Yttrium-based protective film, method for producing same, and member
By using an yttrium protective film with peak strength ratio and high Vickers hardness in the manufacturing of semiconductor components, combined with the design of a multi-layer base layer, the problem of insufficient corrosion resistance of the existing yttrium protective film is solved, and the durability of semiconductor components is significantly improved. Build quality and reliability.
Patent Information
- Application Number
- CN202380022035.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-02-18
- Filing Date
- 2023-02-14
- Publication Date
- 2024-09-24
AI Technical Summary
Existing yttrium protective films have insufficient corrosion resistance when exposed to plasma, which may cause circuit defects during the manufacturing process of semiconductor devices.
By using the ion-assisted evaporation method in a vacuum, an yttrium protective film with a Y5O4F7 peak intensity ratio of more than 60% in the X-ray diffraction pattern, a porosity of less than 1.5 volume%, and a Vickers hardness of more than 500MPa is formed. Y2O3 and YF3 are used as Evaporation source, and form multiple base layers on the surface of the substrate to improve the density and plasma resistance of the protective film.
An yttrium protective film with excellent plasma resistance has been realized, which reduces the occurrence of particles falling off during the plasma etching process and improves the manufacturing quality and reliability of semiconductor components.
Smart Images

Figure CN118696147A
Abstract
Description
Technical Field
[0001] The invention relates to a yttrium protective film and a manufacturing method and component thereof. Background Art
[0002] When manufacturing semiconductor elements, for example, the surface of a semiconductor substrate (silicon wafer) is micro-processed by dry etching using halogen gas plasma in a chamber, or the chamber after removing the semiconductor substrate after dry etching is cleaned using oxygen plasma.
[0003] At this time, the components exposed to the plasma gas in the chamber may corrode, and the corroded parts may fall off from the corroded components in the form of particles. The fallen particles (grains) may adhere to the semiconductor substrate and become foreign matter that causes defects in the circuit.
[0004] Therefore, conventionally, a protective film containing yttrium oxyfluoride (yttrium protective film) is known as a protective film for protecting a member exposed to plasma.
[0005] Patent Document 1 discloses a thermal spray coating formed by thermal spraying and containing yttrium oxyfluoride (yttrium oxyfluoride).
[0006] Prior art literature
[0007] Patent Literature
[0008] Patent Document 1: Japanese Patent Application Publication No. 2018-76546 Summary of the invention
[0009] The present inventors have conducted studies and have found that conventional yttrium protective films may have insufficient plasma resistance (corrosion resistance to plasma).
[0010] The present invention has been made in view of the above circumstances, and an object of the present invention is to provide an yttrium protective film having excellent plasma resistance.
[0011] The present inventors have conducted intensive studies and, as a result, have found that the above-mentioned object can be achieved by adopting the following configuration, thereby completing the present invention.
[0012] That is, the present invention provides the following [1] to
[14] .
[0013] [1] A yttrium protective film, Y in the X-ray diffraction spectrum 5 O 4 F 7 The peak intensity ratio is 60% or more, the porosity is less than 1.5% by volume, and the Vickers hardness is 500 MPa or more.
[0014] [2] The yttrium protective film according to [1] above, wherein the fluorine content is 35 to 60 atomic %.
[0015] [3] The yttrium protective film according to [1] or [2] above, wherein the crystallite size is 30 nm or less.
[0016] [4] The yttrium protective film according to any one of [1] to [3] above, wherein the thickness is 0.3 μm or more.
[0017] [5] The yttrium protective film according to any one of [1] to [4] above, wherein Y 5 O 4 F 7 The half-peak width of the rocking curve of the (151) crystal plane is less than 40°.
[0018] [6] A member comprising a substrate and the yttrium protective film according to any one of [1] to [5] above, which is disposed on a film formation surface which is a surface of the substrate.
[0019] [7] A component according to [6] above, wherein the substrate is composed of at least one selected from ceramics and metals, the ceramic is at least one selected from glass, quartz, alumina, aluminum nitride and aluminum oxynitride, and the metal is at least one selected from aluminum and an alloy containing aluminum.
[0020] [8] The component according to [6] or [7] above, wherein the surface roughness of the film-forming surface is 0.6 μm or less in terms of arithmetic mean roughness Ra.
[0021] [9] The member according to any one of [6] to [8] above, wherein the maximum length of the film-forming surface is 30 mm or more.
[0022]
[10] The member according to any one of [6] to [9], wherein there is one or more underlayers between the substrate and the yttrium protective film, and the underlayer contains a 2 O 3 、SiO 2 , Y 2 O 3 、MgO、ZrO 2 ,La 2 O 3 、Nd 2 O 3 , Yb 2 O 3 、Eu 2 O 3 and Gd 2 O 3 At least one oxide of
[0023]
[11] The component according to
[10] above, wherein there are two or more base layers between the substrate and the yttrium protective film, and the oxides in adjacent base layers are different from each other.
[0024]
[12] A component according to any one of [6] to
[11] above, wherein the substrate has a first film-forming surface with a specified maximum length and a second film-forming surface different from the first film-forming surface as the film-forming surface, the angle between the first film-forming surface and the second film-forming surface is 20° to 120°, and the area of the second film-forming surface is less than 60% of the total area of the film-forming surface.
[0025]
[13] The component according to any one of [6] to
[12] above, which is used inside a plasma etching device or a plasma CVD device.
[0026]
[14] A method for producing a yttrium protective film according to any one of [1] to [5], comprising: irradiating a substrate with ions of at least one element selected from oxygen, argon, neon, krypton and xenon in a vacuum while evaporating an evaporation source to adhere the yttrium protective film to the substrate, using Y 2 O 3 and YF 3 As the above evaporation source.
[0027] According to the present invention, it is possible to provide an yttrium protective film having excellent plasma resistance. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 It is a schematic diagram showing an example of a component.
[0029] Figure 2 This is a schematic diagram showing a ring-shaped substrate with half of it cut away.
[0030] Figure 3 1 is a schematic diagram showing a part of the cross section of another annular base material.
[0031] Figure 4 1 is a schematic diagram showing a part of the cross section of still another annular base material.
[0032] Figure 5 This is a schematic diagram showing an apparatus used for producing the yttrium protective film. DETAILED DESCRIPTION
[0033] The meanings of the terms in the present invention are as follows.
[0034] A numerical range expressed using "to" indicates a range including the numerical values described before and after "to" as the lower limit and the upper limit.
[0035] [Yttrium protective film]
[0036] The X-ray diffraction pattern of the yttrium protective film of this embodiment shows that Y 5 O 4 F 7 The peak intensity ratio is 60% or more, the porosity is less than 1.5% by volume, and the Vickers hardness is 500 MPa or more.
[0037] Hereinafter, the yttrium protective film is also simply referred to as a "protective film", and the yttrium protective film (protective film) of the present embodiment is also referred to as a "present protective film".
[0038] The yttrium protective film contains yttrium oxyfluoride.
[0039] As chemical formulas representing yttrium oxyfluoride, YOF, Y 5 O 4 F 7 YOF is an orthorhombic crystal with a lower hardness. 5 O 4 F 7 It is a special crystal structure called rhombohedron and has a high hardness.
[0040] The protective film has a rhombohedral crystal structure of Y 5 O 4 F 7 That is, the Y 5 O 4 F 7 The peak intensity ratio of is greater than a certain value. Therefore, the protective film is hard and the Vickers hardness is greater than a certain value.
[0041] Furthermore, since the present protective film is formed by the method (present production method) described later, it is dense and has a small porosity.
[0042] Such a protective film of the present invention is excellent in plasma resistance.
[0043] Hereinafter, the present protective film will be described in more detail.
[0044] 〈Peak intensity ratio〉
[0045] The Y in the X-ray diffraction spectrum of this protective film 5 O 4 F 7 The peak intensity ratio (hereinafter also referred to as “Y 5 O 4 F 7 The peak intensity ratio (“peak intensity ratio”) is 60% or more, preferably 80% or more, more preferably 90% or more, further preferably 95% or more, further preferably 98% or more, particularly preferably 99% or more, and most preferably 100%.
[0046] In order to make Y 5 O 4 F 7 The peak intensity ratio is within the above range, and the protective film is preferably produced by the method (present production method) described later.
[0047] Y 5 O 4 F 7 The peak intensity ratio is the value of Y when the sum of the main peak intensities of the following crystalline phases in the X-ray diffraction (XRD) pattern of the protective film is set to 100. 5 O 4 F 7 The ratio of the main peak intensity (unit: %).
[0048] In Y 5 O 4 F 7 The main peak position, Y 6 O 5 F 8 Crystal peak and Y 7 O 6 F 9 The peaks of the crystals overlapped, so they could not be discharged and a small amount of Y was generated. 6 O 5 F 8 and Y 7 O 6 F 9 possibility, but in Y 5 O 4 F 7 All the peaks at the main peak positions are taken as Y 5 O 4 F 7 The peaks are processed.
[0049] For the main peak of each crystalline phase, Y 2 O 3 appears near 2θ=29.2°, YOF appears near 2θ=28.1°, and Y 5 O 4 F 7 Appears near 2θ=28.1°.
[0050] YF 3 The main peak of Y 5 O 4 F 7 overlap, so there is YF 3 In the case of crystals, the YF 3 The intensity of the peak near 2θ=24.5°, the second main peak of the crystal, was multiplied by 1.3 to convert it into the main peak, which was taken as YF 3 The main peak intensity.
[0051] The XRD pattern of the protective film was obtained by performing XRD measurement in a microscopic 2D (two-dimensional) mode using an X-ray diffractometer (D8 DISCOVER Plus, manufactured by Bruker Corporation) under the following conditions.
[0052] ·X-ray source: CuKα ray (output: 45kV, current: 120mA)
[0053] Scanning range: 2θ=10°~80°
[0054] Step time: 0.2s / step
[0055] Scanning speed: 10° / min
[0056] Step width: 0.02°
[0057] Detector: Multi-mode detector EIGER (2D mode)
[0058] ·Incident side optical system: multi-layer film mirror + 1.0mmφ micro-slit + 1.0mmφ collimator
[0059] ·Light receiving side optical system: OPEN
[0060] 〈Vickers Hardness〉
[0061] Because the protective film has excellent plasma resistance, the Vickers hardness of the protective film is 500 MPa or more, preferably 800 MPa or more, more preferably 1000 MPa or more, further preferably 1100 MPa or more, further preferably 1200 MPa or more, particularly preferably 1250 MPa or more, and most preferably 1300 MPa or more.
[0062] The upper limit of the Vickers hardness of the present protective film is not particularly limited, and is, for example, 1500 MPa, preferably 1400 MPa. That is, the Vickers hardness of the present protective film is, for example, 500 to 1500 MPa.
[0063] In order to make the Vickers hardness within the above range, it is preferable to make the Y of the protective film 5 O 4 F 7 The peak intensity ratio is within the above range.
[0064] The Vickers hardness of the protective film was determined in accordance with JIS R1610:2003.
[0065] More specifically, the Vickers hardness (Hv0.2) is determined by applying a test force of 1.96 N using a hard microhardness tester (HMV-1, manufactured by Shimadzu Corporation) with a diamond indenter having a facing angle of 136°.
[0066] 〈Porosity〉
[0067] Due to the excellent plasma resistance of the protective film, the porosity of the protective film is less than 1.5% by volume, preferably less than 1.0% by volume, more preferably less than 0.5% by volume, further preferably less than 0.3% by volume, particularly preferably less than 0.2% by volume, and most preferably less than 0.1% by volume.
[0068] In order to adjust the porosity to the above range, it is preferable to produce the protective film by the method (present production method) described later.
[0069] The porosity of the protective film was determined as follows.
[0070] First, a focused ion beam (FIB) was used to perform a slope process in the thickness direction at an angle of 52° from the surface of the protective film toward the substrate to expose the cross section. The exposed cross section was observed at a magnification of 20,000 times using a field emission scanning electron microscope (FE-SEM) to capture its cross-sectional image.
[0071] The cross-sectional images are captured at multiple locations. Specifically, for example, when the protective film and the substrate are circular, the images are captured at a total of five points, including one point in the center of the surface of the protective film (or the surface of the substrate) and four points at a position 10 mm from the periphery, and the size of the cross-sectional image is set to 6 μm×5 μm. When the thickness of the protective film is 5 μm or more, cross-sectional images are captured at multiple shooting locations to enable observation of the cross section of the protective film in the thickness direction.
[0072] Next, the obtained cross-sectional image was analyzed using image analysis software (ImageJ, manufactured by National Institute of Health) to determine the area of the pore portion in the cross-sectional image. The ratio of the area of the pore portion to the total cross-sectional area of the protective film was calculated and regarded as the porosity of the protective film (unit: volume %). It should be noted that for pores that are too fine to be detected by the image analysis software (pores with a pore diameter of 20 nm or less), their area is regarded as 0.
[0073] <composition>
[0074] Since the present protective film contains yttrium oxyfluoride, it contains yttrium (Y), oxygen (O) and fluorine (F).
[0075] 《Y content》
[0076] The Y content of the present protective film is preferably 10 to 35 atomic %.
[0077] Here, the Y content of the present protective film is preferably 10 atomic % or more, more preferably 20 atomic % or more, further preferably 25 atomic % or more, particularly preferably 26 atomic % or more, and most preferably 27 atomic % or more.
[0078] On the other hand, the Y content of the present protective film is preferably 35 atomic % or less, more preferably 30 atomic % or less, further preferably 29 atomic % or less, and particularly preferably 28 atomic % or less.
[0079] 《O content》
[0080] The O content of the present protective film is preferably 10 to 35 atomic %.
[0081] Here, the O content of the present protective film is preferably 10 atomic % or more, more preferably 15 atomic % or more, further preferably 20 atomic % or more, particularly preferably 21 atomic % or more, and most preferably 22 atomic % or more.
[0082] On the other hand, the O content of the present protective film is preferably 35 atomic % or less, more preferably 30 atomic % or less, further preferably 25 atomic % or less, particularly preferably 24 atomic % or less, and most preferably 23.5 atomic % or less.
[0083] 《F content》
[0084] The F content of the present protective film is preferably 35 to 65 atomic %.
[0085] Here, the F content of the present protective film is preferably 35 atomic % or more, more preferably 40 atomic % or more, further preferably 44 atomic % or more, particularly preferably 47 atomic % or more, and most preferably 49.5 atomic % or more.
[0086] On the other hand, the F content of the protective film is preferably 65 atomic % or less, more preferably 60 atomic % or less, further preferably 55 atomic % or less, further preferably 52 atomic % or less, particularly preferably 51 atomic % or less, and most preferably 50 atomic % or less.
[0087] In order to make the content of each element into the above range, for example, the production conditions such as the amount of the evaporation source are appropriately adjusted in the method (the present production method) described later.
[0088] The contents of Y, O, and F in the protective film (unit: atomic %) were measured using an energy dispersive X-ray analyzer (EX-250SE, manufactured by Horiba, Ltd.).
[0089] <Orientation degree (half-peak width of rocking curve)>
[0090] When the protective film is enlarged in area, from the viewpoint of suppressing the generation of cracks in the protective film, the Y5 O 4 F 7 The higher the orientation degree of the (151) crystal plane (hereinafter, also referred to as "orientation degree"), the better.
[0091] As an index of orientation, Y 5 O 4 F 7 Specifically, the Y obtained using a two-dimensional detector is 5 O 4 F 7 The rocking curve of the peak of the (151) crystal plane is integrated in the 2θ direction, and the half-peak width is used to evaluate the orientation. It can be said that the smaller the half-peak width (unit: °), the higher the orientation degree.
[0092] Y 5 O 4 F 7 The half-value width of the rocking curve of the (151) crystal plane is preferably less than 40°, more preferably less than 30°, further preferably less than 25°, further preferably less than 20°, particularly preferably less than 15°, and most preferably less than 10°.
[0093] In order to adjust the degree of orientation to the above range, it is preferred to produce the protective film by the method described later (this production method).
[0094] 〈Crystalline size〉
[0095] As described above, for example, particles (grains) detached from a member exposed to plasma gas may adhere to a semiconductor substrate and become foreign matter that causes defects in a circuit.
[0096] At this time, the smaller the particle size, the more the generation of defects can be suppressed.
[0097] Therefore, the crystallite size of the present protective film is preferably 30 nm or less, more preferably 25 nm or less, further preferably 20 nm or less, particularly preferably 15 nm or less, and most preferably 10 nm or less.
[0098] On the other hand, the lower limit of the crystallite size of the present protective film is not particularly limited, and is, for example, 2 nm, preferably 5 nm. That is, the crystallite size of the present protective film is, for example, 2 to 30 nm.
[0099] In order to make the crystallite size within the above range, it is preferable to produce the protective film by the method described later (this production method).
[0100] The crystallite size in the protective film is determined by using the Scherrer equation based on data of an XRD pattern obtained by XRD measurement of the mirror-polished protective film.
[0101] <thickness>
[0102] The thickness of the protective film is preferably 0.3 μm or more, more preferably 1 μm or more, further preferably 5 μm or more, further preferably 10 μm or more, particularly preferably 15 μm or more, and most preferably 20 μm or more.
[0103] On the other hand, the upper limit of the thickness of the present protective film is not particularly limited, and is, for example, 300 μm, preferably 200 μm, more preferably 100 μm, further preferably 50 μm, and particularly preferably 30 μm. That is, the thickness of the present protective film is, for example, 0.3 to 300 μm.
[0104] The thickness of the protective film is measured as follows.
[0105] The cross section of the protective film was observed using a scanning electron microscope (SEM), the thickness of the protective film was measured at 5 arbitrary points, and the average value of the measured values at the 5 points was regarded as the thickness of the protective film (unit: μm).
[0106] 〈Thermal conductivity〉
[0107] The thermal conductivity of the protective film is preferably 5.0 W / (m·K) or more, more preferably 7.0 W / (m·K) or more, further preferably 9.0 W / (m·K) or more, particularly preferably 11.0 W / (m·K) or more, and most preferably 12.5 W / (m·K) or more.
[0108] The thermal conductivity of the protective film was determined at room temperature (23° C.) by a xenon lamp flash method using LFA 447 (Nanoflash) manufactured by NETZSCH.
[0109] Specifically, the bulk density of the substrate and the protective film was determined from the mass and volume, and the specific heat capacity of the substrate and the protective film was determined using the differential scanning calorimetry method specified in JIS R 1672: 2006. Furthermore, the thermal diffusivity of the substrate and the protective film was determined by applying the multilayer analysis mode to the temperature rise curve obtained by the flash method. The thermal conductivity was determined from the product of the bulk density, the specific heat capacity, and the thermal diffusivity.
[0110] [member]
[0111] Figure 1 1 is a schematic diagram showing an example of the member 6 .
[0112] The member 6 includes a substrate 5 and an yttrium protective film 4 .
[0113] like Figure 1 As shown, a base layer (base layer 1, base layer 2, and base layer 3) may be disposed between the substrate 5 and the yttrium protective film 4. However, the base layer is not limited to three layers.
[0114] The member of the present embodiment (hereinafter also referred to as “the present member”) has the above-mentioned present protective film as the yttrium protective film.
[0115] Since the surface of the present member is covered with the present protective film, the present member has excellent plasma resistance similar to the present protective film.
[0116] Hereinafter, each part included in this component will be described in detail.
[0117] 〈Base Material〉
[0118] The substrate has at least a surface on which the yttrium protective film (or the base layer described below) can be formed. Hereinafter, for convenience, this surface may be referred to as a "film-forming surface".
[0119] Materials
[0120] The material of the base material is appropriately selected depending on the purpose of the member and the like.
[0121] The substrate is composed of, for example, at least one selected from ceramics and metals.
[0122] Here, the ceramic is selected from glass (soda lime glass, etc.), quartz, alumina (Al 2 O 3 ), at least one of aluminum nitride (AlN) and aluminum oxynitride (AlON).
[0123] The metal is, for example, at least one selected from the group consisting of aluminum and an alloy containing aluminum.
[0124] "shape"
[0125] The shape of the substrate is not particularly limited, and examples thereof include a flat plate shape, a ring shape, a dome shape, a concave shape, or a convex shape, and the shape may be appropriately selected depending on the purpose of the member and the like.
[0126] 《Surface roughness of film-forming surface》
[0127] For reasons described below, the surface roughness of the film-forming surface of the substrate is preferably 0.6 μm or less, more preferably 0.3 μm or less, further preferably 0.1 μm or less, further preferably 0.05 μm or less, particularly preferably 0.01 μm or less, and most preferably 0.005 μm or less in terms of arithmetic mean roughness Ra.
[0128] The surface roughness (arithmetic mean roughness Ra) of the film-formed surface was measured in accordance with JIS B 0601:2001.
[0129] 《Film-forming surface area》
[0130] The area of the film-forming surface of the substrate is not particularly limited, but is, for example, 200 cm2 Above, preferably 2000cm 2 In addition, the upper limit of the area of the film-forming surface of the substrate is, for example, 10000 cm 2 , preferably 5000cm 2 .
[0131] 《Maximum length of film-forming surface》
[0132] The maximum length of the film-forming surface of the substrate is preferably 30 mm or more, more preferably 100 mm or more, further preferably 200 mm or more, further preferably 300 mm or more, particularly preferably 500 mm or more, very preferably 800 mm or more, and most preferably 1000 mm or more.
[0133] It should be noted that the “maximum length” refers to the maximum length of the film-forming surface. Specifically, for example, the film-forming surface is the diameter when it is a circle in plan view, the outer diameter when it is a ring in plan view, and the length of the maximum diagonal when it is a quadrilateral in plan view.
[0134] The upper limit of the maximum length of the film-forming surface is not particularly limited, and is, for example, 2000 mm, preferably 1500 mm. That is, the maximum length of the film-forming surface is, for example, 30 to 2000 mm.
[0135] Figure 2 This is a schematic diagram showing a half of the ring-shaped base material 5 cut away.
[0136] for Figure 2 The substrate 5 shown, for example, has an outer diameter D 1 100mm, inner diameter D 2 When the diameter is 90 mm and the thickness t is 5 mm, the maximum length is 100 mm.
[0137] The substrate 5 has a film-forming surface 7, which may also be Figure 2 Shown with a specified maximum length (outer diameter D 1 ) of the first film forming surface 7a and a second film forming surface 7b different from the first film forming surface 7a.
[0138] The ratio of the area of the second film-forming surface 7 b to the total area of the film-forming surface 7 is, for example, 60% or less.
[0139] Figure 3 It is a schematic diagram showing a part of the cross section of another annular base material 5 .
[0140] like Figure 3 As shown, the substrate 5 may have a plurality of second film forming surfaces 7 b.
[0141] Figure 4 1 is a schematic diagram showing a part of the cross section of still another annular base material 5 .
[0142] The angle between the first film forming surface 7a and the second film forming surface 7b is, for example, 20° to 120°. Figure 4 In the illustrated substrate 5 , the angle formed by the first film forming surface 7 a and the second film forming surface 7 b connected to the first film forming surface 7 a is approximately 30°.
[0143] 〈Basal layer〉
[0144] As described above, one or more underlayers may be disposed between the substrate and the yttrium protective film.
[0145] By forming the base layer, the stress of the yttrium protective film is relaxed, and the adhesion between the yttrium protective film and the substrate is improved.
[0146] The upper limit of the number of base layers is not particularly limited, but is preferably 5 layers or less, more preferably 4 layers or less, further preferably 3 layers or less, particularly preferably 2 layers or less, and most preferably 1 layer.
[0147] The base layer is preferably an amorphous film or a microcrystalline film.
[0148] The base layer preferably contains Al 2 O 3 、SiO 2 , Y 2 O 3 、MgO、ZrO 2 ,La 2 O 3 、Nd 2 O 3 , Yb 2 O 3 、Eu 2 O 3 and Gd 2 O 3 At least one oxide of
[0149] When two or more underlayers are disposed between the substrate and the yttrium protective film, it is preferred that the oxides of the underlayers are different from each other between adjacent underlayers.
[0150] In the case where the oxides of the adjacent base layers are different from each other, specifically, for example, the oxide of the base layer 1 is "SiO 2 ", the oxide of the base layer 2 is "Al 2 O 3 +SiO 2 ", the oxide of the base layer 3 is "Al 2 O 3 " situation.
[0151] The thickness of each base layer is preferably 0.1 μm or more, more preferably 0.4 μm or more, and further preferably 0.8 μm or more.
[0152] On the other hand, the thickness of the base layer is, for example, 15 μm or less, preferably 10 μm or less, more preferably 7 μm or less, and further preferably 3 μm or less. That is, the thickness of the base layer is, for example, 0.1 to 15 μm.
[0153] The thickness of the base layer is measured in the same manner as the thickness of the yttrium protective film.
[0154] 〈Purpose of Components〉
[0155] This member is used as a member such as a top plate inside a semiconductor device manufacturing apparatus (plasma etching apparatus, plasma CVD apparatus, etc.), for example.
[0156] However, the use of this component is not limited to this.
[0157] [Yttrium protective film and method for manufacturing a component]
[0158] Next, a method for producing the yttrium protective film of the present embodiment (hereinafter also referred to as "the present production method") will be described. The present production method is also a method for producing the present member described above.
[0159] This production method is a so-called ion-assisted deposition (IAD) method.
[0160] In general, in a vacuum, while irradiating ions, the evaporation source (Y 2 O 3 and YF 3 ) evaporates and adheres to the substrate, thereby forming Y 5 O 4 F 7 Yttrium protective film with a higher proportion.
[0161] According to the present manufacturing method, the yttrium protective film can be formed very densely. That is, the obtained yttrium protective film has a small porosity and a small crystallite size.
[0162] However, the yttrium protective film is more susceptible to cracks as its thickness increases.
[0163] In addition, the yttrium protective film formed on the film-forming surface is also enlarged by increasing the film-forming surface area. In this case, cracks are easily introduced into the yttrium protective film.
[0164] However, according to the present production method, a dense and hard yttrium protective film can be obtained.
[0165] Furthermore, when the base layer is formed, the stress of the yttrium protective film is relaxed.
[0166] Therefore, the yttrium protective film obtained by the present production method is unlikely to be cracked even if the thickness and area are increased.
[0167] The surface roughness (arithmetic mean roughness Ra) of the film-forming surface of the substrate is preferably within the above range. This makes the formed yttrium protective film denser and harder, and less likely to crack.
[0168] It should be noted that in methods such as thermal spraying and aerosol deposition (AD), the yttrium protective film obtained is likely to have many pores remaining.
[0169] Furthermore, in these methods, it is difficult to control the fluorine content of the obtained yttrium protective film, and it is sometimes difficult to stably obtain a desired composition.
[0170] In addition, as a method different from the IAD method, there is a sputtering method. In the sputtering method, for example, plasma of argon and oxygen is mixed with YO in a vacuum. x F y The sputtering target collides with the substrate to form a film.
[0171] However, in this method, the fluorine content is easily changed, and it is still difficult to stably form Y with a rhombohedral crystal structure. 5 O 4 F 7 Yttrium protective film with a higher proportion.
[0172] <Device Configuration>
[0173] based on Figure 5 This production method will be described in more detail.
[0174] Figure 5 This is a schematic diagram showing an apparatus used for producing the yttrium protective film.
[0175] Figure 5 The device shown has a chamber 11. The interior of the chamber 11 can be evacuated to a vacuum by driving a vacuum pump (not shown).
[0176] Crucibles 12 and 13 and an ion gun 14 are arranged inside the chamber 11 , and a support 17 is arranged above them.
[0177] The holder 17 is integrated with the support shaft 16, and rotates with the rotation of the support shaft 16. The heater 15 is arranged around the holder 17.
[0178] The substrate 5 is held by the holder 17 in a state where the film-forming surface thereof faces downward. The substrate 5 held by the holder 17 is rotated as the holder 17 rotates while being heated by the heater 15 .
[0179] Furthermore, a crystal film thickness monitor 18 and a crystal film thickness monitor 19 are installed in the chamber 11 .
[0180] 〈Formation of yttrium protective film〉
[0181] exist Figure 5 In the device shown in FIG. 1 , a yttrium protective film (on the substrate 5) is formed. Figure 5 The situation (not shown in the figure) is explained.
[0182] First, the evaporation source Y is filled into the crucible 12 on one side. 2 O 3 , fill the other crucible 13 with the evaporation source YF 3 .
[0183] After the substrate 5 is held on the holder 17, the interior of the chamber 11 is evacuated to a vacuum. Specifically, the pressure inside the chamber 11 is preferably 8×10 -2 Below Pa.
[0184] Next, the holder 17 is rotated while the heater 15 is driven. Thus, the substrate 5 is rotated while being heated.
[0185] In this state, ion-assisted vapor deposition is performed to form a film on the substrate 5 .
[0186] That is, while ion gun 14 irradiates ions (ion beam), evaporation source Y of crucible 12 is 2 O 3 The evaporation source YF of the crucible 13 3 The evaporation was carried out in parallel.
[0187] The ions irradiated by the ion gun 14 are preferably ions of at least one element selected from the group consisting of oxygen, argon, neon, krypton, and xenon.
[0188] The evaporation source is irradiated with an electron beam (not shown) to melt and evaporate.
[0189] Then, the evaporated evaporation source adheres to the film formation surface of the substrate 5 to form a yttrium protective film.
[0190] Pressure in the chamber
[0191] The film formation is performed in a vacuum. Specifically, the pressure inside the chamber 11 is preferably 8×10 -2 Pa or less, more preferably 6×10 -2 Pa or less, more preferably 5×10 -2 Pa or less, particularly preferably 3×10 -2 Below Pa.
[0192] The lower limit is preferably 0.5×10 -2That is, the pressure inside the chamber 11 is preferably 0.5×10 -2 Pa~8×10 - 2 Pa.
[0193] Temperature of the substrate
[0194] During film formation, the temperature of the substrate 5 heated by the heater 15 is preferably 200°C or higher, more preferably 250°C or higher. On the other hand, it is preferably 400°C or lower, more preferably 350°C or lower. That is, the temperature of the substrate 5 is preferably 200 to 400°C.
[0195] Film forming speed
[0196] The speed (film formation speed) at which the evaporation source in the crucible 12 evaporates to form a film is monitored in advance using the crystal film thickness monitor 18 .
[0197] In addition, the speed (film formation speed) at which the evaporation source in the crucible 13 evaporates to form a film is monitored in advance using a crystal film thickness monitor 19 .
[0198] The film formation rate is adjusted by controlling the conditions of the electron beam irradiated on the evaporation source and the conditions of the ion beam of the ion gun 14 (current value, current density, etc.).
[0199] In forming the yttrium protective film, the film formation rate (unit: nm / min) of each evaporation source is adjusted to a desired value.
[0200] Evaporation source Y 2 O 3 The film forming speed (unit: nm / min) and the evaporation source YF 3 The film forming rate (unit: nm / min) is the film forming rate ratio (Y 2 O 3 / YF 3 ) is preferably 1 / 9.5 to 1 / 1.1.
[0201] Here, the film forming speed ratio (Y 2 O 3 / YF 3 ) is preferably 1 / 9.5 or more, more preferably 1 / 8.0 or more, further preferably 1 / 6.0 or more, and particularly preferably 1 / 4.5 or more.
[0202] On the other hand, the film forming speed ratio (Y 2 O 3 / YF 3 ) is preferably 1 / 1.1 or less, more preferably 1 / 1.3 or less, further preferably 1 / 1.8 or less, and particularly preferably 1 / 2.5 or less.
[0203] Evaporation source Y 2 O 3 The film forming speed and evaporation source YF 3 The total film-forming rate is preferably 5 to 50 nm / min.
[0204] Here, the total speed is preferably 5 nm / min or more, more preferably 8 nm / min or more, and further preferably 10 nm / min or more. On the other hand, the total speed is preferably 50 nm / min or less, more preferably 35 nm / min or less, and further preferably 20 nm / min or less.
[0205] 《Conditions of ion irradiation》
[0206] The distance between the ion gun 14 and the substrate 5 is preferably 700 to 1500 mm.
[0207] Here, the distance between the ion gun 14 and the substrate 5 is preferably 700 mm or more, more preferably 900 mm or more. On the other hand, the distance is preferably 1500 mm or less, more preferably 1300 mm or less.
[0208] The current value of the ion beam is preferably 1000 to 3000 mA.
[0209] Here, the ion beam current value is preferably 1000 mA or more, and more preferably 1500 mA or more.
[0210] On the other hand, the ion beam current value is preferably 3000 mA or less, and more preferably 2500 mA or less.
[0211] The ion beam current density is preferably 40 to 140 μA / cm 2 .
[0212] Here, the ion beam current value is preferably 40 μA / cm 2 More preferably, 65 μA / cm 2 More preferably, 75 μA / cm 2 Above, particularly preferably 85 μA / cm 2 above.
[0213] On the other hand, the ion beam current density is preferably 140 μA / cm 2 Below, more preferably 120μA / cm 2 the following.
[0214] 〈Formation of the basal layer〉
[0215] It is preferable to form the above-mentioned underlayer (for example, underlayer 1 , underlayer 2 , and underlayer 3 ) on the film formation surface of the substrate 5 before forming the yttrium protective film.
[0216] The base layer is formed by ion-assisted vapor deposition in the same manner as the yttrium protective film.
[0217] For example, the formation of Al 2 O 3 In the case of a base layer composed of Al, the crucible 12 and / or the crucible 13 is filled with Al 2 O 3 As the evaporation source, while irradiating ions (ion beam) from the ion gun 14 , the evaporation source is evaporated and attached to the film formation surface of the substrate 5 .
[0218] The conditions for forming the base layer are the same as those for forming the yttrium protective film.
[0219] Example
[0220] Hereinafter, the present invention will be specifically described with reference to Examples. However, the present invention is not limited to the Examples described below.
[0221] Hereinafter, Examples 1 to 20 are working examples, Examples 21 to 27 are comparative examples, and Examples 28 to 30 are reference examples.
[0222] 〈Example 1~Example 27〉
[0223] Use based Figure 5 The described device is used to manufacture the yttrium protective film (protective film).
[0224] More specifically, under the production conditions shown in Tables 1 to 3 below, the base layer and the protective film shown in Tables 1 to 3 below were formed on the film formation surface of the substrate.
[0225] As the substrate, a circular substrate (thickness: 10 mm) having a film-forming surface with a diameter (maximum length) of 200 mm was used. The composition of the protective film was determined from the content of each element (Y, O, F, etc.).
[0226] As manufacturing conditions not described in the following Tables 1 to 3, oxygen (O) ions were irradiated from an ion gun, the distance between the ion gun and the substrate was 1100 mm, and the current value of the ion beam was 2000 mA.
[0227] In Example 12, commercially available soda-lime glass was used as the substrate (glass).
[0228] In Example 14, one side of an aluminum substrate was treated with an aluminum oxide film (Alumite) to produce an Al 2 O 3 This base layer is described as "aluminum oxide film" in the following Table 2.
[0229] 〈Example 28~Example 30〉
[0230] In Example 28, sapphire is used as the protective film.
[0231] In Example 29, metallic aluminum was used as the protective film.
[0232] In Example 30, quartz was used as the protective film.
[0233] The thickness, Vickers hardness, and presence of cracks of the protective films of Examples 28 to 30 were not evaluated.
[0234] 〈Etching amount〉
[0235] The etching amount of the protective film of each example was determined to evaluate the plasma resistance.
[0236] Specifically, the 10 mm × 5 mm surface of the protective film was mirror-finished. Kapton tape was attached to a portion of the mirror-finished surface for masking, and etching was performed using plasma gas. Then, a stylus-type surface profile measuring instrument (manufactured by ULVAC, Dectak150) was used to measure the height difference between the etched portion and the non-etched portion, thereby determining the etching amount.
[0237] As a plasma etching apparatus, EXAM (manufactured by Shinko Seiki Co., Ltd., model: POEM) was used. In RIE mode (reactive ion etching mode), first, a pressure of 10 Pa and an output of 350 W were used to etch the plasma. 4 The gas (flow rate: 100 sccm) was mixed with O 2 The etching was performed for 180 minutes using a gas (flow rate: 10 sccm). 4 Gas (flow rate: 100 sccm) was used for etching for 180 minutes. 4 The gas (flow rate: 100 sccm) was mixed with O 2 The etching was carried out for 180 minutes using a gas (flow rate: 10 sccm). Finally, CF 4 Gas (flow rate: 100 sccm) was used to perform etching for 180 minutes.
[0238] The smaller the etching amount (unit: nm), the better the plasma resistance can be evaluated.
[0239] Specifically, when the etching amount is 200 nm or less, it is evaluated that the plasma resistance is excellent.
[0240] 〈F content change〉
[0241] After etching, the F content of the protective film was measured, and the amount of change in the F content (unit: atomic %) was determined based on the following formula.
[0242] F content change = {(F content before etching) - (F content after etching)} / (F content before etching)
[0243] The smaller the value of the F content change, the better the plasma resistance and the more stable the protective film can be evaluated. Specifically, the F content change is preferably 10 atomic % or less, more preferably 5 atomic % or less, and further preferably 3 atomic % or less.
[0244] 〈Presence or absence of cracks〉
[0245] After the protective film was formed, it was confirmed whether cracks visible to the naked eye appeared on the protective film. In the following Tables 1 to 3, the case where no cracks appeared was recorded as "no", and the case where cracks appeared was recorded as "yes".
[0246] [Table 1]
[0247]
[0248] [Table 2]
[0249]
[0250] [Table 3]
[0251]
[0252] 〈Summary of evaluation results〉
[0253] As shown in Tables 1 to 3, it is found that the yttrium protective films of Examples 1 to 20 are excellent in plasma resistance. On the other hand, the yttrium protective films of Examples 21 to 27 are insufficient in plasma resistance.
[0254] Above, the embodiments of the present invention have been described, but the embodiments are not limited by the contents of the embodiments. In addition, the above-mentioned constituent elements include elements that can be easily assumed by those skilled in the art, substantially the same elements, and elements of so-called equivalent scopes. Furthermore, the above-mentioned constituent elements can be appropriately combined. In addition, various omissions, substitutions or changes of constituent elements can be performed within the scope of the gist of the above-mentioned embodiments.
[0255] This application is based on the Japanese patent application (Japanese Patent Application No. 2022-024103) filed on February 18, 2022, the contents of which are incorporated herein by reference.
[0256] Explanation of symbols
[0257] 1, 2, 3: Basal layer
[0258] 4: Yttrium protective film
[0259] 5: Base material
[0260] 6: Components
[0261] 7: Film-forming surface
[0262] 7a: First film-forming surface
[0263] 7b: Second film-forming surface
[0264] 11: Chamber
[0265] 12, 13: Crucible
[0266] 14: Ion Gun
[0267] 15: Heater
[0268] 16: Support shaft
[0269] 17: Bracket
[0270] 18, 19: Crystal film thickness monitor
Claims
1. An yttrium protective film, wherein the peak intensity ratio of Y5O4F7 in the X-ray diffraction spectrum is 80% or more, Porosity less than 1.5% by volume, The Vickers hardness is 500 MPa or more.
2. The yttrium protective film according to claim 1, wherein: The fluorine content is 35 to 60 atomic %.
3. The yttrium protective film according to claim 1 or 2, wherein: The crystallite size is less than 30 nm.
4. The yttrium protective film according to any one of claims 1 to 3, wherein The thickness is 0.3 μm or more.
5. The yttrium protective film according to any one of claims 1 to 4, wherein The half-value width of the rocking curve of the (151) crystal plane of Y5O4F7 is less than 40°. 6 . A member comprising a substrate and the yttrium protective film according to claim 1 , which is disposed on a film-forming surface which is a surface of the substrate.
7. The component according to claim 6, wherein The substrate is composed of at least one selected from ceramics and metals, The ceramic is at least one selected from glass, quartz, aluminum oxide, aluminum nitride and aluminum oxynitride, The metal is at least one selected from the group consisting of aluminum and an alloy containing aluminum.
8. A component according to claim 6 or 7, wherein: The surface roughness of the film-forming surface is 0.6 μm or less in terms of arithmetic mean roughness Ra.
9. The member according to any one of claims 6 to 8, wherein The maximum length of the film-forming surface is greater than 30 mm.
10. The member according to any one of claims 6 to 9, wherein There is one or more base layers between the substrate and the yttrium protective film, The base layer contains at least one oxide selected from Al2O3, SiO2, Y2O3, MgO, ZrO2, La2O3, Nd2O3, Yb2O3, Eu2O3 and Gd2O3.
11. The component according to claim 10, wherein There are two or more base layers between the substrate and the yttrium protective film, The oxide is different from each other in adjacent base layers.
12. The member according to any one of claims 6 to 11, wherein The substrate has a first film-forming surface with a predetermined maximum length and a second film-forming surface different from the first film-forming surface as the film-forming surface, The angle between the first film forming surface and the second film forming surface is 20° to 120°, A ratio of the area of the second film-forming surface to the total area of the film-forming surface is 60% or less. 13 . The member according to claim 6 , which is used inside a plasma etching device or a plasma CVD device.
14. A method for producing a yttrium protective film, the method being a method for producing the yttrium protective film according to any one of claims 1 to 5, In a vacuum, while irradiating with ions of at least one element selected from oxygen, argon, neon, krypton and xenon, an evaporation source is evaporated and attached to the substrate. Y2O3 and YF3 were used as the evaporation sources.
Citation Information
Patent Citations
Sintered body
CN107074663A
Method for forming yttrium oxide fluoride coating film and yttrium oxide fluoride coating film prepared thereby
CN110800082A
Yttrium based fluoride thermal spray coating, thermal spray material for forming the same, method for forming thermal spray coating and corrosion-resistant coating including thermal spray coating
JP2019019413A
Film-attached member and method for producing the same
JP2019147995A
Yttrium fluoride sprayed coating, spray material therefor, and corrosion resistant coating including sprayed coating
US20170292182A1