NGE new environmentally friendly solid fuel

Through the synergistic effect of using modified expanded vermiculite and bentonite in solid fuel, the problem of poor sulfur solidification effect of solid fuel is solved, and efficient sulfur solidification effect and environmentally friendly properties are achieved, meeting the needs of green energy.

CN118460261BActive Publication Date: 2024-11-22SHENMU XIANGYU ENERGY CHEM CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410830070.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-06-25
Publication Date
2024-11-22
Estimated Expiration
2044-06-25

AI Technical Summary

Technical Problem

The poor solid sulfur solidification effect of existing solid fuels leads to the emission of harmful sulfur-containing gases during energy conversion, limiting their environmental protection properties.

Method used

NGE new environmentally friendly solid fuel composed of thermal coal, charcoal, modified expanding vermiculite, bentonite and binders, combines modified expanding vermiculite and bentonite with different interlayer cations to improve solids The sulfur-solidation effect of fuel.

Benefits of technology

It significantly improves the sulfur solidification effect of solid fuel, meets the needs of green energy, and ensures the non-toxic, harmless and environmentally friendly components.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The present invention relates to the technical field of solid fuels, and proposes a new type of environmentally friendly solid fuel NGE, which includes the following components by weight: 100 parts of thermal coal, 40-50 parts of charcoal, 1-3 parts of oxidant, 5-10 parts of sulfur-fixing agent, and 1-4 parts of binder; the sulfur-fixing agent includes expanded vermiculite and bentonite. Through the above technical solution, the problem of poor sulfur-fixing effect of solid fuel in related technologies is solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of solid fuels, and in particular to a new type of environmentally friendly solid fuel, NGE. Background Art

[0002] In today's era, the widespread use of traditional fossil solid fuels, especially coal, has become one of the major factors that aggravate air pollution and damage the ecosystem. Faced with the continued rise in global energy demand and the general awakening of environmental protection awareness, the exploration and development of new green energy solid fuels (NGE solid fuels for short) has become a common focus.

[0003] A major limitation of existing solid fuel technology is that its sulfur fixation effect is poor, which leads to the emission of a large amount of harmful sulfur-containing gases during the energy conversion process, seriously restricting its environmental properties. In view of this, it is urgent to develop a new environmentally friendly solid fuel NEG with excellent sulfur fixation performance. Summary of the invention

[0004] The present invention proposes a new type of environmentally friendly solid fuel NGE, which solves the problem of poor sulfur fixation effect of solid fuel in related technologies.

[0005] The technical solution of the present invention is as follows:

[0006] The present invention proposes a new type of NGE environmentally friendly solid fuel, comprising the following components in parts by weight: 100 parts of thermal coal, 40-50 parts of charcoal, 1-3 parts of oxidant, 5-10 parts of sulfur-fixing agent, and 1-4 parts of binder;

[0007] The sulfur-fixing agent includes expanded vermiculite and bentonite.

[0008] As a further technical solution, the weight ratio of the expanded vermiculite to the bentonite is 1:4 to 4:1.

[0009] In the present invention, when the weight ratio of expanded vermiculite to bentonite is 1:4 to 4:1, it helps to further improve the sulfur fixation effect of solid fuel.

[0010] As a further technical solution, the expanded vermiculite is modified expanded vermiculite;

[0011] The raw materials of the modified expanded vermiculite include expanded vermiculite and polyaluminium ferric chloride.

[0012] In the present invention, polyaluminium ferric chloride is used to modify expanded vermiculite, thereby improving the activation ability of the expanded vermiculite and further improving the sulfur fixation effect of the solid fuel.

[0013] As a further technical solution, the preparation method of the modified expanded vermiculite comprises the following steps: dissolving polyaluminium ferric chloride in purified water, adding expanded vermiculite, mixing evenly, eluting, drying, and calcining to obtain the modified expanded vermiculite.

[0014] As a further technical solution, the weight ratio of the polyaluminium ferric chloride to expanded vermiculite is 1:7-15.

[0015] In the present invention, when the weight ratio of polyaluminium ferric chloride to expanded vermiculite is 1:7-15, it helps to further improve the sulfur fixation effect of solid fuel.

[0016] As a further technical solution, during the calcination, the temperature is 600-650° C. and the time is 3-5 hours.

[0017] As a further technical solution, the bentonite includes calcium-based bentonite and sodium-based bentonite.

[0018] In the present invention, when the bentonite includes calcium-based bentonite and sodium-based bentonite, the combined use of two bentonites having different interlayer cations helps to further improve the sulfur fixation effect of the solid fuel.

[0019] As a further technical solution, the weight of the sodium-based bentonite is greater than the weight of the calcium-based bentonite.

[0020] In the present invention, when the weight of the sodium-based bentonite is greater than the weight of the calcium-based bentonite, it helps to further improve the sulfur fixation effect of the solid fuel.

[0021] As a further technical solution, the oxidant includes one or more of potassium permanganate, potassium perchlorate, and sodium hypochlorite.

[0022] As a further technical solution, the binder includes one or both of agarose and curdlan.

[0023] The present invention also provides a method for preparing the NGE novel environmentally friendly solid fuel, which comprises the following steps: uniformly mixing the components, grinding, and granulating to obtain the solid fuel.

[0024] As a further technical solution, the particle size of the solid fuel is 40~75μm.

[0025] The working principle and beneficial effects of the present invention are:

[0026] In the present invention, each component of the solid fuel is non-toxic, harmless, green and environmentally friendly. Among them, the sulfur fixer in the component includes expanded vermiculite and bentonite. Through the synergistic effect of two different minerals with layered structures, the sulfur fixation effect of the solid fuel is improved, so that the solid fuel can fully meet the market demand for green energy. DETAILED DESCRIPTION

[0027] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0028] In the following examples and comparative examples, unless otherwise specified, the total moisture content of thermal coal is 8 wt %, the total moisture content of charcoal is 3 wt %, and the expanded density of expanded vermiculite is 11 g / cm 3 The model of polyaluminium ferric chloride is HL-707, the model of polyaluminium chloride is PAC-01, the model of polyferric chloride is HM-607, the model of calcium-based bentonite is HY-07, the model of sodium-based bentonite is HY-06, and the CAS number of agarose is CAS9012-36-6.

[0029] Example 1

[0030] The preparation method of NGE new environmentally friendly solid fuel comprises the following steps: by weight, 100 parts of thermal coal, 40 parts of charcoal, 1 part of potassium permanganate, 0.5 parts of expanded vermiculite, 4.5 parts of calcium-based bentonite and 1 part of agarose are uniformly mixed, ground and granulated to obtain a solid fuel with a particle size of 50 μm.

[0031] Example 2

[0032] The preparation method of NGE new environmentally friendly solid fuel comprises the following steps: by weight, 100 parts of thermal coal, 50 parts of charcoal, 3 parts of potassium permanganate, 1 part of expanded vermiculite, 9 parts of calcium-based bentonite and 4 parts of agarose are uniformly mixed, ground and granulated to obtain a solid fuel with a particle size of 50 μm.

[0033] Example 3

[0034] The preparation method of NGE new environmentally friendly solid fuel comprises the following steps: by weight, 100 parts of thermal coal, 50 parts of charcoal, 3 parts of potassium permanganate, 9 parts of expanded vermiculite, 1 part of calcium-based bentonite and 4 parts of agarose are uniformly mixed, ground and granulated to obtain a solid fuel with a particle size of 50 μm.

[0035] Example 4

[0036] The preparation method of NGE new environmentally friendly solid fuel comprises the following steps: by weight, 100 parts of thermal coal, 50 parts of charcoal, 3 parts of potassium permanganate, 2 parts of expanded vermiculite, 8 parts of calcium-based bentonite and 4 parts of agarose are mixed evenly, ground and granulated to obtain a solid fuel with a particle size of 50 μm.

[0037] Example 5

[0038] The preparation method of NGE new environmentally friendly solid fuel comprises the following steps: by weight, 100 parts of thermal coal, 50 parts of charcoal, 3 parts of potassium permanganate, 8 parts of expanded vermiculite, 2 parts of calcium-based bentonite and 4 parts of agarose are mixed evenly, ground and granulated to obtain a solid fuel with a particle size of 50 μm.

[0039] Example 6

[0040] The preparation method of the NGE new environmentally friendly solid fuel comprises the following steps: by weight, 100 parts of thermal coal, 50 parts of charcoal, 3 parts of potassium permanganate, 8 parts of modified expanded vermiculite, 2 parts of calcium-based bentonite and 4 parts of agarose are mixed evenly, ground and granulated to obtain a solid fuel with a particle size of 50 μm;

[0041] The preparation method of modified expanded vermiculite comprises the following steps: dissolving 0.25 parts of polyaluminium chloride in purified water, adding 7.75 parts of expanded vermiculite, mixing evenly, eluting and drying, and calcining at 630°C for 4 hours to obtain modified expanded vermiculite.

[0042] Example 7

[0043] The only difference between this embodiment and embodiment 6 is that in this embodiment, the preparation method of modified expanded vermiculite includes the following steps: dissolving 0.25 parts of polyferric chloride in purified water, adding 7.75 parts of expanded vermiculite, mixing evenly, eluting and drying, and calcining at 630° C. for 4 hours to obtain modified expanded vermiculite.

[0044] Example 8

[0045] The only difference between this embodiment and embodiment 6 is that in this embodiment, the preparation method of modified expanded vermiculite includes the following steps: dissolving 0.25 parts of polyaluminum ferric chloride in purified water, adding 7.75 parts of expanded vermiculite, mixing evenly, eluting and drying, and calcining at 630° C. for 4 hours to obtain modified expanded vermiculite.

[0046] Example 9

[0047] The only difference between this embodiment and embodiment 8 is that, in this embodiment, the weight portion of polyaluminium ferric chloride is 1.5 parts, and the weight portion of expanded vermiculite is 6.5 parts.

[0048] Example 10

[0049] The only difference between this embodiment and embodiment 8 is that, in this embodiment, the weight portion of polyaluminium ferric chloride is 0.5 parts, and the weight portion of expanded vermiculite is 7.5 parts.

[0050] Embodiment 11

[0051] The only difference between this embodiment and embodiment 8 is that, in this embodiment, the weight portion of polyaluminium ferric chloride is 1 part, and the weight portion of expanded vermiculite is 7 parts.

[0052] Example 12

[0053] The only difference between this embodiment and embodiment 11 is that in this embodiment, the calcium-based bentonite is replaced by an equal amount of sodium-based bentonite.

[0054] Embodiment 13

[0055] The only difference between this embodiment and embodiment 11 is that in this embodiment, 2 parts of calcium-based bentonite are replaced by 0.5 parts of sodium-based bentonite and 1.5 parts of calcium-based bentonite.

[0056] Embodiment 14

[0057] The only difference between this embodiment and embodiment 11 is that in this embodiment, 2 parts of calcium-based bentonite are replaced by 1 part of sodium-based bentonite and 1 part of calcium-based bentonite.

[0058] Embodiment 15

[0059] The only difference between this embodiment and embodiment 11 is that in this embodiment, 2 parts of calcium-based bentonite are replaced by 1.5 parts of sodium-based bentonite and 0.5 parts of calcium-based bentonite.

[0060] Comparative Example 1

[0061] The difference between this comparative example and Example 1 is that in this comparative example, no expanded vermiculite is added, and the weight portion of calcium-based bentonite added is 5 parts.

[0062] Comparative Example 2

[0063] The difference between this comparative example and Example 1 is that in this comparative example, no calcium-based bentonite is added, and the weight portion of expanded vermiculite added is 5 parts.

[0064] Comparative Example 3

[0065] The only difference between this comparative example and Example 1 is that in this comparative example, calcium-based bentonite and expanded vermiculite are not added.

[0066] Referring to GB / T 31098-2014 "Evaluation Method for Sulfur Fixation Effect of Coal Combustion", the effective sulfur fixation rates of the solid fuel sulfur fixers prepared in Examples 1 to 15 and Comparative Examples 1 to 3 were tested at 800°C and 900°C, respectively. The test results are shown in Table 1 below.

[0067] Table 1 Test results

[0068]

[0069] The comparison between Example 1 and Comparative Examples 1 to 3 shows that the synergistic effect of expanded vermiculite and bentonite, two minerals with a layered structure, can significantly improve the sulfur fixation effect of solid fuels. The comparison between Examples 2 to 3 and Examples 4 to 5 shows that when the weight ratio of expanded vermiculite to bentonite is 1:4 to 4:1, it helps to further improve the sulfur fixation effect of solid fuels. The comparison between Examples 5 and 6 to 11 shows that by modifying the expanded vermiculite, it helps to further improve the sulfur fixation effect of solid fuels. The comparison between Examples 6 to 7 and 8 shows that the use of polyaluminum ferric chloride to modify expanded vermiculite helps to further improve the sulfur fixation effect of solid fuels. The comparison between Examples 8 to 9 and Examples 10 to 11 shows that when the weight ratio of polyaluminum ferric chloride to expanded vermiculite is 1:7 to 15, it helps to further improve the sulfur fixation effect of solid fuels. The comparison between Examples 11 to 12 and 13 shows that when the bentonite includes calcium-based bentonite and sodium-based bentonite, it helps to further improve the sulfur fixation effect of solid fuels. Comparison between Examples 13-14 and Example 15 shows that when the weight of the sodium-based bentonite is greater than the weight of the calcium-based bentonite, it helps to further improve the sulfur fixation effect of the solid fuel.

[0070] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A solid fuel, It is characterized in that The invention comprises the following components in parts by weight: 100 parts of thermal coal, 40-50 parts of charcoal, 1-3 parts of oxidant, 5-10 parts of desulfurizing agent and 1-4 parts of binder; The sulfur-fixing agent includes expanded vermiculite and bentonite; The expanded vermiculite is modified expanded vermiculite; The raw materials of the modified expanded vermiculite include expanded vermiculite and polyaluminium ferric chloride.

2. The solid fuel according to claim 1, It is characterized in that The weight ratio of the expanded vermiculite to the bentonite is 1:4 to 4:

1.

3. The solid fuel according to claim 1, It is characterized in that The preparation method of the modified expanded vermiculite comprises the following steps: dissolving polyaluminium ferric chloride in purified water, adding expanded vermiculite, mixing evenly, eluting, drying, and calcining to obtain the modified expanded vermiculite.

4. The solid fuel according to claim 1, It is characterized in that The weight ratio of the polyaluminium ferric chloride to expanded vermiculite is 1:7-15.

5. The solid fuel according to claim 3, It is characterized in that During the calcination, the temperature is 600-650° C. and the time is 3-5 hours.

6. The solid fuel according to claim 1, It is characterized in that The oxidant includes one or more of potassium permanganate, potassium perchlorate and sodium hypochlorite.

7. The solid fuel according to claim 1, It is characterized in that The binder includes one or both of agarose and curdlan.

8. A method for preparing a solid fuel according to any one of claims 1 to 7, It is characterized in that The following steps are involved: The components are mixed evenly, ground and granulated to obtain solid fuel.

9. A method for preparing a solid fuel according to claim 8, It is characterized in that The particle size of the solid fuel is 40-75 μm.