A PVD film stripping process for titanium-aluminum bonded parts and its application

By using a combination process of pH-adjusted deplating solution and acid defiling solution on titanium-aluminum bonding, the problem of damage to aluminum oxide film in the prior art is solved, and the PVD film layer is efficiently removed and the aluminum oxide film is maintained. Integrity ensures the glossiness of titanium alloy and the protection of aluminum oxide film.

CN118621417BActive Publication Date: 2024-11-05VITAYON FINE CHEM SCI & TECH CO LTD SHENZHEN
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411095881.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-12
Publication Date
2024-11-05
Estimated Expiration
2044-08-12

AI Technical Summary

Technical Problem

The prior art is prone to damage the aluminum alloy oxide film when removing the PVD film layer, resulting in waste of materials and increased costs. It is difficult to achieve efficient deplating without damaging the aluminum oxide layer in mobile phone frames of titanium-aluminum bonds.

Method used

Using a combination process of deplating solution A and acid deplating solution B with pH adjustment to 7-8, the titanium oxide film is removed through the steps of anodizing and cathode energization, combined with citric acid to adjust the pH value and use a high-purity graphite plate to ensure that Deplating efficiency and finished product quality.

Benefits of technology

It has achieved complete removal of the PVD film layer without damaging the aluminum oxide film, maintained the glossiness of the titanium alloy and the integrity of the aluminum oxide film, improved the deplating efficiency and finished product quality, and is suitable for large-scale promotion.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The present invention discloses a PVD film stripping process for titanium-aluminum combination parts and its application. The PVD film stripping process for titanium-aluminum combination parts comprises the following steps: S1: hanging a workpiece and ensuring that different positions of the workpiece have good conductivity, S2: placing the workpiece in a stripping solution A to strip the PVD film, S3: rinsing the workpiece treated by S2, S4: placing the workpiece treated by S3 in a stripping solution B to remove the yellow film, S5: rinsing the workpiece treated by S4, S6: drying the workpiece treated by S5, the stripping solution A is TD311 whose pH value is adjusted to 7-8 by a pH regulator, and the stripping solution B is TM312. The PVD film stripping process for titanium-aluminum combination parts of the present invention can efficiently strip the PVD film on the surface of the titanium alloy without damaging the gloss of the titanium alloy surface and the anodized film on the surface of the aluminum alloy, so as to achieve the requirements of qualified stripping of defective PVD coating products and reuse.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of vacuum coating, and in particular to a PVD film stripping process for a titanium-aluminum combination part and an application thereof. Background Art

[0002] PVD is the abbreviation of Physical Vapor Deposition. The PVD process is a physical process to achieve material transfer, transferring atoms or molecules from the material source to the surface of the substrate. Specifically, it refers to a process that uses low-voltage, high-current arc discharge technology under vacuum conditions, uses gas discharge to evaporate the target material and ionize the evaporated material and gas, and uses the acceleration of the electric field to deposit the evaporated material and its reaction products on the workpiece. The film layer plated by PVD coating technology has the characteristics of high hardness, high wear resistance (low friction coefficient), corrosion resistance and chemical stability. The film layer has a long life and can also play a good decorative role on the appearance of the workpiece. In the mobile phone industry, PVD coating technology can be applied to the coating of mobile phone middle frames, shells, buttons, camera lenses, mobile phone films and other parts. At present, some high-end brand mobile phone frames have adopted PVD plating on titanium alloy materials. Its strength is much higher than that of aluminum alloy materials, and it has a lightweight effect compared to stainless steel materials.

[0003] However, in the actual production process, even with the most mature coating process, the film quality may be poor. If the workpiece is directly scrapped, a lot of material costs will be wasted. For example, the mobile phone middle frame consumes a lot of materials, processing and manpower from material processing to coating. If it is scrapped, the cost is too high, so it needs to be stripped and reworked for re-coating. Traditional stripping processes mostly use strong alkaline solutions such as organic alkalis and inorganic alkalis in combination with oxidants, chelating agents, etc., or use fluorine-containing stripping solutions to remove the PVD film layer, but this process will cause corrosion to the mobile phone middle frame workpiece containing an aluminum alloy oxide film middle plate. Therefore, there is an urgent need for a stripping process that can remove the PVD film layer on the titanium alloy surface of the frame without damaging the aluminum alloy oxide film on the middle plate. Summary of the invention

[0004] In view of the defects in the prior art, the present invention proposes a PVD film stripping process for titanium-aluminum combination parts and its application.

[0005] The present invention provides a titanium-aluminum bonded part PVD film layer stripping process, comprising the following steps:

[0006] S1: Hang the workpiece and ensure that different positions of the workpiece have good conductivity;

[0007] S2: placing the workpiece in a deplating solution A to remove the PVD film layer;

[0008] S3: rinsing the workpiece after being processed in S2;

[0009] S4: placing the workpiece processed in S3 into film stripping liquid B to remove the yellow film;

[0010] S5: rinsing the workpiece after being processed in S4;

[0011] S6: Drying the workpiece after being processed in S5;

[0012] The deplating solution A is TD311 whose pH value is adjusted to 7-8 by a pH regulator;

[0013] The film stripping solution B is TM312.

[0014] Adjusting the pH of TD311 can prevent the original solution from being too alkaline and thus corroding the aluminum oxide layer of the titanium-aluminum joint. Rinsing in step S3 can remove the stripping solution A remaining in the workpiece and the hanger to prevent it from being brought into the stripping solution B tank and causing contamination. Rinsing is done with pure water for 2-3 times. After the PVD film layer is stripped in step S2, the exposed titanium alloy will undergo an anodic oxidation reaction in the stripping solution A under the action of an applied voltage of 8-13 V to generate an amorphous amorphous titanium oxide film, which shows a layer of yellow film under the action of thin film interference, affecting the appearance of the workpiece. Therefore, step S4 is set to remove the yellow titanium oxide film generated in step S2. The acidic stripping solution in step S4, when powered by an external cathode, causes the oxide film on the surface of the titanium alloy to form an amorphous titanium oxide film under the action of H + Dissolution and removal occurs under erosion.

[0015] Furthermore, the pH regulator is citric acid; using citric acid to adjust the pH value of the TD311 stock solution can reduce the alkalinity of the stripping solution A on the one hand, and on the other hand, the citrate radical can also serve as a metal complexing agent to promote the removal of the PVD film layer.

[0016] Furthermore, in step S2, the anode is connected to the workpiece, and the cathode plate is any one of a stainless steel plate or a high-purity graphite plate.

[0017] Furthermore, in step S2, the operating voltage is 8-13 V, the operating temperature is 20-30° C., and the stripping time is 10-20 min. If the operating voltage is too low, the PVD film layer on the surface cannot be stripped or cannot be stripped cleanly; if the operating voltage is too high, although the stripping efficiency is accelerated, a titanium oxide film with a yellower or even purple color will be generated on the exposed titanium alloy surface, increasing the difficulty of stripping in the subsequent process.

[0018] Furthermore, in step S4, the operating voltage is 2-5 V, the operating temperature is 20-30° C., and the time is 5-10 min. If the operating voltage is too low, the film stripping speed is slow and difficult to strip. If the operating voltage is too high, the speed will be faster, but the film stripping is easy to generate dust, and ultrasonic dust removal is required, which increases the complexity of the process. If the operating temperature is too low, the film stripping speed will be reduced. If the operating temperature is too high, it will cause corrosion to the workpiece.

[0019] Furthermore, in step S4, the cathode is connected to the workpiece, and the anode plate is a high-purity graphite plate; since the tank liquid is acidic, the use of a high-purity graphite plate can prevent the anode plate from being corroded.

[0020] Furthermore, the composition of the TD311 includes 3-5% by mass of a main agent, 0.5-1% of a complexing agent and 0.1-0.2% of a dispersant; the main agent is potassium pyrophosphate, the complexing agent is one or both of triethanolamine or disodium ethylenediaminetetraacetate, and the dispersant is NNO.

[0021] Furthermore, the composition of the TM312 includes 6-8% by mass of an organic acid and 0.2-0.5% by mass of a corrosion inhibitor.

[0022] Furthermore, the organic acid is one or more of tartaric acid, citric acid, and malic acid, and the corrosion inhibitor is one or more of sodium molybdate and benzotriazole.

[0023] Furthermore, in step S1, the workpiece is hung up, and a special hanger can be used to hang the workpiece up, or the workpiece is placed on a fixture and then hung up, and its main purpose is to ensure that the product has good conductivity. The conductivity can be confirmed by connecting one end of the multimeter to the hanger and the other end to different parts of the titanium alloy frame of the workpiece to ensure that different positions of the workpiece are conductive.

[0024] Furthermore, the purpose of rinsing the product in step S5 is to remove the residual agent on the surface of the workpiece and clean the product.

[0025] Furthermore, the purpose of drying the product in step S6 is to prevent water residue from causing watermarks, which can be done by blowing, spinning or baking. After the product is dried, it can be packaged for hanging.

[0026] The present invention also provides the application of the stripping process in the stripping of titanium-aluminum combined parts, especially in the stripping of the PVD film layer of the mobile phone middle frame containing an aluminum alloy oxide film middle plate.

[0027] In summary, compared with the prior art, the present invention achieves the following technical effects:

[0028] (1) The PVD film stripping process for titanium-aluminum composite parts provided by the present invention can completely strip the film from the workpiece after stripping and can maintain the original gloss of the titanium alloy. The color of the workpiece after stripping is the original color of the titanium alloy.

[0029] (2) The PVD film stripping process for the titanium-aluminum bonded part provided by the present invention has high stripping efficiency;

[0030] (3) The PVD film stripping process for titanium-aluminum bonded parts provided by the present invention can be applied to titanium-aluminum bonded parts to prevent the aluminum oxide film from being corroded;

[0031] (4) The PVD film stripping process for titanium-aluminum composite parts provided by the present invention can meet the requirements of stripping defective products and reusing them, and the process is simple and can be promoted on a large scale. DETAILED DESCRIPTION

[0032] In order to enable those skilled in the art to better understand the solutions of the present invention, the technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention.

[0033] Example

[0034] The present invention is further described below in conjunction with specific examples and comparative examples. The following specific examples are all preferred embodiments of the present invention, but the embodiments of the present invention are not limited to the following examples, and are particularly not limited to the types of the various component raw materials used in the following specific examples.

[0035] 1. Sources of raw materials for the embodiments and comparative examples:

[0036] Unless otherwise specified, the raw materials used in the examples and comparative examples of the present invention are commercially available.

[0037] TD311: Product of Huizhou Huiyang Youtian Jingye Chemical Co., Ltd.;

[0038] TM312: Product of Huizhou Huiyang Youtian Jingye Chemical Co., Ltd.;

[0039] The workpieces used in the following embodiments and comparative examples are all mobile phone middle frames of titanium-aluminum combinations. The middle plate is made of 6013 aluminum and is anodized, the frame is made of TC4 titanium alloy, and the surface is a chromium-containing silicon carbon nitrogen PVD film layer with a chrome-plated base.

[0040] The PVD film stripping process of the titanium-aluminum bonded member in the embodiment of the present invention and comparative examples 1-5 specifically includes the following steps:

[0041] S1: Hang the workpiece and ensure that different positions of the workpiece have good conductivity;

[0042] S2: removing the PVD film layer from the workpiece, controlling the operating voltage and operating temperature, and the stripping time is 10-20 min;

[0043] S3: The workpiece treated in S2 is rinsed with pure water for 3 times. After rinsing, it is observed and confirmed that the PVD film layer of the titanium alloy frame has been completely removed. At this time, the titanium alloy frame is light yellow;

[0044] S4: placing the workpiece treated in S3 in TM312 to remove the yellow film, controlling the operating voltage and operating temperature, and the time is 5-10 min;

[0045] S5: Rinse the workpiece after S4 treatment with pure water for 3 times, and observe and confirm whether the titanium alloy frame is the original color of TC4 titanium alloy and whether the aluminum alloy oxide film is corroded after rinsing;

[0046] S6: Drying the workpiece after being processed in S5.

[0047] 2. Various performance test methods

[0048] 1. Glossiness test of titanium alloy after stripping: 3nh YG60 gloss meter is used for measurement (the glossiness requirement of the material before coating is 100-110GU, so the glossiness after stripping is also required to be between 100-110GU to be qualified).

[0049] 2. Comprehensive evaluation of finished products after deplating:

[0050] 2.1 PVD film stripping degree

[0051] Check the surroundings of the workpiece frame, the inner wall, the volume hole and other locations. If there are plaque-like or dot-like residues, it is considered that the stripping is not complete;

[0052] 2.2 Color of titanium alloy after film removal

[0053] If the surface of the titanium alloy after film removal is natural color, it is qualified; if the color is yellow or colorful, it is unqualified;

[0054] 2.3 Appearance judgment of corrosion condition of aluminum alloy oxide film in middle plate

[0055] If the aluminum alloy oxide film on the middle plate shows different colors, corrosion spots, or fogging, it is considered to be corroded;

[0056] 2.4 Artificial sweat test of aluminum alloy oxide film on middle plate

[0057] The test was carried out according to the industry standard QB_T 4775-2014 test method for artificial sweat corrosion resistance.

[0058] Example 1

[0059] S1: Hang the workpiece and ensure that different positions of the workpiece have good conductivity;

[0060] S2: The workpiece is placed in TD311 with a pH value of 7.0 adjusted by citric acid to remove the PVD film layer, the operating voltage is 8 V, the operating temperature is 20°C, and the electrolysis is performed for 10 minutes, wherein the anode is connected to the workpiece and the cathode plate is a stainless steel plate;

[0061] S3: Rinse the workpiece treated in S2 with pure water for 3 times;

[0062] S4: Place the workpiece treated in S3 in TM312 to remove the yellow film, with an operating voltage of 2 V, an operating temperature of 20°C, and a time of 5 min;

[0063] S5: Rinse the workpiece treated in S4 with pure water for 3 times;

[0064] S6: Drying the workpiece after being processed in S5.

[0065] Example 2

[0066] S1: Hang the workpiece and ensure that different positions of the workpiece have good conductivity;

[0067] S2: The workpiece is placed in TD311 with a pH value of 7.5 adjusted by citric acid to remove the PVD film layer, the operating voltage is 10.5V, the operating temperature is 25°C, and the electrolysis is performed for 15 minutes, wherein the anode is connected to the workpiece and the cathode plate is a high-purity graphite plate;

[0068] S3: Rinse the workpiece treated in S2 with pure water for 3 times;

[0069] S4: Place the workpiece treated in S3 in TM312 to remove the yellow film, with an operating voltage of 3.5 V, an operating temperature of 25°C, and a time of 7.5 min;

[0070] S5: Rinse the workpiece treated in S4 with pure water for 3 times;

[0071] S6: Drying the workpiece after being processed in S5.

[0072] Example 3

[0073] S1: Hang the workpiece and ensure that different positions of the workpiece have good conductivity;

[0074] S2: The workpiece is placed in TD311 with a pH value of 8.0 adjusted by citric acid to remove the PVD film layer, the operating voltage is 13V, the operating temperature is 30°C, the electrolysis is performed for 20 minutes, the anode is connected to the workpiece, and the cathode plate is a stainless steel plate;

[0075] S3: Rinse the workpiece treated in S2 with pure water for 3 times;

[0076] S4: Place the workpiece treated in S3 in TM312 to remove the yellow film, with an operating voltage of 5 V, an operating temperature of 30°C, and a time of 10 min;

[0077] S5: Rinse the workpiece treated in S4 with pure water for 3 times;

[0078] S6: Drying the workpiece after being processed in S5.

[0079] Example 4

[0080] S1: Hang the workpiece and ensure that different positions of the workpiece have good conductivity;

[0081] S2: The workpiece is placed in TD311 with a pH value adjusted to 7.0 by citric acid to remove the PVD film layer, the operating voltage is 8V, the operating temperature is 20°C, the electrolysis is performed for 10 minutes, the anode is connected to the workpiece, and the cathode plate is a stainless steel plate;

[0082] S3: Rinse the workpiece treated in S2 with pure water for 3 times;

[0083] S4: Place the workpiece treated in S3 in TM312 to remove the yellow film, with an operating voltage of 5 V, an operating temperature of 30°C, and a time of 10 min;

[0084] S5: Rinse the workpiece treated in S4 with pure water for 3 times;

[0085] S6: Drying the workpiece after being processed in S5.

[0086] Example 5

[0087] S1: Hang the workpiece and ensure that different positions of the workpiece have good conductivity;

[0088] S2: The workpiece is placed in TD311 with a pH value of 8.0 adjusted by citric acid to remove the PVD film layer, the operating voltage is 13V, the operating temperature is 30°C, the electrolysis is performed for 20 minutes, the anode is connected to the workpiece, and the cathode plate is a stainless steel plate;

[0089] S3: Rinse the workpiece treated in S2 with pure water for 3 times;

[0090] S4: Place the workpiece treated in S3 in TM312 to remove the yellow film, with an operating voltage of 2 V, an operating temperature of 20°C, and a time of 5 min;

[0091] S5: Rinse the workpiece treated in S4 with pure water for 3 times;

[0092] S6: Drying the workpiece after being processed in S5.

[0093] Comparative Example 1

[0094] S1: Hang the workpiece and ensure that different positions of the workpiece have good conductivity;

[0095] S2: Place the workpiece in TD311 stock solution to remove the PVD film layer. The stock solution pH is 13.3, the operating voltage is 10.5V, the operating temperature is 25°C, and the electrolysis is performed for 15 minutes. The anode is connected to the workpiece, and the cathode plate is a stainless steel plate.

[0096] S3: Rinse the workpiece treated in S2 with pure water for 3 times;

[0097] S4: Place the workpiece treated in S3 in TM312 to remove the yellow film, with an operating voltage of 3.5 V, an operating temperature of 25 ° C, and a time of 7.5 min;

[0098] S5: Rinse the workpiece treated in S4 with pure water for 3 times;

[0099] S6: Drying the workpiece after being processed in S5.

[0100] Comparative Example 2

[0101] S1: Hang the workpiece and ensure that different positions of the workpiece have good conductivity;

[0102] S2: The workpiece is placed in TD311 with a pH value adjusted to 7.5 by citric acid to remove the PVD film layer, the operating voltage is 16V, the operating temperature is 25°C, the electrolysis is performed for 15 minutes, the anode is connected to the workpiece, and the cathode plate is a stainless steel plate;

[0103] S3: Rinse the workpiece treated in S2 with pure water for 3 times;

[0104] S4: Place the workpiece treated in S3 in TM312 to remove the yellow film, with an operating voltage of 3.5 V, an operating temperature of 25 ° C, and a time of 7.5 min;

[0105] S5: Rinse the workpiece treated in S4 with pure water for 3 times;

[0106] S6: Drying the workpiece after being processed in S5.

[0107] Comparative Example 3

[0108] S1: Hang the workpiece and ensure that different positions of the workpiece have good conductivity;

[0109] S2: The workpiece is placed in TD311 with a pH value of 7.5 adjusted by citric acid to remove the PVD film layer, the operating voltage is 10.5V, the operating temperature is 35°C, the electrolysis is performed for 15 minutes, the anode is connected to the workpiece, and the cathode plate is a stainless steel plate;

[0110] S3: Rinse the workpiece treated in S2 with pure water for 3 times;

[0111] S4: Place the workpiece treated in S3 in TM312 to remove the yellow film, with an operating voltage of 3.5 V, an operating temperature of 25 ° C, and a time of 7.5 min;

[0112] S5: Rinse the workpiece treated in S4 with pure water for 3 times;

[0113] S6: Drying the workpiece after being processed in S5.

[0114] Comparative Example 4

[0115] S1: Hang the workpiece and ensure that different positions of the workpiece have good conductivity;

[0116] S2: The workpiece is placed in TD311 with a pH value of 7.5 adjusted by citric acid to remove the PVD film layer, the operating voltage is 10.5V, the operating temperature is 25°C, and the electrolysis is performed for 15 minutes, wherein the anode is connected to the workpiece and the cathode plate is a high-purity graphite plate;

[0117] S3: Rinse the workpiece treated in S2 with pure water for 3 times;

[0118] S4: Place the workpiece treated in S3 in TM312 to remove the yellow film, with an operating voltage of 8 V, an operating temperature of 25°C, and a time of 7.5 min;

[0119] S5: Rinse the workpiece treated in S4 with pure water for 3 times;

[0120] S6: Drying the workpiece after being processed in S5.

[0121] Comparative Example 5

[0122] S1: Hang the workpiece and ensure that different positions of the workpiece have good conductivity;

[0123] S2: The workpiece is placed in TD311 with a pH value of 7.5 adjusted by citric acid to remove the PVD film layer, the operating voltage is 10.5V, the operating temperature is 25°C, and the electrolysis is performed for 15 minutes, wherein the anode is connected to the workpiece and the cathode plate is a high-purity graphite plate;

[0124] S3: Rinse the workpiece treated in S2 with pure water for 3 times;

[0125] S4: Place the workpiece treated in S3 in TM312 to remove the yellow film, with an operating voltage of 3.5 V, an operating temperature of 35°C, and a time of 7.5 min;

[0126] S5: Rinse the workpiece treated in S4 with pure water for 3 times;

[0127] S6: Drying the workpiece after being processed in S5.

[0128] Comparative Example 6

[0129] Use the traditional stripping process 1: use 5% sodium hydroxide + 10% potassium permanganate, soak at 90-100℃ for 30 minutes.

[0130] Comparative Example 7

[0131] Use traditional stripping process 2: use 5% ammonium bifluoride + 5% nitric acid, soak at room temperature for 10 minutes.

[0132] Table 1. Technical effects of embodiments and comparative examples

[0133]

[0134] Examples 1-5 are all deplated according to the deplating process of the present invention, and the deplating solution A and the film stripping solution B with specific pH values ​​of the present invention are used. The workpiece using the deplating process of the present invention can meet the deplating requirements, and the deplating efficiency is high. The titanium-aluminum combination after deplating can keep the aluminum oxide film from being corroded, and the frame is the original color of the titanium alloy and maintains the original gloss, thereby achieving efficient deplating of the PVD film layer of the titanium-aluminum combination.

[0135] In comparative example 1, TD311 stock solution is directly used for stripping, which causes corrosion of the aluminum oxide film on the middle plate; comparative examples 2 and 3 show that if the voltage is too high or the temperature is too high during stripping (the conductivity of the solution increases when the temperature is high), a yellow oxide film layer is easily generated on the surface of the titanium alloy, and it is difficult to restore the original color of the titanium alloy after stripping; comparative example 4 shows that increasing the stripping voltage can speed up the stripping, but the violent reaction will cause the titanium alloy surface to become gray; comparative example 5 increases the temperature of the stripping solution, which can completely strip the titanium alloy surface, but the high temperature acidic solution will cause fogging corrosion to the aluminum alloy oxide film on the middle plate; comparative examples 6-7 use traditional stripping processes, all of which cause serious corrosion to the aluminum alloy oxide film on the middle plate.

[0136] The above comparative examples cannot achieve efficient stripping while keeping the aluminum oxide film of the middle plate of the stripped finished product from being corroded and maintaining the original glossiness of the titanium alloy, and meet the requirements of stripping defective PVD coating products and reusing them.

[0137] Based on the test data of finished product gloss and comprehensive evaluation of finished products in Table 1, the stripped finished products obtained by the stripping processes of Examples 1-5 have obvious advantages over the comparative examples and can effectively meet the high standards of customers and the market.

[0138] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A PVD film stripping process for titanium-aluminum bonded parts, characterized in that: The steps include: S1: Hang the workpiece and ensure that different positions of the workpiece have good conductivity; S2: placing the workpiece in a deplating solution A to remove the PVD film layer; S3: rinsing the workpiece after being processed in S2; S4: placing the workpiece processed in S3 into film stripping liquid B to remove the yellow film; S5: rinsing the workpiece after being processed in S4; S6: Drying the workpiece after being processed in S5; The deplating solution A is TD311 whose pH value is adjusted to 7-8 by a pH regulator; The stripping solution B is TM312; In step S2, the operating voltage is 8-13 V, the operating temperature is 20-30° C., and the stripping time is 10-20 min; In step S4, the operating voltage is 2-5 V, the operating temperature is 20-30° C., and the time is 5-10 min; The composition of TD311 includes 3-5% by mass of a main agent, 0.5-1% of a complexing agent and 0.1-0.2% of a dispersant; The main agent is potassium pyrophosphate, the complexing agent is one or both of triethanolamine and disodium ethylenediaminetetraacetate, and the dispersant is NNO; The composition of the TM312 includes 6-8% by mass of organic acid and 0.2-0.5% by mass of corrosion inhibitor; The organic acid is one or more of tartaric acid, citric acid, malic acid, and oxalic acid, and the corrosion inhibitor is one or more of sodium molybdate and benzotriazole; The surface of the titanium-aluminum bonding piece is a chromium-containing silicon-carbon-nitrogen PVD film layer with a chrome-plated base.

2. The stripping process according to claim 1, characterized in that: The pH adjuster is citric acid.

3. The stripping process according to claim 1, characterized in that: In the step S2, the anode is connected to the workpiece, and the cathode plate is any one of a stainless steel plate and a high-purity graphite plate.

4. The stripping process according to claim 1, characterized in that: In step S4, the cathode is connected to the workpiece, and the anode plate is a high-purity graphite plate.

5. Application of the stripping process according to any one of claims 1 to 4 in the stripping of titanium-aluminum combined parts.