A self-repairing cement-based material based on mineralization of Bacillus sphaericus and its preparation method and application

Through the microbial self-repair technology combined with Bacillus spherical fibers, the problems of environmental pollution and high cost in crack repair in traditional concrete structures are solved, and efficient and environmentally friendly concrete self-repair is achieved, which significantly improves compressive flexural strength and durability. sex.

CN118324461BActive Publication Date: 2024-11-26WUHAN TEXTILE UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410442849.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-04-12
Publication Date
2024-11-26
Estimated Expiration
2044-04-12

AI Technical Summary

Technical Problem

Traditional concrete structures are prone to tiny cracks during long-term use, resulting in invasion of harmful external media, causing structural losses and safety hazards. In addition, traditional restoration methods have problems of environmental pollution and high costs.

Method used

Using Bacillus spherical microbial self-healing technology, the calcium carbonate deposition is induced through nitrogen cycle, and a self-healing cement-based material is prepared by combining Bacillus spherical and cattail fibers to improve the compressive flexural strength and durability of concrete. and achieve environmentally friendly crack repair.

Benefits of technology

It significantly improves the compressive flexural strength and durability of concrete, enhances the self-repairing ability of materials, reduces the risk of environmental pollution, and realizes the resource utilization of waste fibers, providing an environmentally friendly and low-cost construction convenience solution. plan.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004789746190000101
    Figure BDA0004789746190000101
  • Figure BDA0004789746190000121
    Figure BDA0004789746190000121
  • Figure HDA0004789746200000011
    Figure HDA0004789746200000011
Patent Text Reader

Abstract

The present invention relates to the technical field of building materials, and specifically discloses a self-repairing cement-based material based on the mineralization of Bacillus sphaericus, and a preparation method and application thereof. The present invention screens out the microbial mineralization strain Bacillus sphaericus, and optimizes the culture medium formula for culturing the Bacillus sphaericus to produce calcium carbonate, and obtains the "MBS culture medium engineering version", whose components are: 4.8g KH2PO4, 0.2g CaCl2, 0.2gMgSO4, 6g peptone and 2g yeast extract per liter of water, and the solution pH = 7.2. The culture medium is simple in composition and low in cost relative to the LB culture medium. The present invention applies Bacillus sphaericus to the microbial self-repair of microcracks in cement concrete. Further, Bacillus sphaericus is combined with cattail grass fiber to the microbial self-repair of microcracks in cement concrete, which will improve the compressive and flexural strength of cement-based materials and have a good microcrack self-repair effect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of building materials, and in particular to a self-repairing cement-based material based on mineralization of Bacillus sphaericus and a preparation method and application thereof. Background Art

[0002] With the development of the world economy and the continuous improvement of the level of modernization, the construction scale of various construction projects around the world is constantly expanding. Concrete is widely used in modern civil engineering construction activities due to its excellent compressive strength, superior durability, convenient production methods and low production costs. However, concrete will inevitably produce local damage such as micro cracks during long-term use and under the influence of the surrounding complex environment. If these damages cannot be repaired in time with appropriate means, harmful media from the outside will continue to invade the structure through the concrete cracks, causing corrosion of the reinforcement in the building and damage to the internal structure, ultimately causing the loss of mechanical properties and durability of the concrete structure, and in severe cases leading to safety accidents. Traditional crack repair methods such as surface treatment, filling and grouting have certain limitations in repairing micro cracks in concrete, and some chemical reagents used in the repair process are harmful to the environment. Microbial-induced calcite precipitation (MICP) technology has the advantages of low production energy consumption, low carbon and environmental protection, and has gradually attracted the attention of domestic scholars. Microbial repair technology for concrete cracks is based on the principle of MICP technology, using microorganisms to deposit calcium carbonate to achieve the purpose of filling and repairing cracks. Compared with other restoration methods, the restoration process will not cause harm to the environment and has great potential in the future.

[0003] Microbial self-repair uses the metabolism of microorganisms to induce the formation of insoluble substances such as carbonate crystals to fill concrete cracks to achieve self-repair effects. The main difference between it and capsule self-repair is the type of repair agent used and the mechanism of action. Microorganisms can also use capsules as carriers. The main role of microorganisms in the self-repair process is to provide reactants for mineralization reactions and provide nucleation points for the precipitation of minerals such as calcium carbonate.

[0004] Common MICP mineralization mechanisms include: photosynthesis-induced calcium carbonate deposition, sulfate-reducing bacteria-induced calcium carbonate deposition, nitrogen cycle-induced calcium carbonate deposition, etc. Compared with other deposition mechanisms, nitrogen cycle-induced calcium carbonate deposition has special application advantages. Bacillus pasteurianus, Bacillus sphaericus, etc. are representative bacterial genera for nitrogen cycle-induced calcium carbonate deposition. Such bacteria can produce urease, a key protease with the ability to induce mineralization, through metabolism. When the urea content in the environment is high, the urea molecule will be hydrolyzed into ammonia molecules and carbamic acid molecules under the action of urease inside the bacteria; as an intermediate product in the process, one molecule of carbamic acid will spontaneously hydrolyze into one molecule of carbonic acid and one molecule of ammonia in a very short time. In the above reaction, ammonia molecules will react with water to increase the alkalinity of the water environment. The increase in alkalinity promotes the conversion of inorganic carbon dissolved in water into carbonate ions, which ultimately increases the concentration of carbonate ions in the environment and generates calcium carbonate in the presence of a calcium source. Since nitrogen bacteria have good alkaline resistance and benefit from their spore-forming ability, they can survive for hundreds of years without nutrients. Therefore, nitrogen bacteria have the potential to effectively repair concrete cracks in the long term. However, the ability of existing microbial self-repair of concrete microcracks is limited. This article, through the study of self-repairing cement-based materials combined with fiber and Bacillus, can provide a theoretical basis for the application of fiber and microorganisms in construction engineering technology, promote the resource utilization of waste fiber, promote innovation in construction engineering technology, and achieve sustainable development. Summary of the invention

[0005] In view of the deficiencies in the prior art, the purpose of the present invention is to provide a self-repairing cement-based material based on the mineralization of Bacillus sphaericus and its preparation method and application. The self-repairing cement-based material based on the mineralization of Bacillus sphaericus of the present invention has the advantages of improved strength and toughness, enhanced durability, flexibility and plasticity, environmental friendliness and construction convenience compared with traditional cement-based materials. In order to achieve the above purpose, the present invention adopts the following technical solution:

[0006] Technical solution 1: Application of Bacillus sphaericus in microbial self-repair of microcracks in cement concrete, including the following steps:

[0007] Take the powder of microbial mineralization strain Bacillus sphaeroides and add it to the MBS medium engineering version for activation culture until the bacterial solution OD 600=1±0.1, then put the bacterial solution into a water bath at 80-100°C for 30-60 minutes to convert the bacterial solution into a spore solution; the obtained spore solution of Bacillus sphaericus is used to replace part of the water used in the preparation process of cement concrete and mixed with cement, urea and anhydrous calcium chloride in proportion. The components of the engineering version of the above-mentioned MBS medium are: 4.8gKH2PO4, 0.2gCaCl2, 0.2g MgSO4, 6g peptone and 2g yeast extract per liter of water, and the solution pH = 7.2 (preferably using 1mol / LNaOH solution to adjust the pH).

[0008] Furthermore, the water-cement ratio in the system is 0.3; the amount of urea added is 0.8% to 1% of the mass of cement, preferably 0.8%; the amount of anhydrous calcium chloride added is 1% to 2% of the mass of cement, preferably 1.5%; the mass of the spore liquid of Bacillus sphaericus accounts for 10% to 80% of the mass of the total liquid in the system, preferably 70% to 75%. Technical solution 2: Application of Bacillus sphaericus combined with cattail grass fiber in microbial self-repair of microcracks in cement concrete, including the following steps:

[0009] Take the powder of microbial mineralization strain Bacillus sphaeroides and add it to the MBS medium engineering version for activation culture until the bacterial solution OD 600 =1±0.1, and then put the bacterial liquid into a water bath at 80-100°C for 30-60min to convert the bacterial liquid into a spore liquid; wash, shear, dry, and crush the cattail leaves, and pass them through a 60-mesh sieve to obtain cattail fiber; take the cattail fiber and immerse it in the spore liquid of the spherical Bacillus obtained above, and then load it on a shaking table at 25-30°C and 120-150rpm for 4-6h, and then dry it at 30-40°C to constant weight to obtain a cattail fiber-loaded Bacillus material; mix the obtained cattail fiber-loaded Bacillus material with cement, urea, and anhydrous calcium chloride evenly, and then mix them with water in proportion to prepare cement concrete.

[0010] The components of the engineering version of the MBS medium are as follows: 4.8 g KH2PO4, 0.2 g CaCl2, 0.2 g MgSO4, 6 g peptone and 2 g yeast extract per liter of water, and the solution pH = 7.2 (preferably adjusted with 1 mol / L NaOH solution).

[0011] Furthermore, the water-cement ratio in the system is 0.3; the amount of cattail grass fiber added is 0.1% to 0.15% of the cement mass; the amount of urea added is 0.8% to 1% of the cement mass, preferably 0.8%; the amount of anhydrous calcium chloride added is 1% to 2% of the cement mass, preferably 1.5%.

[0012] In specific application, one of the technical solutions: application of Bacillus sphaericus in microbial self-repair of microcracks in cement concrete includes the following steps:

[0013] (1) Preparation of spherical Bacillus spore liquid: Take the microbial mineralization strain spherical Bacillus powder, add it into the MBS medium engineering version for activation culture until the bacterial liquid OD 600 =1±0.1, and then put the bacterial solution into a water bath at 80-100°C for 30-60min to convert the bacterial solution into a spore solution for standby use; the MBS medium engineering version comprises: 4.8g KH2PO4, 0.2g CaCl2, 0.2g MgSO4, 6g peptone and 2g yeast extract per liter of water, and the solution pH = 7.2 (preferably using 1mol / L NaOH solution to adjust the pH);

[0014] (2) Pre-wetting the mixing pot and mixing blades of the cement mortar mixer, pouring cement, urea and anhydrous calcium chloride into the mixing pot and slowly stirring until uniformly mixed, then slowly pouring in the spore liquid of Bacillus sphaericus and water, stirring to obtain uniformly mixed cement mortar; the water-cement ratio in the system is 0.3; the amount of urea added is 0.8% to 1% of the mass of cement, preferably 0.8%; the amount of anhydrous calcium chloride added is 1% to 2% of the mass of cement, preferably 1.5%; the mass of the spore liquid of Bacillus sphaericus accounts for 10% to 80% of the mass of the total liquid in the system, preferably 70% to 75%;

[0015] (3) Pour the evenly mixed cement mortar into the mold and shake out the bubbles;

[0016] (4) After the specimens were formed, they were cured to obtain a self-healing cement-based material based on the mineralization of Bacillus sphaericus.

[0017] In order to further improve the self-repairing effect of cement-based materials, fibers are added to cement-based materials. Specifically, the second technical solution: application of Bacillus sphaericus combined with cattail grass fibers in microbial self-repair of concrete microcracks includes the following steps:

[0018] S1 Preparation of cattail fiber loaded Bacillus material: Take the microbial mineralization strain spherical Bacillus powder, add it into the MBS medium engineering version for activation and culture until the bacterial solution OD 600=1±0.1, then put the bacterial liquid into a water bath at 80-100°C for 30-60min to convert the bacterial liquid into a spore liquid for later use; wash, shear, dry, and crush the cattail leaves, and pass them through a 60-mesh sieve to obtain cattail fiber for later use; take the cattail fiber and immerse it in the spore liquid of Bacillus sphaericus (the spore liquid of Bacillus sphaericus added should be enough to immerse the cattail fiber), then load it on a shaking table at 25-30°C and 120-150rpm for 4-6h, and then dry it at 30-40°C to constant weight to obtain the cattail fiber loaded with Bacillus sphaericus material; S 2. Pre-wetting the mixing pot and the mixing blades of the cement mortar mixer, pouring cement, urea, anhydrous calcium chloride and cattail fiber loaded Bacillus material into the mixing pot, slowly stirring until uniformly mixed, and then slowly pouring water and stirring to obtain uniformly mixed cement mortar; the water-cement ratio in the system is 0.3; the amount of cattail fiber added in step S1 is 0.1% to 0.15% of the mass of cement; the amount of urea added is 0.8% to 1% of the mass of cement, preferably 0.8%; the amount of anhydrous calcium chloride added is 1% to 2% of the mass of cement, preferably 1.5%;

[0019] S3 pours the evenly mixed cement mortar into the mold to shake out the bubbles; S4 cures the specimen after it is formed to obtain a self-healing cement-based material based on the mineralization of Bacillus sphaericus.

[0020] Technical solution three: A self-repairing cement-based material based on the mineralization of Bacillus sphaericus, comprising the following steps: mixing cement, urea, anhydrous calcium chloride with the spore liquid of Bacillus sphaericus in the above application and water to obtain a uniformly mixed cement mortar; or mixing cement, urea, anhydrous calcium chloride with the cattail fiber-loaded Bacillus material in the above application and water to obtain a uniformly mixed cement mortar.

[0021] Compared with the prior art, the present invention has the following advantages and beneficial effects: (1) The traditional treatment method for cracks in concrete structures is mainly regular maintenance and repair. Commonly used repair methods include surface treatment, filling and sealing, pressure grouting, etc. Different repair methods are generally used according to the crack characteristics, width and environment of the concrete structure. Most of these repair methods use inorganic materials (cement, etc.) and organic materials (epoxy resin, methacrylate resin, polyurethane, etc.) to repair cracks. In engineering practice, they have achieved certain treatment effects, but there are also a series of problems, such as poor bonding ability between repair materials and concrete; poor workability of organic materials and cement-based materials, low durability, poor anti-aging performance, and organic materials contain harmful substances. During use, they will cause pollution to the surrounding environment and endanger human health. The process is complicated and the repair cost is high. Environmentally friendly mineralization technology has become a new research direction. In nature, microorganisms play an important role in the formation of sedimentary rock minerals such as limestone. In the process of rock formation, the chemical reaction of microbial mineralization does not cause damage to the natural environment, and its environmental friendliness has been fully proven. Compared with other repair methods, MICP technology has the advantages of low energy consumption and low carbon and environmental protection. The present invention selects the microbial mineralization strain Bacillus sphaericus, and optimizes the culture medium formula for cultivating the Bacillus sphaericus to produce calcium carbonate, and obtains the "MBS culture medium engineering version". The culture medium is simpler in composition and low in cost compared to the LB culture medium. The spore liquid of Bacillus sphaericus cultured in the "MBS culture medium engineering version" is directly added to cement, which will increase the compressive and flexural strength of cement-based materials. A small amount of calcium carbonate will be accompanied by the cracks 7 days after the prefabricated cracks are repaired, and it is not easy to fall off. The crack surface is smooth and flat, and the self-repair effect is good.

[0022] (2) The raw materials required for the cattail fiber-loaded Bacillus sphaericus material are environmentally friendly, the preparation process is simple, the preparation cost is low, and the resource utilization of waste fiber materials is realized. The present invention applies Bacillus sphaericus combined with cattail fiber to the microbial self-repair of concrete microcracks, which can significantly improve the compressive and flexural strengths of cement-based materials. After 7 days of prefabricated crack repair, calcium carbonate precipitation can be clearly seen on the crack surface. The repair effect is obvious, the crack surface is relatively smooth, and the repair effect is better than that of the cement test block that is only mixed with the Bacillus sphaericus spore liquid cultured in the engineering version of MBS culture medium.

[0023] (3) The self-repairing cement-based material prepared by the present invention with cattail fiber loaded with spherical Bacillus has advantages over traditional cement-based materials in terms of improved strength and toughness, enhanced durability, flexibility and plasticity, environmental friendliness, and ease of construction, etc. This makes the material have a wide range of application potentials in construction and civil engineering. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1This is a graph showing the production of calcium carbonate from urea hydrolysis promoted by different Bacillus species.

[0025] Figure 2 This is a graph showing the effects of different components in MBS culture medium on the production and yield of calcium carbonate. Figure 3 This is a graph showing the effect of different KH2PO4 concentrations in MBS medium on the production and yield of calcium carbonate. Figure 4 This is a graph showing the effect of different MgSO4 concentrations in MBS culture medium on the production and yield of calcium carbonate. Figure 5 This is a graph showing the effect of different peptone concentrations in MBS medium on the production and yield of calcium carbonate. Figure 6 This is a graph showing the effect of different yeast extract concentrations in MBS medium on the production and yield of calcium carbonate.

[0026] Figure 7 The compressive and flexural strength diagrams of microbial self-repairing cement-based materials under different culture media. Figure 8 This is a graph showing the compressive and flexural strength of Bacillus-based cement materials added with different strengthening components under LB culture medium.

[0027] Fig. 9 These are the self-healing effects of cement-based materials under different culture media. DETAILED DESCRIPTION

[0028] The applicant will further explain the technical solution of the present invention in detail in conjunction with specific embodiments. It should be understood that the following content should not be interpreted as limiting the scope of protection of the present invention in any way. In view of the deficiencies in the prior art, the applicant has conducted a series of scientific experiments and verifications, and provided a microorganism and culture medium formula suitable for the self-repairing field of cement-based materials, confirming that the formula can economically and efficiently promote the production of calcium carbonate by Bacillus sphaericus, and provide an engineering-applicable microbial loading method for cement self-repairing and a method for preparing a microbial self-repairing cement-based material, and preliminarily verified the engineering use of the above-mentioned cement-based material in the field of crack repair, and determined that the material has the advantages of high strength, self-repairing, enhanced durability, environmental friendliness and construction convenience compared to traditional cement-based materials. This makes the material have a wide range of application potential in construction engineering and civil engineering. The LB medium used in the following examples is prepared as follows: take 5g yeast extract, 10g peptone, 10g sodium chloride, add water to 1L, adjust pH=7.2 with 1mol / L NaOH solution, and then sterilize at 121℃ in a high-pressure steam sterilizer for 20min.

[0029] The sources of the microbial mineralization strains involved in the following examples are: Bacillus C3-41 strain was provided by the laboratory of Researcher Yuan Zhiming of Wuhan Institute of Virology; Bacillus subtilis was a commercial standard strain; and Bacillus cereus was isolated and identified in the laboratory.

[0030] Example 1 The experiment of screening the influence of Bacillus species on the production of calcium carbonate by LB medium comprises the following steps:

[0031] (1) Take 1 mg of each of the microbial mineralization strains Bacillus sphaericus, Bacillus subtilis, and Bacillus cereus powder, add them to 100 mL of LB medium for activation, and inoculate the bacterial solution into the LB medium at a 2% inoculum after activation, and cultivate the bacterial solution until the concentration of OD 600 =1, then put the bacterial solution into a water bath at 80℃ for 30min to convert the bacterial solution into spore solution for later use;

[0032] (2) The three spore solutions obtained in step (1) were added to conical flasks in the amounts listed in the seven groups in Table 1 below, and each group was repeated three times. Then, a binder solution (a mixture of 5 mL of 3 mol / L calcium chloride aqueous solution and 5 mL of 3 mol / L urea aqueous solution) was added and cultured on a shaking table for 48 h (150 rpm, 30° C.), centrifuged, the supernatant was discarded, and the precipitate was placed in an oven at 60° C. and dried until the mass was constant, and the mass of calcium carbonate was weighed. The calcium carbonate yield was then calculated as the mass of calcium carbonate / system volume.

[0033] Table 1

[0034] Group Bacillus sphaericus spore solution / mL Bacillus subtilis spore solution / mL Bacillus cereus spore solution / mL 1 0 0 90 2 0 90 0 3 90 0 0 4 45 45 0 5 45 0 45 6 0 45 45 7 30 30 30

[0035] The yield of calcium carbonate produced by urea hydrolysis promoted by different Bacillus species is shown in Figure 1 .Depend on Figure 1 It can be seen that the yield of calcium carbonate produced by urea hydrolysis promoted by Bacillus sphaericus is 22.7 g / L, which is much higher than the yield of calcium carbonate produced by urea hydrolysis promoted by Bacillus cereus (5.3 g / L) and the yield of calcium carbonate produced by urea hydrolysis promoted by Bacillus subtilis (5.0 g / L). The combined application of Bacillus sphaericus with Bacillus cereus and / or Bacillus subtilis also cannot promote the yield of calcium carbonate produced by urea hydrolysis. Under the given conditions in this example, the calcium carbonate yield of Bacillus pasteurianus is about 10 g / L, which is much lower than that of Bacillus sphaericus.

[0036] Example 2 The experiment of the effect of MBS medium and optimized MBS medium on the calcium carbonate production produced by Bacillus sphaericus comprises the following steps:

[0037] (1) Take 1 mg of microbial mineralization strain Bacillus sphaericus powder and add it to 100 mL of MBS medium for activation. After activation, inoculate the bacterial solution into the MBS medium at a 2% inoculum volume and cultivate the bacterial solution until the concentration of OD 600 =1, then put the bacterial liquid into a water bath at 80℃ for 30min to convert the bacterial liquid into spore liquid for later use; (2) take 90mL of the spore liquid obtained in step (1), add a binder (a mixture of 5mL 3mol / L calcium chloride aqueous solution and 5mL 3mol / L urea aqueous solution), shake and culture for 48h (150rpm, 30℃), centrifuge, discard the supernatant, put the precipitate into an oven at 60℃ and dry it to constant weight, weigh and obtain the calcium carbonate yield, which is 7.1g. This group of experiments serves as the control group;

[0038] (3) Repeat steps (1) and (2), and perform an optimization experiment by adjusting only the components in the MBS medium used for activating and culturing the strain in step (1).

[0039] The MBS medium used for activating and culturing the strain in step (1) is prepared as follows: 1) Prepare Solution 1: Take 2g MnSO4·H2O and 2g ZnSO4·7H2O, add appropriate amount of water to mix, then add water to 1L for standby; Prepare Solution 2: Take 2g Fe2(SO4)3, 105mL H2O and 3mL 98wt% H2SO4, mix, heat for 4min, filter, add water to the filtrate to 1L for standby. 2) Weigh 6.8g KH2PO4, 10g peptone, 2.0g yeast extract, 0.3g MgSO4, 0.2g CaCl2 and measure 10mL Solution 1 and 10mL Solution 2, mix well, then add water to 1L, adjust pH to 7.2 with 1mol / L NaOH solution, and then sterilize at 121°C in a high pressure steam sterilizer for 20min to obtain the MBS medium.

[0040] Specifically, the optimization experiments in step (3) are as follows:

[0041] 1) KH2PO4, MgSO4, Solution 1, and Solution 2 were omitted from the MBS medium, and the calcium carbonate production of each group of experiments was weighed. The effects of different components in the MBS medium on the production and yield of calcium carbonate are shown in Figure 2. Figure 2 MBS medium can promote the production of calcium carbonate produced by urea hydrolysis more than LB medium. In this example and the following examples, the mass of calcium carbonate is directly used as the calcium carbonate yield. The calcium carbonate yield is calculated as the actual mass of calcium carbonate / theoretical mass of calcium carbonate × 100%. Figure 2It can be seen that Solution 1 and Solution 2 have little effect on the production of calcium carbonate. Therefore, the concentration of KH2PO4, peptone, yeast extract, MgSO4 and other components in MBS medium are separately studied to explore the effect of calcium carbonate production.

[0042] 2) Solution 1 and Solution 2 were omitted in the MBS medium, and the concentration of KH2PO4 was adjusted to 3.8 g / L, 4.8 g / L, 5.8 g / L, 6.8 g / L, 7.8 g / L, and 8.8 g / L, respectively. The pH was adjusted to 7.2 with 1 mol / L NaOH solution, and then sterilized in a high-pressure steam sterilizer at 121°C for 20 min. The effect of different KH2PO4 concentrations in MBS medium on the yield and yield of calcium carbonate Figure 3 As shown. Figure 3 It can be seen that when the concentration of KH2PO4 in MBS culture medium is 4.8g / L, the yield of calcium carbonate is the highest.

[0043] 3) Solution 1 and Solution 2 were omitted in the MBS medium, and the concentration of MgSO4 was adjusted to 0.1 g / L, 0.2 g / L, 0.3 g / L, 0.4 g / L, and 0.5 g / L, respectively. The pH was adjusted to 7.2 with 1 mol / L NaOH solution, and then sterilized in a high-pressure steam sterilizer at 121°C for 20 min. The effect of different MgSO4 concentrations in MBS medium on the yield and yield of calcium carbonate Figure 4 As shown. Figure 4 It can be seen that when the concentration of MgSO4 in MBS culture medium is 0.2g / L, the yield of calcium carbonate is the highest.

[0044] 4) Solution 1 and Solution 2 were omitted in the MBS medium, and the concentration of peptone was adjusted to 5 g / L, 6 g / L, 7 g / L, 8 g / L, 9 g / L, and 10 g / L, respectively. The pH was adjusted to 7.2 with 1 mol / L NaOH solution, and then sterilized in a high-pressure steam sterilizer at 121°C for 20 min. Effects of different peptone concentrations in MBS medium on the yield and yield of calcium carbonate Figure 5 As shown. Figure 5 It can be seen that when the concentration of peptone in MBS medium is 6g / L, the yield of calcium carbonate is the highest.

[0045] 5) Solution 1 and Solution 2 were omitted in the MBS medium, and the concentration of yeast extract was adjusted to 0.5 g / L, 1 g / L, 1.5 g / L, 2 g / L, 2.5 g / L, and 3 g / L, respectively. The pH was adjusted to 7.2 with 1 mol / L NaOH solution, and then sterilized in a high-pressure steam sterilizer at 121°C for 20 min. Effects of different yeast extract concentrations in MBS medium on the yield and yield of calcium carbonate Figure 6 As shown. Figure 6 It can be seen that when the concentration of yeast extract in the MBS medium is 2g / L, the calcium carbonate production is the highest. Based on the results of various MBS mediums on the calcium carbonate production of Bacillus sphaericus, the optimized MBS medium for culturing Bacillus sphaericus to produce calcium carbonate is obtained, and its components are: 4.8g / L KH2PO4, 0.2g / L CaCl2, 0.2g / LMgSO4, 6g / L peptone, 2g / L yeast extract, see Table 2 below, and then adjust the pH to 7.2 with 1mol / L NaOH solution, sterilize, and the result is obtained. The optimized MBS medium is referred to as the "MBS medium engineering version" below. Compared with the LB medium components, the components of the MBS medium engineering version reduce the amount of peptone by 40%, the amount of yeast extract by 60%, and the total economic cost by about 40.9%.

[0046] Table 2

[0047]

[0048]

[0049] Example 3 The strength test of microbial self-repairing cement-based materials under different culture media includes the following steps:

[0050] (1) Take 1 mg of the microbial mineralization strain Bacillus sphaericus powder and add it to 100 mL of LB medium for activation. After activation, inoculate the bacterial solution into the LB medium at a 2% inoculum volume and culture the bacterial solution until the OD 600 =1, and then put the bacterial liquid into a water bath at 80°C for 30 minutes to convert the bacterial liquid into spore liquid for standby use; (2) pre-wetting the mixing pot and mixing blades of the cement mortar mixer, pouring 1500g of cement, 12g of urea, and 22g of anhydrous calcium chloride into the mixing pot and slowly stirring until uniformly mixed, then slowly pouring 125g of water and 325g of the spore liquid prepared in step (1), with a water-cement ratio of 0.3, slowly stirring for 30s, and then starting to quickly stir for 120s to obtain a uniformly mixed cement mortar;

[0051] (3) Apply a thin layer of silicone oil on the inner surface of a 160 mm × 40 mm × 40 mm mold (to facilitate demoulding later), then pour the uniformly mixed cement mortar obtained in step (2) into the mold, shake out bubbles (to prevent the flexural strength of the cement test block from being reduced due to bubbles), and use a metal scraping ruler to scrape it flat;

[0052] (4) After the specimens are formed, they are cured in a cement concrete constant temperature and humidity standard curing box at a temperature of 30°C ± 2°C and a relative humidity of 98% for 24 hours, the specimens are numbered and demolded, and after demolding, they are continued to be placed in the aforementioned standard curing box for curing for 7 days to obtain an LB-based microbial self-repairing cement-based material; in addition, steps (1) to (4) are repeated, and only the culture medium used for activating and culturing the strains in step (1) is adjusted, and the LB culture medium is replaced with the MBS culture medium and the MBS culture medium engineering plate in Example 2, respectively, to obtain MBS-based microbial self-repairing cement-based material and MBS engineering plate-based microbial self-repairing cement-based material, respectively.

[0053] As a control, 1500 g of cement was mixed with 450 g of water to obtain a normal slurry cement group, which was cured according to steps (3) to (4) to obtain a blank control group cement-based material.

[0054] Figure 7 The compressive and flexural strength diagrams of microbial self-repairing cement-based materials under different culture media. Figure 7 It can be seen that the 7d flexural strength of the blank control group material is 7.1MPa, and the 7d compressive strength is 48.4MPa. The 7d flexural strength of the LB group material is 5.4MPa, and the 7d compressive strength is 41.9MPa. The 7d flexural strength of the MBS group material is 8.8MPa, and the 7d compressive strength is 56.6MPa. The 7d flexural strength of the MBS engineering version material is 9.2MPa, and the 7d compressive strength is 58.1MPa. It can be seen that the MBS medium engineering version has simple ingredients and low cost, but the material has better compressive and flexural strength. The spore liquid cultured in LB medium is directly added to cement, which will hinder the cement hydration reaction and have an adverse effect on the early compressive and flexural strength of cement-based materials; while MBS medium and MBS medium engineering version have no adverse effect on the early compressive and flexural strength of cement-based materials.

[0055] Example 4 The strength test of the self-repairing cement-based material with different strengthening components added with Bacillus-based microorganisms under LB medium includes the following steps:

[0056] (1) Take 1 mg of the microbial mineralization strain Bacillus sphaericus powder and add it to 100 mL of LB medium for activation. After activation, inoculate the bacterial solution into the LB medium at a 2% inoculum volume and culture the bacterial solution until the OD 600=1, then put the bacterial solution into a water bath at 80℃ for 30min to convert the bacterial solution into spore solution for later use;

[0057] (2) Pretreatment of cattail fiber: Take the strip leaves of cattail (picked in May in Wuhan Textile University), wash, cut, dry, break, pass through a 60-mesh sieve, and set aside;

[0058] (3) Preparation of cattail grass biochar: The cattail grass fiber obtained in step (2) is placed in a tubular furnace at 700° C. for pyrolysis for 30 min, and then cooled to room temperature to obtain cattail grass biochar (hereinafter referred to as “biochar”), which is set aside;

[0059] (4) Weigh 2 g of each of the cattail fiber and biochar obtained in step (2) and (3), immerse them in the spore solution (325 g) prepared in step (1), and then load them on a shaking table (30° C., 150 rpm) for 4 h and then dry them at 30° C. to constant weight, thereby obtaining cattail fiber-loaded Bacillus material (hereinafter referred to as “cattail-loaded Bacillus”) and cattail biochar-loaded Bacillus material (hereinafter referred to as “biochar-loaded Bacillus”);

[0060] (5) Pre-wetting the mixing pot and mixing blades of the cement mortar mixer, pouring cement, urea, anhydrous calcium chloride and strengthening components (any one of cattail fiber, biochar, cattail loaded Bacillus, biochar loaded Bacillus) into the mixing pot and starting to slowly stir until evenly mixed, then slowly pouring water and / or the spore solution prepared in step (1) into the mixing pot, with a water-cement ratio of 0.3, slowly stirring for 30 seconds, and then starting to quickly stir for 120 seconds to obtain evenly mixed cement mortar; wherein, the experiment set up a blank group, a direct bacteria-doped group, a cattail direct-doped group, a biochar direct-doped group, a cattail loaded group, and a biochar loaded group, and the amount of each group is shown in Table 3. The specific mixing materials of each group are as follows: the blank group is the ordinary pure cement group, in which cement and water are directly mixed; the direct bacteria-adding group is to evenly mix cement, urea and anhydrous calcium chloride, and then directly replace part of the mixing water with the spore liquid and add it into the cement mixture together with water; the cattail grass direct-adding group and the biochar direct-adding group are to evenly mix cement, urea, anhydrous calcium chloride, cattail grass fiber or biochar, and then directly replace part of the mixing water with the spore liquid and add it into the cement mixture together with water; the cattail grass loading group and the biochar loading group are to evenly mix cement, urea, anhydrous calcium chloride, cattail grass loaded Bacillus or biochar loaded Bacillus, and then add water into the cement mixture;

[0061] (6) Apply a thin layer of silicone oil on the inner surface of a 160 mm × 40 mm × 40 mm mold (to facilitate demoulding later), then pour the uniformly mixed cement mortar obtained in step (5) into the mold, shake out bubbles (to prevent the flexural strength of the cement test block from being reduced due to bubbles), and use a metal scraping ruler to scrape it flat;

[0062] (7) After the specimens are formed, they are cured in a standard constant temperature and humidity curing box for cement concrete at a temperature of 30°C ± 2°C and a relative humidity of 98% for 24 hours. The specimens are numbered and demolded. After demolding, they are placed in the aforementioned standard curing box for curing for 7 days to obtain the self-repairing cement-based material.

[0063] Table 3

[0064]

[0065] Figure 8 The figure shows the compressive and flexural strength of cement materials with different strengthening components added to Bacillus-based cement under LB culture medium. Figure 8 It can be seen that: 1) the 7d flexural strength of the blank group is 7.05MPa, and the 7d compressive strength is 48MPa; the 7d flexural strength of the direct bacteria-doped group is 22.5% lower than that of the blank group, and the 7d compressive strength is 12.7% lower; the 7d flexural strength of the cattail grass loading group is 15.9% higher than that of the blank group, and the 7d compressive strength is 57.1% higher; the 7d flexural strength of the biochar loading group is 0.7% higher than that of the blank group, and the 7d compressive strength is 11.7% higher. This shows that the incorporation method of spherical Bacillus has a certain effect on the performance of cement. A large amount of spore liquid cultured in LB medium is directly added to cement, which will hinder the cement hydration reaction and have an adverse effect on the early (7d) compressive and flexural strength of cement-based materials. This is consistent with the results of Example 3, but spherical Bacillus is first attached to the carrier and then added to the cement to alleviate this adverse effect, and even enhance the compressive and flexural strength of cement-based materials.

[0066] 2) The 7-day flexural strength of the cattail grass direct-mixed group was 12.2% higher than that of the biochar direct-mixed group, and the 7-day compressive strength was 9.6% higher. This shows that cattail grass fiber is better than carbonized biochar in improving the compressive and flexural strength of cement-based materials.

[0067] 3) The 7-day flexural strength of the cattail grass direct-mixing group was 4.5% lower than that of the blank group, and the 7-day compressive strength was 2.5% lower; the 7-day flexural strength of the biochar direct-mixing group was 14.9% lower than that of the blank group, and the 7-day compressive strength was 11% lower; however, the 7-day flexural strength of the cattail grass direct-mixing group was 17.3% lower than that of the cattail grass loading group, and the 7-day compressive strength was 37.9% lower; the 7-day flexural strength of the biochar direct-mixing group was 15.5% lower than that of the biochar loading group, and the 7-day compressive strength was 20.3% lower. This shows that the way of adding bacteria has a certain impact on the performance of cement. If Bacillus sphaericus and the carrier are not loaded and added directly to cement, it will hinder the cement hydration reaction and have an adverse effect on the early compressive and flexural strength of cement-based materials. However, if Bacillus sphaericus is first attached to the carrier and then added to cement, this adverse effect will be appropriately reduced. Biochar has little effect on cement hydration reaction when used as a carrier. Cattail fiber is used as a carrier. Bacillus sphericalus is first attached to the carrier and then added to cement, which will improve the early compressive and flexural strength of cement-based materials. The 7d flexural strength of the cattail loading group is 15.1% higher than that of the biochar loading group, and the 7d compressive strength is 38.8% higher.

[0068] The compressive and flexural tests of Examples 3-4 refer to GB / T17671-2021 "Test method for strength of cement mortar (ISO method)". After curing for 7 days, the flexural strength and compressive strength are measured using a microcomputer servo flexural and compressive testing machine.

[0069] Example 5 The self-repair test of cement-based materials under different culture media comprises the following steps:

[0070] (1) Take 1 mg of microbial mineralization strain Bacillus sphaericus powder and add it to 100 mL LB medium for activation. After activation, inoculate the bacterial solution into the LB medium at a 2% inoculum volume and culture the bacterial solution until the concentration of OD 600 =1, and then put the bacterial liquid into a water bath at 80°C for 30 minutes to convert the bacterial liquid into spore liquid for standby use; (2) pre-wetting the mixing pot and mixing blades of the cement mortar mixer, pouring 1500g of cement, 12g of urea, and 22g of anhydrous calcium chloride into the mixing pot and slowly stirring until uniformly mixed, then slowly pouring 125g of water and 325g of the spore liquid prepared in step (1), with a water-cement ratio of 0.3, slowly stirring for 30s, and then starting to quickly stir for 120s to obtain a uniformly mixed cement mortar;

[0071] (3) Take a 40 mm × 40 mm × 40 mm mold, apply a thin layer of silicone oil on the inner surface of the mold (to facilitate demoulding later), then pour the uniformly mixed cement mortar obtained in step (3) into the mold, shake out bubbles (to prevent the cement test block from reducing its flexural strength due to bubbles), and use a metal scraping ruler to scrape it flat. After the test piece is formed, it is cured in a standard constant temperature and humidity curing box for cement concrete at a temperature of 30°C ± 2°C and a relative humidity of 98% for 24 hours, then taken out, numbered, and demolded. (4) After demoulding, use a compression and flexural machine to prefabricate cracks, place the cement crack test block in the aforementioned standard curing box at 30°C ± 2°C and a relative humidity of 98% for further curing for 7 days, take it out and record it as "LB culture medium cement repair 7-day material", and record the self-repair effect of the crack and whether a relatively obvious calcium carbonate precipitation is produced by continuous photography. After prefabrication of the crack, take a photo of the cement-based material before further curing as a control group without culture medium repair.

[0072] As a control, 1500g of cement was mixed with 450g of water to obtain a common pure cement group, and prefabricated cracks and cured according to steps (3) to (4) to obtain a "blank control group cement repair 7-day material". In addition, steps (1) to (4) were repeated, and only the culture medium used for activating and culturing the strain in step (1) was adjusted, and the LB culture medium was replaced with the MBS culture medium and the MBS engineering version of the culture medium in Example 2, respectively, to obtain "MBS culture medium cement repair 7-day material" and "MBS engineering version culture medium cement repair 7-day material", respectively.

[0073] In addition, the engineered version of MBS medium combined with the enhanced component (Bacillus loaded with Typha) was used for self-repair experiments, and the steps were as follows:

[0074] S1 Take 1 mg of microbial mineralization strain Bacillus sphaeroides powder and add it to 100 mL of MBS medium engineering plate for activation. After activation, inoculate the bacterial solution into the MBS medium engineering plate at a 2% inoculation rate and cultivate the bacterial solution to an OD 600 =1, then put the bacterial solution into a water bath at 80℃ for 30min to convert the bacterial solution into spore solution for later use;

[0075] S2 Pretreatment of cattail fiber: Wash, cut, dry, and crush the cattail fiber, and pass it through a 60-mesh sieve for later use;

[0076] S3: Weigh 2 g of cattail fiber obtained in step S2, immerse it in the spore solution (325 g) prepared in step S1, and then load it on a shaking table (30°C, 150 rpm) for 4 hours and then dry it at 30°C to constant weight to obtain a cattail fiber loaded with Bacillus material (hereinafter referred to as "cattail loaded with Bacillus"); S4: Pre-wet the mixing pot and mixing blades of the cement mortar mixer, pour 1500 g of cement, 12 g of urea, 22 g of anhydrous calcium chloride, and the cattail loaded with Bacillus (about 2 g) obtained in S3 into the mixing pot and start to slowly stir until evenly mixed, then slowly pour in 450 g of water with a water-cement ratio of 0.3, slowly stir for 30 seconds, and then start to stir rapidly for 120 seconds to obtain a uniformly mixed cement mortar; S5: Take a 40 mm × 40 mm × 40 mm mold, apply a thin layer of silicone oil on the inner surface of the mold (for later Demoulding), then pouring the uniformly mixed cement mortar obtained in step S4 into the mold, shaking out bubbles (to avoid the cement test block from reducing its flexural strength due to bubbles), and leveling it with a metal scraping ruler. After the test piece is formed, it is cured in a standard constant temperature and humidity curing box for cement concrete at a temperature of 30°C±2°C and a relative humidity of 98% for 24 hours, then taken out, and the test piece is numbered and demolded; S6 After demolding, cracks are prefabricated using a compression and flexural machine, and the cement crack test block is placed in the aforementioned standard curing box at 30°C±2°C and a relative humidity of 98% for continued curing for 7 days, and is taken out and recorded as "Cattail grass loaded Bacillus-based cement repair material for 7 days", and the self-repair effect of the cracks and whether a relatively obvious calcium carbonate precipitation is produced are recorded by continuous photography. After prefabricating the cracks, the cement-based material is photographed before further curing as a control group without culture medium repair.

[0077] Fig. 9 The self-repairing effect diagram of cement-based materials under different culture media. Fig. 9It can be seen that after 7 days, the cracks of the cement block without the addition of Bacillus sphaericus spore liquid have basically no change, indicating that the cement block can hardly be self-repaired through maintenance. After 7 days of repair, the cracks of the cement block with the addition of Bacillus sphaericus spore liquid cultured in MBS medium have not been completely repaired, but the broken test block can be kept from falling, and the crack surface is relatively smooth. After 7 days of repair, the cracks of the cement block with the addition of Bacillus sphaericus spore liquid cultured in LB medium have not been completely repaired, but the broken test block can be kept from falling, and the crack surface is rough and uneven. After 7 days of repair, the cracks of the cement block with the addition of Bacillus sphaericus spore liquid cultured in MBS medium engineering version are accompanied by a small amount of calcium carbonate around the cracks, which is not easy to fall off, the crack surface is smooth and flat, and the self-repair effect is good. After the cattail grass fiber was loaded with the spore solution of Bacillus sphaericus cultured in the engineering version of MBS medium and then added to cement, calcium carbonate precipitation could be clearly seen on the surface of the crack after 7 days of prefabricated crack repair. The repair effect was obvious, and the crack surface was relatively smooth, which was better than the repair effect of the cement block only mixed with the spore solution of Bacillus sphaericus cultured in the engineering version of MBS medium. This shows that the synergistic effect of fiber and Bacillus sphaericus on repairing cement cracks is better than that of Bacillus sphaericus alone, because they combine the dual effects of mechanical strengthening and biological curing. The fiber can provide good mechanical support, prevent crack expansion, and maintain the stability of the crack. The biological action of Bacillus sphaericus can promote the self-healing repair process of cement and enhance the durability of the repaired part.

Claims

1. Application of Bacillus sphaericus combined with cattail fiber in microbial self-repair of microcracks in cement concrete, It is characterized in that The steps include: Take the powder of microbial mineralization strain Bacillus sphaeroides and add it to the MBS medium engineering version for activation culture until the bacterial liquid OD 600 =1±0.1, then put the bacterial liquid into a water bath at 80~100℃ for 30~60min to convert the bacterial liquid into spore liquid; wash, shear, dry, and crush the leaves of cattail grass, and pass them through a 60-mesh sieve to obtain cattail grass fiber; take the cattail grass fiber and immerse it in the spore liquid of the spherical Bacillus obtained above, then load it on a shaking table at 25~30℃ and 120~150 rpm for 4~6h, and then dry it at 30~40℃ to constant weight to obtain the cattail grass fiber-loaded Bacillus material; mix the obtained cattail grass fiber-loaded Bacillus material with cement, urea, and anhydrous calcium chloride, and then mix them with water in proportion to prepare cement concrete; the water-cement ratio in the system is 0.3; the amount of cattail grass fiber added is 0.1%~0.15% of the cement mass; the amount of urea added is 0.8%~1% of the cement mass; the amount of anhydrous calcium chloride added is 1%~2% of the cement mass; The components of the engineering version of the MBS medium are: 4.8g KH 2 PO 4 , 0.2 g CaCl 2 、0.2gMgSO 4 , 6g peptone and 2g yeast extract, solution pH = 7.

2.

2. The use according to claim 1, It is characterized in that The water-cement ratio in the system is 0.3; the amount of cattail grass fiber added is 0.1%~0.15% of the cement mass; the amount of urea added is 0.8%~1% of the cement mass; and the amount of anhydrous calcium chloride added is 1%~1.5% of the cement mass.

3. A self-healing cement-based material based on mineralization of Bacillus sphaericus, It is characterized in that The method comprises the following steps: mixing cement, urea, anhydrous calcium chloride, the cattail fiber loaded bacillus material in any one of claims 1 to 2 and water to prepare uniformly mixed cement mortar.