A natural porous peat moss-based photothermal water-collecting material and its application
By combining zwitterionic sulfobetaine hydrogel with hygroscopic salt LiCl and carbon black with natural porous peat moss, a natural porous peat moss-based photothermal water collection material was prepared, which solved the complex preparation and leakage problems of existing water collection materials. , achieves efficient water capture and light-to-heat conversion, and is suitable for recycling agricultural water resources.
Patent Information
- Application Number
- CN202410936511.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-12
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2044-07-12
AI Technical Summary
Existing water collection materials have complex preparation procedures and high costs in large-scale production, and hygroscopic salts can easily cause leakage and environmental pollution, making it difficult to effectively solve the problem of agricultural water shortage.
Zwitterionic sulfobetaine hydrogel is mixed with hygroscopic salt LiCl and carbon black to form an interpenetrating polymer network, which is combined with natural porous peat moss and freeze-dried to prepare a natural porous peat moss-based photothermal water collection material. .
It achieves efficient moisture capture and light-to-heat conversion, prevents salt leakage, has low material cost, is environmentally friendly, has excellent water absorption efficiency and reusability, and is suitable for efficient recycling of agricultural water resources.
Smart Images

Figure CN118480274B_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the application of biomass water-collecting materials in the agricultural field, and in particular, to a natural porous peat moss-based photothermal water-collecting material and its application. Background Art
[0002] Globally, agricultural water accounts for about 70% of the total freshwater withdrawal, of which more than 90% is used for irrigation. Arid and semi-arid regions have long faced the problem of agricultural water shortage. Farmland drought caused by water shortage is a key factor affecting the sustainable development of agricultural production and food output. In the agricultural production process, more than 70% of the water will be dissipated through evaporation. Therefore, it is of great significance to develop evaporation water collection technology based on solar-driven photothermal conversion, improve the efficient recycling efficiency of agricultural water resources, and overcome the adverse effects of drought on crops to solve the current problem of agricultural water shortage.
[0003] So far, with the continuous development of atmospheric water harvesting technology, the industry has designed and developed many materials with high-efficiency water harvesting performance based on adsorption method, including metal organic frameworks, covalent organic frameworks, hydrogels, hygroscopic salts and their composite materials. However, although materials such as metal organic frameworks and covalent organic frameworks have significant effects, they are usually complicated to prepare and relatively expensive, and are still challenging in practical applications that require large-scale production. Hygroscopic salts have excellent water absorption capacity in a wide relative humidity range, but they are prone to leakage, resulting in performance degradation, environmental pollution and other problems.
[0004] As we all know, peat moss, known as a "natural humidifier", contains a large number of hydrophilic chemical groups and has many uneven protrusions and microporous structures, which makes it easy for water droplets to be adsorbed in large quantities in its porous structure. The low cost, easy accessibility and environmental friendliness of peat moss make it a sustainable and cost-effective alternative. Summary of the invention
[0005] In view of the above-mentioned shortcomings of existing water-collecting materials, the present invention provides a natural porous peat moss-based photothermal water-collecting material, in which zwitterionic sulfobetaine hydrogel is mixed with hygroscopic salt LiCl and carbon black to form an interpenetrating polymer network, which is then added to cleaned dry peat moss, and the water-collecting material is obtained through freeze-drying.
[0006] Specifically, the preparation method of the natural porous peat moss-based photothermal water-collecting material comprises the following steps:
[0007] S1. The peat moss is washed with 75wt% alcohol and deionized water, then drained and dried to obtain pretreated peat moss (0.1-0.5g) which is placed in a mold; the raw material peat moss has a natural porous water transport structure.
[0008] S2. Dispersing a zwitterionic monomer, an initiator and a cross-linker in pure water to obtain a zwitterionic sulfonate betaine hydrogel, wherein the zwitterionic monomer, initiator and cross-linker are: [2-(methacryloyloxy)ethyl]dimethyl-(3-sulfonatepropyl)ammonium hydroxide, ammonium persulfate and N,N-methylenebisacrylamide, respectively; the zwitterionic sulfonate betaine hydrogel has cationic and anionic functional groups with opposite charges along its polymer chain, exhibiting a unique salt-responsive anti-polyelectrolyte effect, and poly (sulfonate betaine) has better swelling ability in salt solution, and its unique salt-responsive characteristics help to coordinate more salt species and achieve more stretched conformations to achieve water capture.
[0009] S3, adding hygroscopic salt LiCl and carbon black to the zwitterionic sulfonate hydrogel of step S2 to carry out chemical crosslinking reaction to obtain a polymer solution; the hygroscopic salt LiCl and the zwitterionic sulfonate hydrogel form an interpenetrating polymer network, and the carbon black with high specific surface area and excellent light absorption capacity is dispersed; wherein, the hygroscopic salt LiCl gives the water-collecting material a high water-collecting capacity, and also promotes the self-association and dissociation between the cationic and anionic groups of the zwitterionic sulfonate gel, and the carbon black has a very high specific surface area and porosity, so that the prepared natural porous peat moss-based photothermal water-collecting material has strong adsorption and dispersion properties.
[0010] S4, pouring the polymer solution obtained in step S3 into the pretreated peat moss in step S1 and allowing it to stand for polymerization to form a peat moss-based hydrogel (SZL); wherein the natural peat moss material pretreated in step S1 and wound in a circular array is used as a skeleton to provide a multi-level, multi-size pore structure for the polymer. The mass ratio of the polymer solution to the pretreated peat moss is 20:1 to 5:1.
[0011] S5. Freeze-dry the peat moss-based hydrogel to obtain a natural porous peat moss-based photothermal water-collecting material (SZLC).
[0012] In step S1, the peat moss is washed alternately with 75 wt % alcohol and deionized water for 2 to 5 times.
[0013] In step S1, drying is performed in an oven at 60° C. for 6 h.
[0014] In the zwitterionic sulfobetaine hydrogel of step S2, the concentration of zwitterionic monomer is 1-10 mmol / mL, the mass fraction of initiator is 0.01-0.1%, and the mass fraction of crosslinker is 0.005-0.01%. Dispersion is performed by ultrasonic treatment at 40 KHz for 10-30 min.
[0015] In the polymer solution of step S3, the concentrations of hygroscopic salt LiCl and carbon black are 0.05-0.3 g / mL and 0.005-0.2 g / mL, respectively.
[0016] In step S3, chemical cross-linking reaction is performed by ultrasonic treatment at room temperature at 40 KHz for 10 to 30 minutes.
[0017] The polymerization temperature in step S4 is 60-110° C. and the polymerization time is 6-12 hours.
[0018] In step S5, the natural porous peat moss-based hydrogel is first cooled to room temperature and then freeze-dried.
[0019] The freeze-drying time in step S5 is 24 hours to 72 hours.
[0020] The natural porous peat moss-based photothermal water-collecting material includes natural plant materials with obvious pores and supporting structures, and the thickness is set to 0.5 mm to 40 mm.
[0021] The present invention also provides an application of a natural porous peat moss-based photothermal water-collecting material in photothermal conversion and efficient recycling of water resources.
[0022] Compared with the prior art, the beneficial effects of the present invention include:
[0023] The photothermal water-collecting material prepared by the present invention has a rapid water vapor dissipation and evaporative liquid transport channel under the triple blessing of the hydrophilic properties of the peat moss skeleton, the rough structure and the interconnected water pores between cells. The hygroscopic salt LiCl gives the photothermal water-collecting material a high water-collecting capacity, and also promotes the self-association and dissociation between the cationic and anionic groups of the zwitterionic sulfonobetaine gel, so that the zwitterionic sulfonobetaine gel has better swelling capacity. Carbon black has a very high specific surface area and porosity, which makes the prepared natural porous peat moss-based photothermal water-collecting material have strong adsorption and dispersion properties, and the maximum water absorption can reach 2.25g / g.
[0024] The photothermal water-collecting material prepared by the present invention causes multi-level scattering of sunlight inside the pores of the material, so that the material has high light absorption in the wavelength range of 300nm to 2500nm. Under standard sunlight irradiation, the photothermal conversion efficiency of the natural porous peat moss-based photothermal water-collecting material is as high as 90.5%.
[0025] The photothermal water-collecting material prepared by the present invention effectively prevents the problem of salt leakage under the cross-linking of zwitterionic sulfobetaine gel and hygroscopic salt, can evaporate for a long time without cleaning and material replacement, and has good reusability.
[0026] The photothermal water collection material of the present invention has a wide range of raw materials, low cost, no byproducts harmful to the environment and human body, and has excellent water absorption efficiency, photothermal conversion performance and environmental applicability. It has a wide range of application prospects in the field of solar-driven water collection and can promote the development of efficient and long-lasting sustainable recycling technology for agricultural evaporation water. Its preparation method is simple, has low requirements on reaction conditions, short preparation cycle, high probability of successful preparation, and stable reproducibility. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 The process flow and application diagram of the natural porous peat moss-based photothermal water-collecting material of Example 1 of the present invention;
[0028] Figure 2 Schematic diagram of the reaction structure of lithium chloride in Example 1 of the present invention;
[0029] Figure 3 This is a scanning electron microscope image of the natural porous peat moss-based photothermal water-collecting material prepared in Example 1 of the present invention, wherein ab is the surface absorption structure of peat moss; cd is the side water-transporting structure of peat moss; ef is the morphological characteristics of the gel formed after the hygroscopic salt LiCl is filled into the pores of peat moss; gh is the morphological characteristics of the natural porous peat moss-based photothermal water-collecting material;
[0030] Figure 4 This is a mapping analysis diagram of the pores of the natural porous peat moss-based photothermal water-collecting material prepared in Example 1 of the present invention, wherein a is a distribution diagram of C, N, O, and Cl elements, and b is a distribution diagram of Cl elements;
[0031] Figure 5 The morphology and contact angle of the natural porous peat moss-based photothermal water-collecting material after absorbing water prepared in Example 1 of the present invention, wherein a is a scanning electron microscope image of the natural porous peat moss-based photothermal water-collecting material after absorbing water, b is the contact angle of the natural porous peat moss-based photothermal water-collecting material, c is the contact angle of peat moss, and d is the contact angle of zwitterionic gel;
[0032] Figure 6a This is a surface thermal imaging image of the natural porous peat moss-based photothermal water-collecting material at 0 min during the photothermal conversion test in Example 1 of the present invention;
[0033] Figure 6b This is a surface thermal imaging image of the natural porous peat moss-based photothermal water-collecting material in Example 1 of the present invention at 5 minutes during the photothermal conversion test;
[0034] Figure 6c This is a surface thermal imaging image of the natural porous peat moss-based photothermal water-collecting material in Example 1 of the present invention at 15 minutes during the photothermal conversion test;
[0035] Figure 6d This is a surface thermal imaging image of the natural porous peat moss-based photothermal water-collecting material in Example 1 of the present invention at 20 minutes during the photothermal conversion test;
[0036] Figure 7 This is a UV-visible absorption spectrum of the natural porous peat moss-based photothermal water-collecting material prepared in Example 1 of the present invention;
[0037] Figure 8 The water absorption performance of the natural porous peat moss-based photothermal water-collecting material prepared in Example 1 of the present invention at different humidity levels;
[0038] Fig. 9 This is a test chart of the cyclic performance of the natural porous peat moss-based photothermal water-collecting material prepared in Example 1 of the present invention under low humidity (40%). DETAILED DESCRIPTION
[0039] The present invention is further illustrated and described below in conjunction with embodiments, but the described embodiments are only a part of the embodiments of the present invention, rather than all the embodiments. Based on the present invention and embodiments, all other inventions and embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0040] Unless otherwise specified, the experimental methods used in the following examples are conventional methods.
[0041] Unless otherwise specified, the materials and reagents used in the following examples can be obtained from commercial sources.
[0042] Example 1: A natural porous peat moss-based photothermal water-collecting material
[0043] like Figure 1 As shown, the preparation method thereof comprises the following steps:
[0044] S1. Take fresh peat moss as raw material, wash it alternately with 75wt% alcohol and deionized water for 3 times, drain the water, dry it at 60℃ for 6h to obtain pretreated peat moss, and place it in a mold for physical interweaving.
[0045] S2. Every 8.36g of [2-(methacryloyloxy)ethyl]dimethyl-(3-sulfonatepropyl)ammonium hydroxide (DMAPS) was added to 50mL of pure water, and 14.2mg of ammonium persulfate (APS, 99%) and 5mg of N,N-methylenebisacrylamide (MBA) were added to the obtained solution, and ultrasonic dispersion treatment was carried out at 40KHz at room temperature for 20min to obtain zwitterionic sulfobetaine hydrogel.
[0046] S3. 12.5 g of lithium chloride (LiCl) and 0.5 g of carbon black were added to the zwitterionic sulfobetaine hydrogel in sequence and subjected to ultrasonic treatment at room temperature at 40 KHz for 20 min for chemical crosslinking reaction to form an interpenetrating polymer network to obtain a polymer solution. The reaction structure of lithium chloride (LiCl) and zwitterionic sulfobetaine hydrogel is as follows: Figure 2 shown.
[0047] S4. Pour the polymer solution formed in step S3 into a mold containing peat moss at a mass ratio of polymer solution to pretreated peat moss = 5:1, and allow to stand and polymerize at 100°C for 12 hours to obtain a natural porous peat moss-based hydrogel (SZL).
[0048] S5. Freeze-dry the natural porous peat moss-based hydrogel for 24 hours to obtain a natural porous peat moss-based photothermal water-collecting material (SZLC).
[0049] The natural porous peat moss-based photothermal water-harvesting material was characterized and its performance was tested. The characterization mainly included: scanning electron microscopy, mapping analysis, UV-visible absorption spectroscopy, contact angle, etc. The prepared natural porous peat moss-based photothermal water-harvesting material was placed in a constant temperature and humidity chamber and a solar radiation simulator environment alternately, and an electronic balance was used to record the mass change of the material, so as to test its adsorption / desorption and cycle performance.
[0050] The results are as follows Figure 3-9 The specific analysis is as follows:
[0051] Figure 3 This is a scanning electron microscope photo of the natural porous peat moss-based photothermal water-collecting material prepared in this example. Figure 3 It can be seen that the natural porous peat moss-based photothermal water-harvesting composite material retains the hydrophilic surface and porous characteristics of the raw materials, and the hygroscopic salt is firmly embedded in it.
[0052] Figure 4 This is the mapping analysis diagram of the natural porous peat moss-based photothermal water-collecting material prepared in this embodiment. Figure 4 As can be seen in a, C, O, and N are evenly distributed on the pore surface of the SZLC material. The Cl element distribution results ( Figure 3 (b) shows the distribution of LiCl in the pores of the composite, confirming that LiCl was successfully loaded into the SZLC pore framework.
[0053] Figure 5 The morphology and contact angle of the natural porous peat moss-based photothermal water-collecting material prepared in this example after absorbing water are important indicators for measuring the hydrophilic and hydrophobic properties of the material surface. Figure 5 It can be seen that compared with the single sphagnum moss ( Figure 5 c) and zwitterionic gel materials ( Figure 5(d) Hydrophilic properties of natural porous peat moss-based photothermal water harvesting composite materials ( Figure 5 a) and b) are significantly improved, it can quickly absorb the captured moisture and bind it firmly, while avoiding the leakage of hygroscopic salt and the loss of moisture.
[0054] Figure 7 The UV-visible absorption spectrum of the natural porous peat moss-based photothermal water-collecting material prepared in this embodiment is shown in FIG. Figure 7 It can be seen that the surface absorption rate of natural porous peat moss-based photothermal water-collecting material for light with a wavelength of 250 to 2500 nm is 90.5%.
[0055] Figure 8 The water absorption performance of the natural porous peat moss-based photothermal water-collecting material prepared in this embodiment at different humidity levels is shown in FIG. Figure 8 It can be seen that the material prepared in this example has excellent water absorption, and the maximum water absorption can reach 2.25 g / g.
[0056] A xenon lamp was used as a solar radiation simulator to provide light with an intensity of one sun, which was vertically irradiated on the surface of the material prepared in this embodiment. Figure 6a This is a surface thermal imaging image of the natural porous peat moss-based photothermal water-collecting material at 0 min during the photothermal conversion test in Example 1 of the present invention; Figure 6b This is a surface thermal imaging image of the natural porous peat moss-based photothermal water-collecting material in Example 1 of the present invention at 5 minutes during the photothermal conversion test; Figure 6c This is a surface thermal imaging image of the natural porous peat moss-based photothermal water-collecting material in Example 1 of the present invention at 15 minutes during the photothermal conversion test; Figure 6d This is a surface thermal imaging image of the natural porous peat moss-based photothermal water-collecting material in Example 1 of the present invention at 20 minutes during the photothermal conversion test. Figure 6a As shown in the figure, the temperature at the center of the material is 28.2°C at 0 min, and the highest temperature is 28.9°C. Figure 6b As shown in the figure, the temperature at the center of the material is 39.5°C at 5 minutes, and the highest temperature is 39.8°C. Figure 6c As shown in the figure, the temperature at the center of the material is 53.1°C at 15 minutes, and the highest temperature is 55.9°C. Figure 6d As shown in the figure, the temperature of the material center is 60.3℃ at 20min, and the highest temperature is 61.8℃. Figure 6a~Figure 6d It can be seen that within 20 minutes, the temperature at the center of the material quickly rises to about 60.3℃, and then the water is decomposed and absorbed; Fig. 9 As shown, the performance has not changed significantly after 15 cycles.
[0057] In summary, the effective design of the structure of the natural porous peat moss-based photothermal water-collecting material prepared by the present invention not only has the properties of high photothermal conversion efficiency and high water absorption capacity, but also ensures the reusability of the material.
Claims
1. A natural porous peat moss-based photothermal water-collecting material, characterized in that: The zwitterionic sulfobetaine hydrogel is mixed with hygroscopic salt LiCl and carbon black to form an interpenetrating polymer network, which is then added to cleaned dry peat moss, and the natural porous peat moss-based photothermal water-collecting material is obtained through freeze-drying. The preparation method of the natural porous peat moss-based photothermal water-collecting material comprises the following steps: S1, the peat moss is washed with 75wt% alcohol and deionized water, the water is drained, and the pretreated peat moss is dried and placed in a mold; S2, dispersing a zwitterionic monomer, an initiator and a cross-linking agent in pure water to obtain a zwitterionic sulfobetaine hydrogel, wherein the zwitterionic monomer, the initiator and the cross-linking agent are: [2-(methacryloyloxy)ethyl]dimethyl-(3-sulfonic acid propyl)ammonium hydroxide, ammonium persulfate and N,N-methylenebisacrylamide; S3, adding hygroscopic salt LiCl and carbon black to the zwitterionic sulfobetaine hydrogel of step S2 to carry out a chemical crosslinking reaction to obtain a polymer solution; S4, pouring the polymer solution obtained in step S3 into the pretreated peat moss in step S1 and allowing to stand and polymerize to form a peat moss-based hydrogel; S5, freeze-drying the peat moss-based hydrogel to obtain the natural porous peat moss-based photothermal water-collecting material; In the zwitterionic sulfobetaine hydrogel of step S2, the concentration of the zwitterionic monomer is 1-10 mmol / mL, the mass fraction of the initiator is 0.01-0.1%, and the mass fraction of the crosslinker is 0.005-0.01%; In the polymer solution of step S3, the concentrations of hygroscopic salt LiCl and carbon black are 0.05-0.3 g / mL and 0.005-0.2 g / mL, respectively; In the step S4, the mass ratio of the polymer solution to the pretreated peat moss is 20:1 to 5:
1.
2. The natural porous peat moss-based photothermal water-collecting material according to claim 1, characterized in that: Includes one or more of the following (1)-(8): (1) In step S1, the peat moss is washed alternately with 75 wt% alcohol and deionized water for 2 to 5 times; (2) In step S1, drying at 60° C. for 6 hours; (3) In step S2, the dispersion is carried out by ultrasonic treatment at 40 KHz for 20 min; (4) In step S3, chemical cross-linking reaction is performed by ultrasonic treatment at 40 KHz for 20 min at room temperature; (5) The polymerization temperature in step S4 is 60-110°C and the polymerization time is 6-12h; (6) In step S5, the natural porous peat moss-based hydrogel is first cooled to room temperature and then freeze-dried; (7) The freeze-drying time in step S5 is 24 hours to 72 hours; (8) The thickness of the natural porous peat moss-based photothermal water-collecting material is set to 0.5 mm to 40 mm.
3. Application of the natural porous peat moss-based photothermal water-collecting material according to claim 1 or 2 in the field of photothermal conversion or efficient recycling of water resources.
Citation Information
Patent Citations
Polypyrrole-coated cattail wool-based ultra-light biomass porous foam as well as preparation method and application thereof
CN113321939A
Salt-sensitive photo-thermal gel as well as preparation and application thereof
CN114605591A