each cycle is 160W irradiation for 20s, 270W irradiation for 10s, 330W irradiation for 10s, 350W irradiation for 10s, and stop for 10s.
[0020] Beneficial effects of the present invention: First, in terms of synthetic raw materials, this method is greener than the current technology of artificially synthesizing lithium soapstone. At present, researchers use high-purity chemical products as raw materials for laboratory synthetic lithium soapstone. For example, in terms of the use of silicon sources, sodium silicate and other chemicals are mostly selected. The synthetic raw materials used in the present invention are not entirely chemical products. The silicon source we use is the silicon element produced by acid depolymerization of natural clay as a synthetic raw material, which to a certain extent alleviates the pollution problem of the upper end of the synthetic raw materials caused by the use of silicon-containing chemicals. In addition, for the depolymerization method of natural clay, we have originally proposed and adopted a superimposed composite process of a solid-phase method and a microwave progressive irradiation method, that is, firstly separate the natural clay from the acid solution in a microwave digestion tank, and use microwave irradiation to heat and evaporate the acid solution to produce acid vapor, and then react with the natural clay. In this way, not only can the low-concentration acid solution play the effect of high-concentration acid solution, effectively improve the use efficiency of the acid solution, but also can realize its multiple recycling by appropriately adding acid solution, avoid large-scale discharge of acid solution, and facilitate industrial-scale production. In addition, under this microwave progressive irradiation environment, affected by the solid-phase system, the natural clay powder is directly irradiated with microwaves. Since different chemical bonds receive microwaves differently, they can be directly activated, and the chemical bond activation and broken parts will be consistent. This is also the reason why natural clay can be depolymerized without a high-temperature activation step in the technology of the present invention. More importantly, compared with an alkaline environment, an acidic depolymerization environment can retain the elementary structure in the crystal structure of natural clay (i.e., the topological structure of natural clay) to the maximum extent, which directly makes it (clay-based active silicon source) show much higher chemical activity than chemicals in the process of synthesizing lithium laponite, prompting it to crystallize into lithium laponite more quickly.
[0021] It is worth noting that in this technology, the fast synthesis speed is only one of the many reasons for selecting the microwave progressive irradiation method. The clay-based active silicon source we obtained has super high activity, so compared with traditional chemical raw materials, it is faster in the generation of the initial crystal nucleus of lithium soapstone. If the traditional microwave synthesis method is directly used, due to the uncontrollable heat supply, the crystal nucleus will quickly grow up through the Oswald reaction after generation, and the lithium soapstone obtained will show the characteristics of chaotic crystal size distribution. However, when using the microwave progressive irradiation method, since the chemical bonds broken by the silicon raw material have consistency, and the heat supply method is regularized, it is beneficial to the uniform crystallization of the synthetic raw materials in the synthesis system in terms of both synthetic materials and synthetic conditions. In other words, the method for protection applied for by the present invention is conducive to controlling the consistency of the initial crystal nucleus generation of lithium soapstone and the controllability of the growth rate, and can simply control the size of the synthesized lithium soapstone by controlling the synthesis cycle, so as to obtain nano lithium soapstone. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] In order to more clearly illustrate the specific embodiments of the present invention or the technical solutions in the prior art, the following is a brief introduction to the drawings required for the specific embodiments or the description of the prior art. In all the drawings, similar elements or parts are generally identified by similar reference numerals. In the drawings, the elements or parts are not necessarily drawn according to the actual scale.
[0023] Figure 1 XRD pattern of the clay-based active silicon source product involved in Example 1.
[0024] Figure 2 XRD patterns of the product hectorite of Examples 1-5.
[0025] from Figure 1 It can be seen that the clay-based active silicon source product presents an amorphous structure, indicating that its inherent crystal structure has been completely depolymerized into active species suitable for synthesizing hectorite.
[0026] Figure 2 1 is the XRD diagram of the product synthesized under the conditions of each embodiment. According to its diffraction peak, it can be determined that the synthesized product is nano-hectorite. DETAILED DESCRIPTION
[0027] In order to clearly and completely describe the technical solution and its specific working process of the present invention, the specific implementation methods of the present invention are as follows in conjunction with the accompanying drawings of the specification:
[0028] Example 1
[0029] This embodiment provides a method for preparing nano-hectorite by microwave irradiation using clay as a raw material, and the specific steps of the method are as follows:
[0030] S1, selecting natural clay ore, flotation and impurity removal, grinding into powder, and then sieving through a 100-mesh sieve to obtain natural clay powder;
[0031] S2, natural clay powder and acid solution are loaded into a microwave digestion tank according to a certain solid-liquid ratio, and the ratio range is natural clay (weight): acid solution (volume) = 1g: 2.5ml;
[0032] S3, the microwave digestion tank installed in step S2 is loaded into a microwave digestion instrument, and irradiated according to specific irradiation conditions, specifically, the irradiation temperature is 200 ° C, and the irradiation cycle is 30;
[0033] S4, take out the microwave digestion tank after microwave irradiation, filter the solid product until it is neutral, and place it in a constant temperature oven at 90°C to dry for 12 hours. The obtained solid powder is the clay-based active silicon source;
[0034] S5, the lithium source, magnesium source, clay-based active silicon source according to the amount of substance ratio of 1:3:1.7 mixed and stirred well, transferred to a microwave digestion tank, ammonia was added dropwise to maintain the PH of the reaction system at 12;
[0035] S6, the loaded microwave digestion tank is loaded into the microwave digestion instrument, and the irradiation reaction is carried out. The reaction conditions are: the irradiation temperature is 110 ° C, and the irradiation cycle is 30;
[0036] S7, taking out the microwave digestion tank after microwave irradiation, filtering the solid product to neutrality, and placing it in a constant temperature oven at 90° C. to dry for 12 hours. The obtained solid powder is nano-lithium laponite.
[0037] Furthermore, the natural clay in step S1 is kaolin.
[0038] Furthermore, the acid solution used in step S2 is hydrochloric acid, and its concentration is 4 mol / L.
[0039] Furthermore, in step S2, the natural clay and the acid solution are isolated from each other, that is, during the microwave irradiation process, only the acid solution is heated to form acidic steam as the reaction medium.
[0040] Furthermore, the irradiation cycle mentioned in step S3, specifically each cycle is 200W irradiation for 10s, 230W irradiation for 10s, 270W irradiation for 10s, 330W irradiation for 10s, 350W irradiation for 10s, and stop for 10s.
[0041] Furthermore, in step S5, the lithium source is lithium carbonate; and the magnesium source is magnesium chloride.
[0042] Furthermore, the irradiation cycle mentioned in step S6 is specifically that each cycle is 160W irradiation for 20s, 270W irradiation for 10s, 330W irradiation for 10s, 350W irradiation for 10s, and stop for 10s.
[0043] Example 2
[0044] This embodiment provides a method for preparing nano-hectorite by microwave irradiation using clay as a raw material, and the specific steps of the method are as follows:
[0045] S1, selecting natural clay ore, flotation removing impurities, grinding into powder, and then sieving through a 100-mesh sieve to obtain natural clay powder;
[0046] S2, natural clay powder and acid solution are loaded into a microwave digestion tank according to a certain solid-liquid ratio, and the ratio range is natural clay (weight): acid solution (volume) = 1g: 2.5 ml;
[0047] S3, the microwave digestion tank installed in step S2 is loaded into a microwave digestion instrument, and irradiated according to specific irradiation conditions, specifically, the irradiation temperature is 200 ° C, and the irradiation cycle is 30;
[0048] S4, take out the microwave digestion tank after microwave irradiation, filter the solid product until it is neutral, and place it in a constant temperature oven at 90°C to dry for 12 hours. The obtained solid powder is the clay-based active silicon source;
[0049] S5, the lithium source, magnesium source, clay-based active silicon source according to the amount of substance ratio of 1:3:1.7 mixed and stirred thoroughly, transferred to a microwave digestion tank, ammonia was added dropwise to maintain the PH of the reaction system at 12;
[0050] S6, the loaded microwave digestion tank is loaded into the microwave digestion instrument, and the irradiation reaction is carried out. The reaction conditions are: the irradiation temperature is 180 ° C, and the irradiation cycle is 10;
[0051] S7, taking out the microwave digestion tank after microwave irradiation, filtering the solid product to neutrality, and placing it in a constant temperature oven at 90° C. to dry for 12 hours. The obtained solid powder is nano-lithium laponite.
[0052] Furthermore, the natural clay in step S1 is montmorillonite.
[0053] Furthermore, the acid solution used in step S2 is hydrochloric acid, and its concentration is 4 mol / L.
[0054] Furthermore, in step S2, the natural clay and the acid solution are isolated from each other, that is, during the microwave irradiation process, only the acid solution is heated to form acidic steam as the reaction medium.
[0055] Furthermore, the irradiation cycle mentioned in step S3, specifically each cycle is 200W irradiation for 10s, 230W irradiation for 10s, 270W irradiation for 10s, 330W irradiation for 10s, 350W irradiation for 10s, and stop for 10s.
[0056] Furthermore, in step S5, the lithium source is lithium fluoride; and the magnesium source is magnesium hydroxide.
[0057] Furthermore, the irradiation cycle mentioned in step S6 is specifically that each cycle is 160W irradiation for 20s, 270W irradiation for 10s, 330W irradiation for 10s, 350W irradiation for 10s, and stop for 10s.
[0058] Example 3
[0059] This embodiment provides a method for preparing nano-hectorite by microwave irradiation using clay as a raw material, and the specific steps of the method are as follows:
[0060] S1, selecting natural clay ore for flotation removal and then sieving through a 100-mesh sieve to obtain natural clay powder;
[0061] S2, natural clay powder and acid solution are loaded into a microwave digestion tank according to a certain solid-liquid ratio, and the ratio range is natural clay (weight): acid solution (volume) = 1g: 5ml;
[0062] S3, the microwave digestion tank installed in step S2 is loaded into a microwave digestion instrument, and irradiated according to specific irradiation conditions, specifically, the irradiation temperature is 110 ° C, and the irradiation cycle is 30;
[0063] S4, take out the microwave digestion tank after microwave irradiation, filter the solid product until it is neutral, and place it in a constant temperature oven at 90°C to dry for 12 hours. The obtained solid powder is the clay-based active silicon source;
[0064] S5, the lithium source, magnesium source, clay-based active silicon source according to the amount of substance ratio of 1:3:1.7 mixed and stirred well, transferred to a microwave digestion tank, ammonia was added dropwise to maintain the PH of the reaction system at 9;
[0065] S6, the loaded microwave digestion tank is loaded into the microwave digestion instrument, and the irradiation reaction is carried out. The reaction conditions are: the irradiation temperature is 180 ° C, and the irradiation cycle is 30;
[0066] S7, taking out the microwave digestion tank after microwave irradiation, filtering the solid product to neutrality, and placing it in a constant temperature oven at 90° C. to dry for 12 hours. The obtained solid powder is nano-lithium laponite.
[0067] Furthermore, the natural clay in step S1 is rectorite.
[0068] Furthermore, the acid solution used in step S2 is hydrochloric acid, and its concentration is 4 mol / L.
[0069] Furthermore, in step S2, the natural clay and the acid solution are isolated from each other, that is, during the microwave irradiation process, only the acid solution is heated to form acidic steam as the reaction medium.
[0070] Furthermore, the irradiation cycle mentioned in step S3, specifically each cycle is 200W irradiation for 10s, 230W irradiation for 10s, 270W irradiation for 10s, 330W irradiation for 10s, 350W irradiation for 10s, and stop for 10s.
[0071] Furthermore, in step S5, the lithium source is lithium carbonate; and the magnesium source is magnesium chloride.
[0072] Furthermore, the irradiation cycle mentioned in step S6 is specifically that each cycle is 160W irradiation for 20s, 270W irradiation for 10s, 330W irradiation for 10s, 350W irradiation for 10s, and stop for 10s.
[0073] Example 4
[0074] This embodiment provides a method for preparing nano-hectorite by microwave irradiation using clay as a raw material, and the specific steps of the method are as follows:
[0075] S1, selecting natural clay ore, flotation and impurity removal, grinding into powder, and then sieving through a 100-mesh sieve to obtain natural clay powder;
[0076] S2, natural clay powder and acid solution are loaded into a microwave digestion tank according to a certain solid-liquid ratio, and the ratio range is natural clay (weight): acid solution (volume) = 1:5 g / ml;
[0077] S3, the microwave digestion tank installed in step S2 is loaded into a microwave digestion instrument, and irradiated according to specific irradiation conditions, specifically, the irradiation temperature is 110 ° C, and the irradiation cycle is 30;
[0078] S4, take out the microwave digestion tank after microwave irradiation, filter the solid product until it is neutral, and place it in a constant temperature oven at 90°C to dry for 12 hours. The obtained solid powder is the clay-based active silicon source;
[0079] S5, the lithium source, magnesium source, clay-based active silicon source according to the amount of substance ratio of 1:3:1.7 mixed and stirred thoroughly, transferred to a microwave digestion tank, ammonia was added dropwise to maintain the PH of the reaction system at 12;
[0080] S6, the loaded microwave digestion tank is loaded into the microwave digestion instrument, and the irradiation reaction is carried out. The reaction conditions are: the irradiation temperature is 180 ° C, and the irradiation cycle is 10;
[0081] S7, taking out the microwave digestion tank after microwave irradiation, filtering the solid product to neutrality, and placing it in a constant temperature oven at 90° C. to dry for 12 hours. The obtained solid powder is nano-lithium laponite.
[0082] Furthermore, the natural clay in step S1 is rectorite.
[0083] Furthermore, the acid solution used in step S2 is hydrochloric acid, and its concentration is 4 mol / L.
[0084] Furthermore, in step S2, the natural clay and the acid solution are isolated from each other, that is, during the microwave irradiation process, only the acid solution is heated to form acidic steam as the reaction medium.
[0085] Furthermore, the irradiation cycle mentioned in step S3, specifically each cycle is 200W irradiation for 10s, 230W irradiation for 10s, 270W irradiation for 10s, 330W irradiation for 10s, 350W irradiation for 10s, and stop for 10s.
[0086] Furthermore, in step S5, the lithium source is lithium carbonate; and the magnesium source is magnesium hydroxide.
[0087] Furthermore, the irradiation cycle mentioned in step S6 is specifically that each cycle is 160W irradiation for 20s, 270W irradiation for 10s, 330W irradiation for 10s, 350W irradiation for 10s, and stop for 10s.
[0088] Example 5
[0089] This embodiment provides a method for preparing nano-hectorite by microwave irradiation using clay as a raw material, and the specific steps of the method are as follows:
[0090] S1, selecting natural clay ore, flotation removing impurities, grinding into powder, and then sieving through a 100-mesh sieve to obtain natural clay powder;
[0091] S2, natural clay powder and acid solution are loaded into a microwave digestion tank according to a certain solid-liquid ratio, and the ratio range is natural clay (weight): acid solution (volume) = 1:5 g / ml;
[0092] S3, the microwave digestion tank installed in step S2 is loaded into a microwave digestion instrument, and irradiated according to specific irradiation conditions, specifically, the irradiation temperature is 200 ° C, and the irradiation cycle is 10;
[0093] S4, take out the microwave digestion tank after microwave irradiation, filter the solid product until it is neutral, and place it in a constant temperature oven at 90°C to dry for 12 hours. The obtained solid powder is the clay-based active silicon source;
[0094] S5, the lithium source, magnesium source, clay-based active silicon source according to the amount of substance ratio of 1:3:1.7 mixed and stirred well, transferred to a microwave digestion tank, ammonia was added dropwise to maintain the PH of the reaction system at 9;
[0095] S6, the loaded microwave digestion tank is loaded into the microwave digestion instrument, and the irradiation reaction is carried out. The reaction conditions are: the irradiation temperature is 180 ° C, and the irradiation cycle is 30;
[0096] S7, taking out the microwave digestion tank after microwave irradiation, filtering the solid product to neutrality, and placing it in a constant temperature oven at 90° C. to dry for 12 hours. The obtained solid powder is nano-lithium laponite.
[0097] Furthermore, the natural clay in step S1 is rectorite.
[0098] Furthermore, the acid solution used in step S2 is hydrochloric acid, and its concentration is 2 mol / L.
[0099] Furthermore, in step S2, the natural clay and the acid solution are isolated from each other, that is, during the microwave irradiation process, only the acid solution is heated to form acidic steam as the reaction medium.
[0100] Furthermore, the irradiation cycle mentioned in step S3, specifically each cycle is 200W irradiation for 10s, 230W irradiation for 10s, 270W irradiation for 10s, 330W irradiation for 10s, 350W irradiation for 10s, and stop for 10s.
[0101] Furthermore, in step S5, the lithium source is lithium carbonate; and the magnesium source is magnesium hydroxide.
[0102] Furthermore, the irradiation cycle mentioned in step S6 is specifically that each cycle is 160W irradiation for 20s, 270W irradiation for 10s, 330W irradiation for 10s, 350W irradiation for 10s, and stop for 10s.
[0103] Finally, it should be noted that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for preparing nano-hectorite by microwave irradiation using clay as raw material, It is characterized in that The specific steps are as follows: S1, selecting natural clay ore, flotation and impurity removal, grinding into powder, and then sieving through a 100-mesh sieve to obtain natural clay powder; S2, natural clay powder and acid solution are loaded into a microwave digestion tank according to a certain solid-liquid ratio, and the ratio range is natural clay: acid solution = 1g: 2.5ml~5ml; S3, loading the microwave digestion vessel prepared in step S2 into a microwave digestion instrument, and irradiating the microwave digestion vessel according to specific irradiation conditions, specifically, the irradiation temperature is 110-200° C., and the irradiation cycle is 30; S4, taking out the microwave digestion tank after microwave irradiation, filtering the solid product until it is neutral, and placing it in a constant temperature oven at 90° C. to dry for 12 hours. The obtained solid powder is the clay-based active silicon source; S5, mixing the lithium source, magnesium source, and clay-based active silicon source in a molar ratio of 1:3:1.7 and stirring thoroughly, transferring the mixture to a microwave digestion tank, and adding ammonia water dropwise to maintain the pH of the reaction system at 9-12; S6, loading the prepared microwave digestion tank into a microwave digestion instrument for irradiation reaction, the reaction conditions are: irradiation temperature of 110-180°C, irradiation cycle of 10-30; S7, taking out the microwave digestion tank after microwave irradiation, filtering the solid product to neutrality, and placing it in a constant temperature oven at 90° C. to dry for 12 hours, and the obtained solid powder is nano-hectorite; The natural clay in step S1 is a mixture of one or more of kaolin, montmorillonite and rectorite; The acid solution used in step S2 is hydrochloric acid, and its concentration is 2-4 mol / L; In step S2, the natural clay and the acid solution are isolated from each other, that is, during the microwave irradiation process, only the acid solution is heated to form acidic steam as the reaction medium; The irradiation cycle mentioned in step S3 is specifically that each cycle is 200w irradiation for 10s, 230w irradiation for 10s, 270w irradiation for 10s, 330w irradiation for 10s, 350w irradiation for 10s, and stop for 10s; The irradiation cycle mentioned in step S6 is as follows: each cycle is 160W irradiation for 20s, 270W irradiation for 10s, 330W irradiation for 10s, 350W irradiation for 10s, and stop for 10s.
2. According to claim 1, a method for preparing nano-hectorite by microwave irradiation using clay as a raw material, It is characterized in that In step S5, the lithium source is one of lithium fluoride and lithium carbonate or a mixture of the two; the magnesium source is one of magnesium chloride and magnesium hydroxide or a mixture of the two.