A kind of iron-based soft magnetic amorphous alloy powder and preparation method thereof

By combining the addition of specific elements and preparing by aerosolization or water atomization method, the problems of complex process and insufficient iron loss performance of iron-based soft magnetic amorphous alloy powder are solved, and amorphous powder with high spherical shape and low iron loss are achieved , improves magnetic properties and corrosion resistance.

CN118653110BActive Publication Date: 2024-11-22HUICI (JIAXING) NEW MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411125286.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-16
Publication Date
2024-11-22
Estimated Expiration
2044-08-16

AI Technical Summary

Technical Problem

The preparation process of existing iron-based soft magnetic amorphous alloy powders is complex, and the powder is not easy to form a spherical shape, and the iron loss performance needs to be improved.

Method used

By reasonably combining the addition of chromium elements, M elements (such as Ni, Co, Mn and Y), silicon, boron, carbon and phosphorus, and introducing a small amount of oxygen elements, iron-based soft magnetism is prepared by aerosolization or water atomization method. Amorphous alloy powder, amorphous powder with high spherical shape and low iron loss.

Benefits of technology

It significantly improves the saturated magnetic induction strength and magnetic permeability of iron-based amorphous alloy powder, reduces high-frequency iron loss, and improves corrosion resistance. The preparation process is relatively simple and does not contain precious metal elements.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118653110B_ABST
    Figure CN118653110B_ABST
Patent Text Reader

Abstract

The present invention discloses an iron-based soft magnetic amorphous alloy powder and a preparation method thereof. The composition of the iron-based soft magnetic amorphous alloy powder is expressed as follows: Fe 100‑x‑y‑a‑b‑c‑d Cr x M y Si a B b C c P d O e , wherein the element M is composed of at least one of Ni, Co, Mn and Y, and x, y, a, b, c, d and e represent the mass percentage of the corresponding components, respectively, wherein 0.5%≤x≤5%, 0%<y≤5%, 0.1%≤a≤10.6%, 0.1%≤b≤5.8%, 0.1%≤c≤1.6%, 0.1%≤d≤10%, 0.05%≤e≤1.0% and 1%≤x+y≤6% and 3%≤a+b+c+d+e≤20% are satisfied; through the implementation of the present invention, amorphous powders with high sphericity of different particle sizes can be prepared.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of magnetic materials, and in particular to an iron-based soft magnetic amorphous alloy powder and a preparation method thereof. Background Art

[0002] Soft magnetic materials are magnetic materials with low coercivity and high magnetic permeability. They can be easily magnetized and demagnetized under the action of an external magnetic field. They are mainly used in equipment and devices for magnetic conductivity, electromagnetic energy conversion and transmission. The development of soft magnetic materials has gone through multiple systems, including electrical pure iron, Fe-Si alloy (silicon steel), Fe-Ni alloy (Permalloy), Fe-Al alloy, Fe-Si-Al alloy, Fe-Co alloy, soft ferrite, and iron-based amorphous and nanocrystalline alloys. At present, the most widely used soft magnetic materials are silicon steel and soft ferrite. Among them, silicon steel has high saturation magnetic induction intensity, but its iron loss is high at high frequency and is not suitable for high-frequency applications. Soft ferrite has low loss at high frequency, but due to its low saturation magnetization intensity and poor temperature characteristics, it is not suitable for some fields that require high magnetic energy density and high temperature tolerance. Therefore, studying how to prepare materials with both high saturation magnetization intensity and low iron loss has become a hot topic in the field of soft magnetism. Among them, the development of iron-based amorphous alloys is the most promising research direction.

[0003] Different from traditional crystalline materials, amorphous alloys have the characteristics of low coercivity, high magnetic permeability and low loss due to their uniform structure, lack of crystal anisotropy, high resistivity, low coercivity, high magnetic permeability and low loss. Their comprehensive soft magnetic properties are superior to traditional magnetic materials such as oriented silicon steel, ferrite and Permalloy. Currently, the more mature amorphous soft magnetic alloys mainly include iron-based, cobalt-based, iron-cobalt-based and iron-nickel-based. Among them, cobalt-based and iron-nickel-based amorphous have high magnetic permeability and are often used in magnetic shielding and other fields. Iron-cobalt-based has the characteristics of high saturation magnetic induction intensity and high Curie temperature and is often used in high temperature fields.

[0004] Iron-based amorphous alloys were born in the 1960s and were first produced by Allied Chemical in the United States with a registered brand name of Metglas. Iron-based bulk amorphous alloys were first produced by Akihisa Inoue, one of the inventors of the present invention, in 1995. Due to their low cost and excellent comprehensive magnetic properties, iron-based amorphous alloys have become the most widely used amorphous magnetic materials and have broad application prospects.

[0005] Soft magnetic powder is an important component material for preparing magnetic powder cores. Due to its small particle size, soft magnetic powder is separated by insulating materials in the magnetic powder core. The change of magnetic permeability with frequency is relatively stable, and the eddy current loss is extremely low. It can be applied to higher frequencies and is often used in high-frequency inductors. Soft magnetic powders include iron powder, iron silicon powder, iron silicon aluminum alloy powder, Permalloy (iron nickel) powder, ferrite powder and other crystalline magnetic powders and iron-based amorphous soft magnetic powders.

[0006] Iron powder has high saturation magnetic induction intensity and low cost, but it is easily corroded, and its performance degrades significantly and has large losses at high frequencies; iron silicon powder has high saturation magnetic induction intensity, good magnetic permeability and low hysteresis loss, and its performance is better than iron powder, but its processing cost is usually higher than ordinary iron powder, with low resistivity and large high-frequency losses; sendustine powder is the most widely used magnetic powder at present, with a magnetostriction coefficient close to zero, high saturation magnetic induction intensity and magnetic permeability, and low losses, but poor DC bias characteristics; iron-nickel alloy powder has very high magnetic permeability, low hysteresis loss, good frequency characteristics and DC bias characteristics, but its cost is much higher than iron powder or silicon steel powder; iron-nickel-molybdenum alloy powder has excellent performance, but its high cost also limits its application accordingly; ferrite powder has high resistivity, can reduce eddy current losses, and is suitable for high-frequency applications; but compared with metallic soft magnetic materials, ferrite has low saturation flux density and poor temperature characteristics. Amorphous soft magnetic powder has good comprehensive properties, high magnetic permeability, high resistance, etc., which makes it more and more widely used in electronic and power applications; but because its amorphous forming ability is affected by the composition, the lower the amorphous forming ability, the more stringent the preparation conditions are, and the constraints of the preparation process prevent it from exerting its performance advantages.

[0007] At present, in order to solve the above problems of soft magnetic powder, researchers have studied a variety of alloy systems and their preparation methods and applied for a number of national invention patents, including:

[0008] Chinese patent CN104190945A discloses a method of embrittlement of an amorphous strip and crushing the embrittled amorphous strip to obtain an amorphous metal powder Fe-Si-B powder. The alloy powder prepared by the strip crushing method has sharp edges and corners, which is difficult to insulate, thereby worsening the loss of its magnetic powder core. The iron loss recorded in the patent at 100kHz and 100mT is relatively high, which is 630-690 mW / cm 3 .

[0009] Chinese patent CN103730224A discloses a preparation process of an iron-based amorphous powder, which is divided into three main steps: first, the iron-based amorphous ribbon made by ultra-rapid solidification technology is heat-treated to increase its brittleness and facilitate crushing; then, the embrittled iron-based amorphous ribbon is crushed into powder; finally, the obtained iron-based amorphous powder is sieved and proportioned to mix into a mixed powder containing 40% to 70% coarse powder and 30% to 60% fine powder. The powder has a magnetic permeability of more than 200, but the data on its iron loss performance has not been published.

[0010] Chinese patent CN107683512B prepares magnetic powder with low magnetic loss and good corrosion resistance by mixing a plurality of powders such as a first alloy powder prepared by an aerosol method and a second alloy powder prepared by a water mist method and having an average particle size smaller than that of the first alloy powder. The magnetic powder is judged as having good corrosion resistance if the surface color of the sample is the same gray as before the test, and as having poor corrosion resistance if the surface color of the sample changes to ochre or even brown. The loss does not exceed 4000 mW / cm at a frequency of 1 MHz and a magnetic field of 40 mT. 3 The sample is judged as good quality and will exceed 4000 mW / cm 3 The sample was judged as a defective product. It can be seen that the powder preparation requires at least two preparation processes and needs to mix two or more powders for preparation, and the preparation process is relatively complicated.

[0011] Chinese patent CN101802240A discloses an iron-based soft magnetic amorphous alloy powder, the composition of which is [Fe a (Si x B y P z ) 1-a ] 100-b L b Indicated by . Wherein, L is one or more elements selected from Al, Cr, Zr, Nb, Mo, Hf, Ta and W. The iron-based soft magnetic amorphous alloy has high saturation magnetic induction intensity and magnetic permeability, but poor corrosion resistance and high iron loss. The iron loss at 100kHz and 100mT is 760-1380 mW / cm 3 .

[0012] Chinese patent CN102264938B discloses a composition of Fe 100-x-u J x R u The alloy comprises: R is composed of at least one of P, C, B and Si, and J is composed of at least one of Cr, Co, Ni and Nb; the powder can achieve the characteristics of high magnetic permeability and low iron loss, and its minimum iron loss reaches 276 mW / cm 3 , which is a significant improvement over the previously mentioned patents, however, there is still room for further improvement.

[0013] The above patents have improved the soft magnetic properties of amorphous alloy powders to varying degrees by designing composition and improving preparation processes. However, they have the following obvious defects in general: (1) The preparation process is complicated; (2) The alloy powder prepared by the strip crushing method has sharp edges and cannot be spherical or nearly spherical; (3) The iron loss performance still needs to be further improved.

[0014] In summary, developing an amorphous soft magnetic alloy powder with a simple preparation process, no precious metal elements, a nearly spherical shape, and high saturation magnetic induction intensity, low coercive force and low iron loss is of significant importance for the application and development of amorphous soft magnetic alloys. Summary of the invention

[0015] In view of the deficiencies in the prior art, the present invention provides an iron-based soft magnetic amorphous alloy powder and a preparation method thereof, aiming to solve the problems that the preparation process is complicated, the alloy powder cannot be spherical or nearly spherical, and the iron loss performance still needs to be improved.

[0016] To achieve the above object, the present invention provides the following technical solutions:

[0017] In one aspect, the present invention provides an iron-based soft magnetic amorphous alloy powder, wherein the composition of the iron-based soft magnetic amorphous alloy powder is expressed as follows: Fe 100-x-y-a-b-c-d Cr x M y Si a B b C c P d O e , wherein the element M is composed of at least one of Ni, Co, Mn and Y, and x, y, a, b, c, d and e represent the mass percentage of the corresponding components, wherein 0.5%≤x≤5%, 0%<y≤5%, 0.1%≤a≤10.6%, 0.1%≤b≤5.8%, 0.1%≤c≤1.6%, 0.1%≤d≤10%, 0.05%≤e≤1.0% and 1%≤x+y≤6% and 3%≤a+b+c+d+e≤20%. By cleverly combining and adding metal elements such as chromium and M elements and non-metallic elements such as silicon, boron, carbon and phosphorus, as well as introducing a small amount of oxygen, the excellent amorphous forming ability of the amorphous alloy is successfully achieved. This innovative design can easily prepare amorphous powders with a high degree of sphericity, and the prepared iron-based amorphous alloy powders have significantly improved saturation magnetic induction intensity, excellent magnetic permeability, significantly reduced high-frequency iron loss, and improved corrosion resistance.

[0018] Preferably, the element O is added by adding oxides during smelting or by adding the atmosphere during smelting the alloy.

[0019] Preferably, 1.2%≤x≤4.0%, 0%<y≤1%, 1%≤a≤7.5%, 0.5%≤b≤4.3%, 0.3%≤c≤1.1%, 1%≤d≤7.5%, 0.15%≤e≤0.6% and 1.5%≤x+y≤4% and 4%≤a+b+c+d+e≤18.5%.

[0020] In another aspect, the present invention provides a method for preparing an iron-based soft magnetic amorphous alloy powder, comprising the following steps:

[0021] Step 1: Prepare the master alloy raw materials: mix Fe 100-x-y-a-b-c-d Cr x M y Si a B b C c P d O e , wherein the element M is composed of at least one of Ni, Co, Mn and Y, and x, y, a, b, c and d represent the mass percentage of the corresponding components, respectively, wherein 0.5%≤x≤5%, 0%<y≤5%, 0.1%≤a≤10.6%, 0.1%≤b≤5.8%, 0.1%≤c≤1.6%, 0.1%≤d≤10%, 0.05%≤e≤1.0% and 1%≤x+y≤6% and 3%≤a+b+c+d+e≤20% are satisfied;

[0022] Step 2: preparing a master alloy: adding the master alloy raw materials prepared in step 1 into a smelting furnace, heating them in air or under a protective atmosphere until they are melted and keeping them warm for a period of time to fully melt the master alloy raw materials, and stirring them during the smelting process to make the alloy composition uniform, thereby obtaining an alloy ingot with uniform composition;

[0023] Step 3: remelting the master alloy: crush the master alloy prepared in step 2, add it into the melting furnace of the atomizing equipment for remelting, heat it in air or under a protective atmosphere until it melts, and keep it warm for 5 to 60 minutes. At the same time, after the master alloy is completely melted, open or continue to maintain the protective atmosphere and remove the slag to obtain the melt;

[0024] Step 4: preparing alloy powder: preparing iron-based soft magnetic amorphous alloy powder from the melt obtained in step 3 by gas atomization or water atomization;

[0025] Step 5: Screening the prepared iron-based soft magnetic amorphous alloy powder to obtain iron-based soft magnetic amorphous alloy powder with a target particle size.

[0026] Preferably, in step 2, the master alloy raw material prepared in step 1 is added into a smelting furnace, heated to melt in air or under a protective atmosphere, and kept warm for at least 5 minutes, and the protective atmosphere is a gas that is not easy to chemically react with the alloy.

[0027] Preferably, in step 4, the atomization pressure of the iron-based soft magnetic amorphous alloy powder prepared by gas atomization is 1.5 to 17.5 MPa.

[0028] Preferably, in step 4, the atomization pressure of the iron-based soft magnetic amorphous alloy powder prepared by water atomization is 5 to 100 MPa.

[0029] Preferably, in step 5, the prepared iron-based soft magnetic amorphous alloy powder is sieved to obtain iron-based soft magnetic amorphous alloy powder of target particle size, and the target particle size of the iron-based soft magnetic amorphous alloy powder is between 1 and 150 μm, and the average particle size is 5 to 50 μm.

[0030] Preferably, the saturation magnetic induction intensity of the iron-based soft magnetic amorphous alloy powder is 1.20-1.50 T, and the effective magnetic permeability is 30-70.

[0031] Preferably, the iron-based soft magnetic amorphous alloy powder has a low iron loss of 100 to 350 mW / cm under the conditions of 100 kHz and 100 mT. 3 .

[0032] Substantial effects of the present invention:

[0033] 1. In the present invention, the excellent amorphous forming ability of the amorphous alloy is successfully achieved by ingeniously combining and adding metal elements such as chromium and M elements and non-metallic elements such as silicon, boron, carbon and phosphorus, and introducing a small amount of oxygen elements. This innovative design can easily prepare amorphous powders with a high degree of sphericity, and the prepared iron-based amorphous alloy powder has a significantly improved saturation magnetic induction intensity, excellent magnetic permeability, significantly reduced high-frequency iron loss, and improved corrosion resistance. The preparation process is relatively simple and does not contain precious metal elements, which is of great importance for the application and development of amorphous soft magnetic alloys;

[0034] 2. In the present invention, the alloy composition proposed not only has outstanding advantages in amorphous forming ability, but also has made significant breakthroughs in the sphericity of the prepared powder, which provides greater flexibility for preparing amorphous powders of different particle sizes and can customize the required specifications according to specific needs;

[0035] 3. In the present invention, the introduction of oxygen element not only has no adverse effect on the magnetic properties, but also effectively improves the resistivity and reduces the loss of the alloy. Compared with other alloy systems, the oxygen content in the alloy is different from other alloy systems in that the lower the better, so the conditions for preparing the alloy are relatively loose; in addition, the high saturation magnetic induction intensity and excellent magnetic permeability exhibited by the alloy powder make it have a wide range of potential applications in the field of magnetic applications, and the characteristics of low high-frequency iron loss provide more possibilities for the design of high-frequency electronic devices;

[0036] 4. The present invention not only provides a more efficient way for the preparation of amorphous alloy powders, but also expands the application potential of alloy powders in the field of magnetic materials, brings new prospects for research and industrial applications in related fields, and has certain use value and promotion value. BRIEF DESCRIPTION OF THE DRAWINGS

[0037] Figure 1 This is a SEM appearance morphology of the iron-based amorphous alloy powder prepared in Example 1.

[0038] Figure 2 This is the XRD spectrum of the iron-based amorphous alloy powder prepared in Example 1.

[0039] Figure 3 This is the particle size distribution diagram of the iron-based amorphous alloy powder prepared in Example 1.

[0040] Figure 4 It is a comparison chart of the iron loss of the iron-based amorphous alloy powder prepared in Example 1 and the iron loss of the alloy in the comparative example.

[0041] Figure 5 This is the particle size distribution diagram of the iron-based amorphous alloy powder prepared in Example 2. DETAILED DESCRIPTION

[0042] In order to facilitate the understanding of the present invention, the present invention is described in more detail below in conjunction with the accompanying drawings and specific implementation methods.

[0043] Unless otherwise defined, all technical and scientific terms used in this specification have the same meaning as those commonly understood by those skilled in the art to which the present invention belongs. The terms used in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The term "and / or" used in this specification includes any and all combinations of one or more of the related listed items.

[0044] An iron-based soft magnetic amorphous alloy powder, the composition of the iron-based soft magnetic amorphous alloy powder is expressed as: Fe 100-x-y-a-b-c-d Cr x M y Si a B b C c P d O e , wherein the element M is composed of at least one of Ni, Co, Mn and Y, and x, y, a, b, c, d and e represent the mass percentage of the corresponding components respectively, wherein 0.5%≤x≤5%, 0%<y≤5%, 0.1%≤a≤10.6%, 0.1%≤b≤5.8%, 0.1%≤c≤1.6%, 0.1%≤d≤10%, 0.05%≤e≤1.0% and satisfies 1%≤x+y≤6% and 3%≤a+b+c+d+e≤20%.

[0045] As an embodiment, the element O (oxygen element) in the chemical formula is added by adding oxides during smelting or by the atmosphere during smelting of the alloy.

[0046] As an embodiment, the iron-based soft magnetic amorphous alloy powder refers to an amorphous alloy component having an iron content of 50% or more; based on the viewpoint of increasing the saturation magnetic induction intensity of the amorphous alloy powder, the added amount of the iron element is 81% or more.

[0047] As an implementation method, the addition of Cr (chromium) element can improve the corrosion resistance of the magnetic powder, and because chromium is antiferromagnetic, in order to ensure the saturation magnetic induction intensity of the alloy, the content of chromium element is greater than 1.2% and less than 4.0%.

[0048] As an implementation mode, the addition of M (at least one of nickel Ni, cobalt Co, manganese Mn and yttrium Y) element can improve the amorphous forming ability of the alloy, wherein the addition of cobalt element can further improve the saturation magnetic induction intensity of the alloy and reduce the magnetostriction of the alloy, and the addition of nickel element can further improve the magnetic permeability of the alloy. The amount of M element added is to reduce the cost of the alloy, and the content is greater than 0% and less than 1%.

[0049] The sum of the amounts of Cr (chromium) element and M element added is 1.5% or more and 4% or less.

[0050] Silicon, boron, carbon and phosphorus elements can effectively improve the amorphous forming ability and resistivity of the alloy.

[0051] The content of Si (silicon) element is 1% or more and 7.5% or less.

[0052] The B (boron) element content is 0.5% or more and 4.3% or less.

[0053] The content of the C (carbon) element is 0.3% or more and 1.1% or less.

[0054] The content of the P (phosphorus) element is 1% or more and 7.5% or less.

[0055] O (oxygen) is generally considered to be an element that is harmful to performance, but in this alloy, a small amount of oxygen not only does not deteriorate the magnetic properties, but can effectively reduce iron loss. Oxygen can be added by adding oxides during smelting, or by adding the atmosphere during smelting of the alloy, and the oxygen content is 0.15% or more and 0.6% or less.

[0056] The sum of the added amounts of the five elements of silicon, boron, carbon, phosphorus and oxygen is 4% or more and 18.5% or less.

[0057] The preparation method of iron-based soft magnetic amorphous alloy powder is as follows:

[0058] Step 1: Prepare the master alloy raw materials: mix Fe 100-x-y-a-b-c-d Cr x M y Sia B b C c P d O e , in the chemical formula, the element M is composed of at least one of Ni, Co, Mn and Y, and x, y, a, b, c and d represent the mass percentage of the corresponding components, respectively, wherein 0.5%≤x≤5%, 0%<y≤5%, 0.1%≤a≤10.6%, 0.1%≤b≤5.8%, 0.1%≤c≤1.6%, 0.1%≤d≤10%, 0.05%≤e≤1.0% and 1%≤x+y≤6% and 3%≤a+b+c+d+e≤20% are satisfied;

[0059] Step 2: preparing a master alloy: adding the master alloy raw materials prepared in step 1 into a smelting furnace, heating them to melt in air or argon or nitrogen and other gases that are not easy to react chemically with the alloy, and keeping them warm for at least 5 minutes, so that the master alloy raw materials are fully melted, and stirring is performed during the smelting process to make the alloy composition uniform, so as to obtain an alloy ingot with uniform composition;

[0060] Step 3: remelting the master alloy: crush the master alloy prepared in step 2, add it into the melting furnace of the atomizing equipment for remelting, heat it in air or under a protective atmosphere until it melts, and keep it warm for 5 to 60 minutes. At the same time, after the master alloy is completely melted, open or continue to maintain the protective atmosphere and remove the slag to obtain the melt;

[0061] Step 4: preparing alloy powder: preparing iron-based soft magnetic amorphous alloy powder from the melt obtained in step 3 by gas atomization or water atomization;

[0062] Step 5: Screening the prepared iron-based soft magnetic amorphous alloy powder to obtain iron-based soft magnetic amorphous alloy powder with a target particle size.

[0063] As an implementation mode, in step 4, the atomization pressure of preparing the iron-based soft magnetic amorphous alloy powder by gas atomization is 1.5 to 17.5 MPa.

[0064] As an implementation mode, in step 4, the atomization pressure of preparing the iron-based soft magnetic amorphous alloy powder by water atomization is 5 to 100 MPa.

[0065] As an implementation mode, in step 5, the prepared iron-based soft magnetic amorphous alloy powder is sieved to obtain iron-based soft magnetic amorphous alloy powder of target particle size. The target particle size of the iron-based soft magnetic amorphous alloy powder is between 1 and 150 μm, and the average particle size is 5 to 50 μm.

[0066] As an implementation mode, the saturation magnetic induction intensity of the iron-based soft magnetic amorphous alloy powder is 1.20-1.50T, and the effective magnetic permeability is 30-70.

[0067] As an implementation method, the iron-based soft magnetic amorphous alloy powder has a low iron loss of 100 to 350 mW / cm at 100 kHz and 100 mT. 3 . Embodiment 1:

[0068] Weigh the raw materials containing at least iron, chromium, nickel, silicon, boron, carbon, phosphorus and oxygen as single substances or compounds containing these elements according to the alloy composition Fe 87.3 Cr 1.9 Ni 0.2 Si3B2C 0.5 P5O 0.1 The raw materials with good proportions are then charged into an induction melting furnace and heated to above the melting point to make the alloy molten and kept warm for 10 minutes, and then poured to obtain an alloy ingot with uniform composition.

[0069] The alloy ingots were crushed and loaded into a melting furnace equipped with gas atomization equipment to prepare alloy powder by gas atomization. Argon was used as the atomizing gas for atomization treatment, and the atomization pressure was 8 MPa. The alloy powder was dried in a vacuum drying oven to obtain the target powder. The morphology of the target powder was analyzed by scanning electron microscopy (SEM). Figure 1 As shown, it can be seen that the powder is spherical, with a smooth surface and no obvious defects such as holes. The structure was detected by X-ray diffractometer (XRD), and the results are as follows Figure 2 As shown, it can be seen that there is no diffraction peak corresponding to any crystal in the XRD spectrum, only a broad diffuse scattering peak, indicating that the prepared powder is completely amorphous.

[0070] Particle size distribution Figure 3 As shown, the target particle size of the iron-based soft magnetic amorphous alloy powder is 2 to 96 μm, and the average particle size is 12.55 μm.

[0071] The iron loss of the iron-based amorphous alloy powder prepared in this embodiment at 100kHz and 100mT is 212.6 mW / cm 3 ; Figure 4 : is a comparison chart of the iron loss of the iron-based amorphous alloy powder prepared in Example 1 and the iron loss of the alloy in the comparative example. It can be seen from the comparison that the iron loss of the alloy in Example 1 of the present invention is much lower than the iron loss of the alloy powder in the comparative example.

[0072] The iron-based amorphous alloy powder prepared in this embodiment exhibits a high saturation magnetic induction intensity of 1.25 T and an effective magnetic permeability of 44.0.

[0073] The structure and properties of the alloy powder prepared above are listed in Table 1. For comparison, the alloy properties of commonly used soft magnetic powders are listed in Table 1 as Comparative Examples 1-5. It can be seen from the comparison that the alloy properties in this embodiment are much higher than those of the commonly used alloy powders. Embodiment 2:

[0074] Weigh the raw materials containing at least iron, chromium, cobalt, silicon, boron, carbon, phosphorus and oxygen as single substances or compounds containing these elements according to the alloy composition Fe 90 Cr2Co 0.4 SiC 1.75 C 0.5 P3O 0.35 The raw materials with good proportions are then charged into an induction melting furnace and heated to above the melting point to make the alloy molten and kept warm for 10 minutes, and then poured to obtain an alloy ingot with uniform composition.

[0075] The above alloy ingots were crushed and loaded into a smelting furnace equipped with gas atomization equipment. The alloy powder was prepared by water atomization. The pressure of the coolant during spraying was set to 70 MPa. The alloy powder was dried in a vacuum drying oven to obtain the target powder. The powder was spherical, with a smooth surface and no obvious defects such as pores or holes. There was no diffraction peak corresponding to any crystallization on the XRD spectrum, only a broad diffuse scattering peak, indicating that the prepared powder was completely amorphous.

[0076] Particle size distribution Figure 4 As shown, the target particle size of the iron-based soft magnetic amorphous alloy powder is 3.5-40 μm, and the average particle size is 10.05 μm.

[0077] The iron-based amorphous alloy powder prepared in this embodiment exhibits a high saturation magnetic induction intensity of 1.41T, an effective magnetic permeability of 39.3, and an iron loss of 175.9 mW / cm at 100kHz and 100mT. 3 .

[0078] The structure and properties of the alloy powder prepared above are also listed in Table 1. It can be seen from the comparison that the alloy performance in this embodiment is much higher than that of the currently commonly used alloy powder. Embodiment 3:

[0079] Weigh the raw materials containing at least iron, chromium, manganese, silicon, boron, carbon, phosphorus and oxygen as single substances or compounds containing these elements according to the alloy composition Fe 91 Cr 1.5 Mn 0.4 SiC 2.49 C 0.5 P2O 0.11The raw materials with good proportions are then charged into an induction melting furnace and heated to above the melting point to make the alloy molten and kept warm for 10 minutes, and then poured to obtain an alloy ingot with uniform composition.

[0080] The alloy ingots were crushed and loaded into a melting furnace equipped with gas atomization equipment, and alloy powders were prepared by water atomization. The pressure of the coolant during spraying was set to 65MPa. After the alloy powders were dried in a vacuum drying oven, the target powders were obtained. The powders were spherical, smooth in surface, and free of obvious defects such as holes and pores. In addition, there were no diffraction peaks corresponding to crystallization on the XRD spectrum, only a broad diffuse scattering peak, indicating that the prepared powders were completely amorphous.

[0081] The target particle size of the iron-based soft magnetic amorphous alloy powder is 4 to 49 μm, and the average particle size is 11.96 μm.

[0082] The iron-based amorphous alloy powder prepared in this embodiment exhibits a high saturation magnetic induction intensity of 1.39T, an effective magnetic permeability of 42.6, and an iron loss of 227.8 mW / cm at 100kHz and 100mT. 3 .

[0083] The structure and properties of the alloy powder prepared above are listed in Table 1. It can be seen from the comparison that the alloy performance in this embodiment is much higher than that of the currently commonly used alloy powder.

[0084] Table 1:

[0085]

[0086] The raw materials and equipment used in the present invention, unless otherwise specified, are all commonly used raw materials and equipment in the art; the methods used in the present invention, unless otherwise specified, are all conventional methods in the art.

[0087] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any way. Any simple modification, change and equivalent transformation made to the above embodiment based on the technical essence of the present invention still falls within the protection scope of the technical solution of the present invention.

Claims

1. An iron-based soft magnetic amorphous alloy powder, characterized in that: The composition of the iron-based soft magnetic amorphous alloy powder is expressed as: Fe 100-x-y-a-b-c-d Cr x M y Si a B b C c P d O e , wherein the element M is composed of at least one of Ni, Co, Mn and Y, and x, y, a, b, c, d and e represent the mass percentage of the corresponding components, respectively, wherein 0.5%≤x≤5%, 0%<y≤5%, 0.1%≤a≤10.6%, 0.1%≤b≤5.8%, 0.1%≤c≤1.6%, 0.1%≤d≤10%, and 0.15%≤e≤0.6%.

2. The iron-based soft magnetic amorphous alloy powder according to claim 1, characterized in that: The x, y, a, b, c, d and e respectively represent the mass percentage of the corresponding components, wherein 0.5%≤x≤5%, 0%<y≤5%, 0.1%≤a≤10.6%, 0.1%≤b≤5.8%, 0.1%≤c≤1.6%, 0.1%≤d≤10%, 0.15%≤e≤0.6% and satisfy 1%≤x+y≤6% and 3%≤a+b+c+d+e≤20%.

3. The iron-based soft magnetic amorphous alloy powder according to claim 2, characterized in that: The element O is added by adding oxides during smelting or by adding the atmosphere during smelting the alloy.

4. A method for preparing an iron-based soft magnetic amorphous alloy powder, characterized in that: The following steps are involved: Step 1: Prepare the master alloy raw materials: mix Fe 100-x-y-a-b-c-d Cr x M y Si a B b C c P d O e , wherein the element M is composed of at least one of Ni, Co, Mn and Y, and x, y, a, b, c and d represent the mass percentage of the corresponding components, respectively, wherein 0.5%≤x≤5%, 0%<y≤5%, 0.1%≤a≤10.6%, 0.1%≤b≤5.8%, 0.1%≤c≤1.6%, 0.1%≤d≤10%, 0.15%≤e≤0.6% and 1%≤x+y≤6% and 3%≤a+b+c+d+e≤20% are satisfied; Step 2: preparing a master alloy: adding the master alloy raw materials prepared in step 1 into a smelting furnace, heating them in air or under a protective atmosphere until they are melted and keeping them warm for a period of time to fully melt the master alloy raw materials, and stirring them during the smelting process to make the alloy composition uniform, thereby obtaining an alloy ingot with uniform composition; Step 3: remelting the master alloy: crush the master alloy prepared in step 2, add it into the melting furnace of the atomizing equipment for remelting, heat it in air or under a protective atmosphere until it melts, and keep it warm for 5 to 60 minutes. At the same time, after the master alloy is completely melted, open or continue to maintain the protective atmosphere and remove the slag to obtain the melt; Step 4: preparing alloy powder: preparing iron-based soft magnetic amorphous alloy powder from the melt obtained in step 3 by gas atomization or water atomization; Step 5: Screening the prepared iron-based soft magnetic amorphous alloy powder to obtain iron-based soft magnetic amorphous alloy powder with a target particle size.

5. The method for preparing an iron-based soft magnetic amorphous alloy powder according to claim 4, characterized in that: In the step 2, the master alloy raw material prepared in step 1 is added into a smelting furnace, heated to melt in air or under a protective atmosphere, and kept warm for at least 5 minutes, and the protective atmosphere is a gas that is not easy to chemically react with the alloy.

6. The method for preparing an iron-based soft magnetic amorphous alloy powder according to claim 4, characterized in that: In the step 4, the atomization pressure of the iron-based soft magnetic amorphous alloy powder prepared by gas atomization is 1.5-17.5 MPa.

7. The method for preparing an iron-based soft magnetic amorphous alloy powder according to claim 4, characterized in that: In the step 4, the atomization pressure of the iron-based soft magnetic amorphous alloy powder prepared by the water atomization method is 5 to 100 MPa.

8. The method for preparing an iron-based soft magnetic amorphous alloy powder according to claim 4, characterized in that: In step 5, the prepared iron-based soft magnetic amorphous alloy powder is sieved to obtain iron-based soft magnetic amorphous alloy powder with a target particle size. The target particle size of the iron-based soft magnetic amorphous alloy powder is between 1 and 150 μm, and the average particle size is 5 to 50 μm.

9. The method for preparing an iron-based soft magnetic amorphous alloy powder according to claim 4, characterized in that: The saturation magnetic induction intensity of the iron-based soft magnetic amorphous alloy powder is 1.20-1.50T, and the effective magnetic permeability is 30-70.

10. The method for preparing an iron-based soft magnetic amorphous alloy powder according to claim 4, characterized in that: The iron-based soft magnetic amorphous alloy powder has a low iron loss of 100 to 350 mW / cm under the conditions of 100 kHz and 100 mT. 3 .