Substrate processing method, method of manufacturing semiconductor device, substrate processing apparatus, and recording medium

By continuously supplying a gas combination of specific elements to the substrate, the problem of low film formation rate is solved, the film formation efficiency is increased, and the quality and resistance characteristics of the film are improved.

CN118726940APending Publication Date: 2024-10-01KOKUSAI DENKI KK
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202410141206.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2023-03-31
Filing Date
2024-01-31
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

In the process of forming a film, the film formation speed (film formation rate) is low, which affects the manufacturing efficiency of semiconductor devices.

Method used

By continuously supplying a combination of gases containing specific elements to the substrate, including a gas containing a first element and a halogen element, a gas of a second element different from the first element, a gas of a third element with reducing properties, and a gas with reducing properties. For the gas of the fourth element, make a timing plan for gas supply to increase the film formation rate.

Benefits of technology

The film formation rate is significantly increased, the generation and adsorption of by-products are reduced, and the quality and resistance characteristics of the film are improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118726940A_ABST
    Figure CN118726940A_ABST
Patent Text Reader

Abstract

The invention relates to a substrate processing method, a method of manufacturing a semiconductor device, a substrate processing apparatus, and a recording medium. Provided is a technique capable of improving the film formation rate. Comprising the following steps: (a) supplying a first gas containing a first element and a halogen element to a substrate; (b) a step in which a second gas containing a second element different from the first element is supplied to the substrate; (c) supplying a third gas containing a third element and having reducibility to the substrate; and (d) a step for forming a film containing the first element and the second element on the substrate by continuously performing (a) and (d) and performing (b) and (c) for a predetermined number of times in a manner in which (a) and (d) are continuously performed and (b) and (c) are continuously performed.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a substrate processing method, a method for manufacturing a semiconductor device, a substrate processing apparatus and a recording medium. Background Art

[0002] One of the manufacturing processes of a semiconductor device is a process of forming a film on the surface of a substrate (see, for example, Patent Document 1).

[0003] Prior art literature

[0004] Patent Literature

[0005] Patent Document 1: International Publication No. 2019 / 058608 Summary of the invention

[0006] Problems to be solved by the invention

[0007] In the process of forming a film, the film forming speed (film forming rate) may be reduced.

[0008] The present invention provides a technique capable of increasing the film forming rate.

[0009] Means for solving problems

[0010] According to one embodiment of the present invention, a technique is provided in which

[0011] (a) a step of supplying a first gas containing a first element and a halogen element to a substrate;

[0012] (b) supplying a second gas containing a second element different from the first element to the substrate;

[0013] (c) supplying a third gas containing a third element and having reducing properties to the substrate; and

[0014] (d) Step of supplying a fourth gas containing a fourth element and having reducing properties

[0015] (a) and (d) are performed continuously, and (b) and (c) are performed continuously a predetermined number of times, thereby forming a film including the first element and the second element on the substrate.

[0016] Effects of the Invention

[0017] According to the present invention, the film forming rate can be increased. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] [ Figure 1 ] Figure 1 It is a longitudinal sectional view schematically showing a substrate processing apparatus in an embodiment.

[0019] [ Figure 2 ] Figure 2 for Figure 1 AA line schematic cross-sectional view.

[0020] [ Figure 3 ] Figure 3 It is a schematic configuration diagram of a controller of a substrate processing apparatus in an embodiment, and is a diagram showing a control system of the controller in the form of a block diagram.

[0021] [ Figure 4 ] Figure 4 (A) is a diagram showing the timing of gas supply in an embodiment;

[0022] Figure 4 (B) is a diagram showing the timing of gas supply in Modification 1 of the embodiment;

[0023] Figure 4 (C) in FIG. 1 is a diagram showing the timing of gas supply in Modification 2 of the embodiment.

[0024] [ Figure 5 ] Figure 5 (A) is a diagram showing the timing of gas supply in Comparative Example 1 of the Experimental Example; Figure 5 (B) is a diagram showing the timing of gas supply in Comparative Example 2 of the Experimental Example; Figure 5 (C) in FIG. 1 is a diagram showing the timing of gas supply in Comparative Example 3 of the Experimental Example.

[0025] [ Figure 6 ] Figure 6 To illustrate the addition to Figure 1 A schematic diagram of parts of a substrate processing apparatus and its surroundings.

[0026] [ Figure 7 ] Figure 7 This is a diagram showing the results of XRD measurement in the experimental example.

[0027] Description of Reference Numerals

[0028] 10 Substrate processing device

[0029] 121 Controller

[0030] 200 wafers (substrate)

[0031] Processing Room 201 DETAILED DESCRIPTION

[0032] <Implementation Method>

[0033] Below, refer to Figures 1 to 3 , Figure 4 (A) Figure 6One embodiment of the present invention is described. The drawings used in the following description are schematic drawings, and the relationship between the dimensions of the elements and the ratio of the elements shown in the drawings may not be consistent with the actual situation. In addition, the relationship between the dimensions of the elements and the ratio of the elements may not be consistent between multiple drawings.

[0034] (1) Configuration of substrate processing apparatus

[0035] The substrate processing apparatus 10 includes a processing furnace 202 provided with a heater 207 as a heating means (heating mechanism, heating system). The heater 207 has a cylindrical shape and is vertically mounted by being supported by a heater base (not shown) as a holding plate.

[0036] On the inner side of the heater 207, an outer tube 203 constituting a reaction vessel (processing vessel) is arranged concentrically with the heater 207. The outer tube 203 is formed of a heat-resistant material such as quartz (SiO2) and silicon carbide (SiC), and is formed into a cylindrical shape with a closed upper end and an open lower end. Below the outer tube 203, a manifold (inlet flange) 209 is arranged concentrically with the outer tube 203. The manifold 209 is formed of a metal such as stainless steel (SUS), and is formed into a cylindrical shape with an upper end and a lower end open. An O-ring 220a as a sealing member is provided between the upper end of the manifold 209 and the outer tube 203. The manifold 209 is supported on the heater base, so that the outer tube 203 is in a vertically mounted state.

[0037] An inner tube 204 constituting a reaction vessel is disposed inside the outer tube 203. The inner tube 204 is formed of a heat-resistant material such as quartz or SiC, and is formed into a cylindrical shape with a closed upper end and an open lower end. The outer tube 203, the inner tube 204, and the manifold 209 mainly constitute a processing vessel (reaction vessel). A processing chamber 201 is formed in the hollow portion of the processing vessel (inside the inner tube 204).

[0038] The processing chamber 201 is configured to accommodate wafers 200 as substrates arranged in multiple layers in a horizontal posture in the vertical direction using a wafer boat 217 described later. In the processing chamber 201, nozzles 410, 420, and 430 are provided in a manner penetrating the side wall of the manifold 209 and the inner tube 204. Gas supply pipes 310, 320, and 330 are connected to the nozzles 410, 420, and 430, respectively.

[0039] The gas supply pipes 310, 320, 330 are provided with mass flow controllers (MFCs) 312, 322, 332 as flow controllers (flow control units) in order from the upstream side. In addition, the gas supply pipes 310, 320, 330 are provided with valves 314, 324, 334 as opening and closing valves. The gas supply pipes 510, 520, 530 for supplying inert gas are connected to the downstream side of the valves 314, 324, 334 of the gas supply pipes 310, 320, 330, respectively. The gas supply pipes 510, 520, 530 are provided with MFCs 512, 522, 532 as flow controllers (flow control units) and valves 514, 524, 534 as opening and closing valves in order from the upstream side.

[0040] Nozzles 410, 420, 430 are connected to the front ends of the gas supply pipes 310, 320, 330, respectively. The nozzles 410, 420, 430 are configured as L-shaped nozzles, and the horizontal portions thereof are provided so as to penetrate the side wall of the manifold 209 and the inner tube 204. The vertical portions of the nozzles 410, 420, 430 are provided inside the preliminary chamber 201a which is formed in a channel shape (groove shape) so as to protrude radially outward from the inner tube 204 and extend in the vertical direction, and are provided upward (above the arrangement direction of the wafers 200) along the inner wall of the inner tube 204 in the preliminary chamber 201a.

[0041] The nozzles 410, 420, 430 are arranged in a manner extending from the lower region of the processing chamber 201 to the upper region of the processing chamber 201, and a plurality of gas supply holes 410a, 420a, 430a are respectively provided at positions opposite to the wafer 200. Thus, the processing gas is respectively supplied to the wafer 200 from the gas supply holes 410a, 420a, 430a of the nozzles 410, 420, 430. The gas supply holes 410a, 420a, 430a are provided in plurality in the range from the lower part to the upper part of the inner tube 204, each having the same opening area and being arranged at the same opening pitch. However, the gas supply holes 410a, 420a, 430a are not limited to the above-mentioned manner. For example, the opening area may be gradually increased from the lower part to the upper part of the inner tube 204. Thus, the flow rate of the gas supplied from the gas supply holes 410a, 420a, 430a can be made more uniform.

[0042] The gas supply holes 410a, 420a, 430a of the nozzles 410, 420, 430 are provided in a plurality of height positions from the lower part to the upper part of the wafer boat 217 described later. Therefore, the processing gas supplied from the gas supply holes 410a, 420a, 430a of the nozzles 410, 420, 430 to the processing chamber 201 is supplied to the entire area of ​​the wafers 200 accommodated in the wafer boat 217 from the lower part to the upper part. The nozzles 410, 420, 430 may be provided in a manner extending from the lower area to the upper area of ​​the processing chamber 201, and are preferably provided in a manner extending to the vicinity of the top plate of the wafer boat 217.

[0043] A first gas (raw material gas, halogen-containing gas) containing a first element and a halogen element is supplied as a processing gas from a gas supply pipe 310 into the processing chamber 201 via the MFC 312, the valve 314, and the nozzle 410. As the first gas, for example, a gas containing a metal element as the first element and a halogen element (halogen-containing metal gas) can be used.

[0044] A third gas having reducing properties and containing a third element is supplied as a processing gas from the gas supply pipe 320 through the MFC 322 , the valve 324 , and the nozzle 420 into the processing chamber 201 .

[0045] like Figure 6 As shown, in Figure 1 A gas supply pipe 340 for supplying a fourth gas is provided downstream of a valve 324 of a gas supply pipe 320 of a substrate processing apparatus. Figure 6 Other elements of Figure 1 The substrate processing apparatus shown in the figure is similarly constructed and Figure 1 Elements substantially the same as those described in the above are given the same reference numerals, and their description is omitted. The gas supply pipe 340 is provided with an MFC 342 as a flow controller and a valve 344 as an on-off valve in order from the upstream side.

[0046] The fourth gas containing the fourth element having reducing properties is supplied as the processing gas from the gas supply pipe 340 via the MFC 342, the valve 344, the gas supply pipe 320 and the nozzle 420 into the processing chamber 201. Here, for reasons described below, it is preferable that the third gas has a higher decomposition temperature than the fourth gas.

[0047] A second gas (reaction gas) containing a second element different from the first element is supplied as a processing gas from the gas supply pipe 330 into the processing chamber 201 via the MFC 332 , the valve 334 , and the nozzle 430 .

[0048] Nitrogen (N2) gas is supplied as an inert gas from gas supply pipes 510, 520, 530 into the processing chamber 201 via MFCs 512, 522, 532, valves 514, 524, 534, and nozzles 410, 420, 430, respectively. Hereinafter, an example in which N2 gas is used as the inert gas will be described, but as the inert gas, for example, argon (Ar) gas, helium (He) gas, neon (Ne) gas, xenon (Xe) gas, or other rare gases may be used in addition to N2 gas.

[0049] The processing gas supply system is mainly composed of gas supply pipes 310, 320, 330, MFCs 312, 322, 332, valves 314, 324, 334, and nozzles 410, 420, 430, but only nozzles 410, 420, 430 may be regarded as the processing gas supply system. The processing gas supply system may also be referred to as the gas supply system. In addition, the inactive gas supply system is mainly composed of gas supply pipes 510, 520, 530, MFCs 512, 522, 532, and valves 514, 524, 534.

[0050] When the first gas flows in from the gas supply pipe 310, the first gas supply system is mainly composed of the gas supply pipe 310, the MFC 312, and the valve 314. Here, it is also possible to consider that the nozzle 410 is included in the first gas supply system. In addition, when the third gas flows in from the gas supply pipe 320, the third gas supply system is mainly composed of the gas supply pipe 320, the MFC 322, and the valve 324. Here, it is also possible to consider that the nozzle 420 is included in the third gas supply system. In addition, when the second gas flows in from the gas supply pipe 330, the second gas supply system is mainly composed of the gas supply pipe 330, the MFC 332, and the valve 334. Here, it is also possible to consider that the nozzle 430 is included in the second gas supply system. In addition, the gas supply pipe 340, MFC342, and valve 344 are included in the gas supply pipes 310, 320, 330, MFC312, 322, 332, valves 314, 324, 334, and nozzles 410, 420, and 430 to form a processing gas supply system. The fourth gas supply system is mainly composed of the gas supply pipe 340, MFC342, valve 344, and gas supply pipe 320. Here, it is also considered that the nozzle 420 is included in the fourth gas supply system.

[0051] In the gas supply method of this embodiment, the gas is transported through the nozzles 410, 420, and 430 arranged in the preparatory chamber 201a in the annular long space defined by the inner wall of the inner tube 204 and the ends of the plurality of wafers 200. Then, the gas is ejected into the inner tube 204 from the plurality of gas supply holes 410a, 420a, and 430a provided at the positions of the nozzles 410, 420, and 430 facing the wafers. More specifically, the first gas and the like are ejected in a direction parallel to the surface of the wafer 200 by the gas supply holes 410a of the nozzle 410, the gas supply holes 420a of the nozzle 420, and the gas supply holes 430a of the nozzle 430.

[0052] The exhaust hole (exhaust port) 204a is a through hole formed in the side wall of the inner tube 204 at a position opposite to the nozzles 410, 420, 430, and is, for example, a slit-shaped through hole opened in a vertical direction. The gas supplied from the gas supply holes 410a, 420a, 430a of the nozzles 410, 420, 430 into the processing chamber 201 and flowing on the surface of the wafer 200 flows into the exhaust passage 206 formed by the gap formed between the inner tube 204 and the outer tube 203 through the exhaust hole 204a. In addition, the gas flowing into the exhaust passage 206 flows into the exhaust pipe 231 and is exhausted to the outside of the processing furnace 202.

[0053] The exhaust hole 204a is provided at a position opposite to the plurality of wafers 200. The gas supplied from the gas supply holes 410a, 420a, and 430a to the vicinity of the wafers 200 in the processing chamber 201 flows in a horizontal direction and then flows into the exhaust passage 206 through the exhaust hole 204a. The exhaust hole 204a is not limited to being a slit-shaped through hole, but may be composed of a plurality of holes.

[0054] The manifold 209 is provided with an exhaust pipe 231 for exhausting the atmosphere in the processing chamber 201. The exhaust pipe 231 is connected to a pressure sensor 245 as a pressure detector (pressure detection unit) for detecting the pressure in the processing chamber 201, an APC (Auto Pressure Controller) valve 243, and a vacuum pump 246 as a vacuum exhaust device in sequence from the upstream side. The APC valve 243 can perform vacuum exhaust and stop vacuum exhaust in the processing chamber 201 by opening and closing the valve while the vacuum pump 246 is in operation. In addition, the pressure in the processing chamber 201 can be adjusted by adjusting the valve opening while the vacuum pump 246 is in operation. The exhaust system is mainly composed of the exhaust hole 204a, the exhaust passage 206, the exhaust pipe 231, the APC valve 243 and the pressure sensor 245. It is also conceivable to include the vacuum pump 246 in the exhaust system.

[0055] Below the manifold 209, there is provided a sealing cover 219 as a furnace port cover body capable of hermetically closing the lower end opening of the manifold 209. The sealing cover 219 is configured to abut against the lower end of the manifold 209 from the lower side in the vertical direction. The sealing cover 219 is formed of a metal such as SUS and is formed in a disc shape. On the upper surface of the sealing cover 219, there is provided an O-ring 220b as a sealing member abutting against the lower end of the manifold 209. On the opposite side of the processing chamber 201 in the sealing cover 219, there is provided a rotating mechanism 267 for rotating the wafer boat 217 accommodating the wafer 200. The rotating shaft 255 of the rotating mechanism 267 penetrates the sealing cover 219 and is connected to the wafer boat 217. The rotating mechanism 267 is configured to rotate the wafer 200 by rotating the wafer boat 217. The sealing cover 219 is configured to be raised and lowered in the vertical direction by a boat elevator 115 as an elevating mechanism vertically provided outside the outer tube 203. The boat elevator 115 is configured to be able to move the boat 217 into and out of the processing chamber 201 by raising and lowering the sealing cover 219. The boat elevator 115 is configured as a transport device (transport mechanism) that transports the boat 217 and the wafers 200 accommodated in the boat 217 into and out of the processing chamber 201.

[0056] The wafer boat 217 as a substrate support is configured to arrange a plurality of wafers 200, for example, 25 to 200 wafers 200, in a horizontal posture and with their centers aligned with each other, at intervals in the vertical direction. Here, the expression of a numerical range such as "25 to 200 wafers" in this specification means that the lower limit and the upper limit are included in the range. Therefore, for example, the so-called "25 to 200 wafers" means "more than 25 wafers and less than 200 wafers". The same is true for other numerical ranges.

[0057] The wafer boat 217 is made of a heat-resistant material such as quartz or SiC. A heat-insulating plate 218 made of a heat-resistant material such as quartz or SiC is supported in a horizontal posture and in multiple layers (not shown) at the bottom of the wafer boat 217 .

[0058] like Figure 2 As shown in FIG. 1 , a temperature sensor 263 as a temperature detector is provided in the inner tube 204, and the amount of current supplied to the heater 207 is adjusted based on the temperature information detected by the temperature sensor 263, so that the temperature in the processing chamber 201 becomes a desired temperature distribution. The temperature sensor 263 is configured in an L shape similarly to the nozzles 410, 420, and 430, and is provided along the inner wall of the inner tube 204.

[0059] like Figure 3As shown, the controller 121 as a control unit (control unit) is configured in the form of a computer having a CPU (Central Processing Unit) 121a, a RAM (Random Access Memory) 121b, a storage device 121c, and an I / O port 121d. The RAM 121b, the storage device 121c, and the I / O port 121d are configured so as to be able to exchange data with the CPU 121a via an internal bus. An input / output device 122 such as a touch panel is connected to the controller 121. In addition, the controller 121 can be configured to connect an external storage device (for example, a magnetic disk such as a magnetic tape, a floppy disk, a hard disk, an optical disk such as a CD, a DVD, an optical magnetic disk such as an MO, a USB memory, a semiconductor memory such as a memory card) 123.

[0060] Here, the substrate processing apparatus may be configured to include one control unit or multiple control units. That is, one control unit may be used to perform control for performing the substrate processing process described later, or multiple control units may be used to perform control for performing the substrate processing process described later. In addition, multiple control units may be configured as a control system interconnected by a wired or wireless communication network, or the control system as a whole may be used to perform control for performing the substrate processing process described later. When the term "control unit" is used in this specification, there may be a case where one control unit is included, and there may be a case where a control system includes multiple control units and is composed of multiple control units.

[0061] The storage device 121c is composed of, for example, a flash memory, an HDD (Hard Disk Drive), etc. In the storage device 121c, a control program configured to control the operation of the substrate processing device, a process process recording the steps, conditions, etc. of the manufacturing method of the semiconductor device described later, etc. are stored in a readable manner. The process process is configured in a manner that enables the controller 121 to execute each process (step) in the manufacturing method of the semiconductor device described later, and is combined in a manner that can obtain a specified result, and functions as a program. Hereinafter, the process process, control program, etc. are also collectively referred to as programs. When the word "program" is used in this specification, there are cases where only the process process itself is included, only the control program itself is included, or a combination of the process process and the control program is included. RAM121b is configured as a memory area (work area) that temporarily holds programs, data, etc. read by CPU121a.

[0062] The I / O port 121d is connected to the above-mentioned MFC312, 322, 332, 342, 512, 522, 532, valves 314, 324, 334, 344, 514, 524, 534, pressure sensor 245, APC valve 243, vacuum pump 246, heater 207, temperature sensor 263, rotating mechanism 267, wafer boat elevator 115, etc.

[0063] The CPU 121 a is configured to read a control program from the storage device 121 c and execute it, and to read a recipe or the like from the storage device 121 c in response to input of an operation command from the input / output device 122 or the like. CPU121a is configured to control the following actions according to the content of the read process: flow regulation action of various gases performed by MFC312, 322, 332, 342, 512, 522, 532, opening and closing action of valves 314, 324, 334, 344, 514, 524, 534, opening and closing action of APC valve 243 and pressure regulation action based on pressure sensor 245 using APC valve 243, temperature regulation action of heater 207 based on temperature sensor 263, starting and stopping of vacuum pump 246, rotation of wafer boat 217 and rotation speed regulation action performed by rotating mechanism 267, lifting and lowering action of wafer boat 217 by wafer boat elevator 115, and storage action of wafer 200 into wafer boat 217, etc.

[0064] The controller 121 can be configured by installing the above-mentioned program stored in the external storage device 123 into a computer. The storage device 121c and the external storage device 123 are configured as a computer-readable recording medium. Hereinafter, they are also collectively referred to as recording media. In this specification, there is a case where the recording medium only includes the storage device 121c itself, only includes the external storage device 123 itself, or includes both. The program can also be provided to the computer without using the external storage device 123, but using a communication mechanism such as the Internet and a dedicated line.

[0065] (2) Substrate processing step (film forming step)

[0066] use Figure 4 (A) in the figure describes an example of a process of forming a film on a wafer 200 as one process of manufacturing a semiconductor device. The process of forming a film is performed using the above-mentioned substrate processing apparatus 10. In the following description, the operation of each unit constituting the substrate processing apparatus 10 is controlled by the controller 121.

[0067] In the substrate processing step (semiconductor device manufacturing step) according to this embodiment,

[0068] (a) a step of supplying a first gas containing a first element and a halogen element to the wafer 200;

[0069] (b) a step of supplying a second gas containing a second element different from the first element to the wafer 200;

[0070] (c) a step of supplying a third gas containing a third element and having reducing properties to the wafer 200; and

[0071] (d) Step of supplying a fourth gas containing a fourth element and having reducing properties to the wafer 200

[0072] By performing (a) and (d) successively and (b) and (c) successively a predetermined number of times, a film containing the first element and the second element is formed on the wafer 200 .

[0073] When the term "wafer" is used in this specification, it may mean "the wafer itself" or "a laminate of a wafer and a predetermined layer, film, etc. formed on its surface". When the term "surface of a wafer" is used in this specification, it may mean "the surface of the wafer itself" or "the surface of a predetermined layer, film, etc. formed on the wafer". When the term "substrate" is used in this specification, it has the same meaning as when the term "wafer" is used.

[0074] In addition, in this specification, "a film that does not contain a certain element A" refers to a film that does not substantially contain the element A. "Substantially containing no element A" means that the content of the element A in the film is extremely low, including a case where the element A is almost not contained in the film, in addition to the case where the element A is not contained in the film at all. For example, it also includes a case where the content of the element A in the film is about 4% in atomic composition percentage, and preferably less than 4% in atomic composition percentage.

[0075] (Wafer loading)

[0076] When a plurality of wafers 200 are loaded into the wafer boat 217 (wafer filling), as shown in FIG. Figure 1 As shown, the boat 217 supporting a plurality of wafers 200 is lifted by the boat elevator 115 and carried into the processing chamber 201 (boat loading). In this state, the sealing cap 219 closes the lower end opening of the reaction tube 203 via the O-ring 220 .

[0077] (Pressure regulation and temperature regulation)

[0078] The vacuum pump 246 performs vacuum exhaust in the processing chamber 201 so that the desired pressure (vacuum degree) is achieved. At this time, the pressure in the processing chamber 201 is measured by the pressure sensor 245, and the APC valve 243 is feedback-controlled (pressure regulated) based on the measured pressure information. The vacuum pump 246 is always kept in an operating state at least until the processing of the wafer 200 is completed. In addition, the heater 207 performs heating in the processing chamber 201 so that the desired temperature is achieved. At this time, the amount of power supplied to the heater 207 is feedback-controlled (temperature regulated) based on the temperature information detected by the temperature sensor 263 so that the desired temperature distribution is achieved in the processing chamber 201. The heating in the processing chamber 201 by the heater 207 is continuously performed at least until the processing of the wafer 200 is completed.

[0079] [1st step]

[0080] (First gas supply)

[0081] The valve 314 is opened, and the first gas as the raw material gas flows into the gas supply pipe 310. The first gas is flow-regulated by the MFC 312 and supplied into the processing chamber 201 from the gas supply hole 410a of the nozzle 410. At this time, the valve 514 is opened, and an inert gas such as N2 gas flows into the gas supply pipe 510. The N2 gas flowing in the gas supply pipe 510 is flow-regulated by the MFC 512 and supplied into the processing chamber 201 together with the first gas.

[0082] At this time, the valves 524 and 534 are opened, and N2 gas is supplied into the processing chamber 201 through the gas supply pipes 520, 530, 320, 330 and the nozzles 420 and 430. Thus, the first gas can be prevented from entering the nozzles 420 and 430. That is, the first gas and N2 gas are supplied to the wafer 200. The first gas and N2 gas supplied into the processing chamber 201 are exhausted from the exhaust pipe 231.

[0083] At this time, the APC valve 243 is adjusted to set the pressure in the processing chamber 201 to a pressure in the range of, for example, 1 to 3990 Pa. The supply flow rate of the first gas controlled by the MFC 312 is set to a flow rate in the range of, for example, 0.1 to 2.0 slm. The supply flow rates of the N2 gas controlled by the MFCs 512, 522, and 532 are respectively set to a flow rate in the range of, for example, 0.1 to 20 slm. At this time, the temperature of the heater 207 is set so that the temperature of the wafer 200 becomes, for example, a temperature in the range of 300 to 600° C.

[0084] At this time, the gases flowing into the processing chamber 201 are only the first gas and the N2 gas. The first element-containing layer is formed on the wafer 200 (or the base film on the surface of the wafer 200) by the supply of the first gas. The first element-containing layer may be a first element layer containing a halogen element, or may be an adsorption layer of the first gas, or may contain both of the above.

[0085] (Fourth gas supply)

[0086] After a predetermined time, for example, 0.01 to 5 seconds, has passed since the supply of the first gas began, the valve 344 is opened to allow the fourth gas to flow into the gas supply pipe 340. Here, the fourth gas is flow-regulated by the MFC 342 and supplied into the processing chamber 201 from the gas supply hole 420a of the nozzle 420 via the gas supply pipe 320.

[0087] At this time, the valve 524 is opened at the same time, and an inert gas such as N2 gas flows into the gas supply pipe 520. The N2 gas flowing in the gas supply pipe 520 is adjusted in flow rate by the MFC 522, and is supplied to the processing chamber 201 together with the fourth gas. At this time, the valves 524 and 534 are opened, and the gas is supplied to the processing chamber 201 through the gas supply pipes 520, 530, 320, 330, and the nozzles 420 and 430. That is, the first gas, the fourth gas, and the N2 gas are supplied to the wafer 200.

[0088] At this time, the APC valve 243 is adjusted to set the pressure in the processing chamber 201 to a pressure in the range of, for example, 1 to 3990 Pa. The supply flow rate of the second gas controlled by the MFC 312 is set to a flow rate in the range of, for example, 0.1 to 2.0 slm. For example, the supply flow rate of the N2 gas controlled by the MFCs 512, 522, and 532 and the temperature of the heater 207 are set in the same manner as when the first gas is supplied.

[0089] After a predetermined time, for example, 0.01 to 10 seconds, has passed since the supply of the first gas began, the valve 314 of the gas supply pipe 310 is closed to stop the supply of the first gas. That is, the time for supplying the first gas to the wafer 200 is set to, for example, a time in the range of 0.01 to 10 seconds. At this time, in order to prevent the fourth gas from intruding into the nozzles 410 and 430, the valves 514 and 534 are opened to flow N2 gas into the gas supply pipes 510 and 530. At this time, the fourth gas and N2 gas are supplied to the wafer 200.

[0090] At this time, the APC valve 243 is adjusted to set the pressure in the processing chamber 201 to a pressure in the range of, for example, 130 to 3990 Pa. By setting the pressure in such a range, a film that does not contain the fourth element can be formed. In addition, the supply flow rate of the fourth gas controlled by the MFC 342 is set to a flow rate in the range of, for example, 0.1 to 5 slm. The supply flow rate of the N2 gas controlled by the MFCs 512, 522, and 532 and the temperature of the heater 207 are set in the same manner as when the first gas is supplied.

[0091] In the first step, the supply of the fourth gas is started simultaneously with the stop of the supply of the first gas or before the stop of the supply of the first gas. Thus, the process of supplying the first gas to the wafer 200 and the process of supplying the fourth gas to the wafer 200 are continuously performed. In other words, in the first step, a state in which at least one of the first gas and the fourth gas exists in the processing chamber 201 is maintained.

[0092] [Step 2]

[0093] (Residual gas removal)

[0094] After a predetermined time, for example, 0.01 to 10 seconds, has passed since the supply of the fourth gas started, the valve 344 is closed to stop the supply of the fourth gas. The processing chamber 201 may be evacuated by the vacuum pump 246 while the APC valve 243 of the exhaust pipe 231 is kept open. At this time, the first gas remaining in the processing chamber 201 that has not reacted or contributed to the formation of the first element-containing layer, and the fourth gas that has not reacted or reacted with the by-product are discharged from the processing chamber 201. At this time, the supply of N2 gas to the processing chamber 201 may be maintained while the valves 514, 524, and 534 are kept open. The N2 gas acts as a purge gas, which can improve the effect of discharging the first gas remaining in the processing chamber 201 that has not reacted or contributed to the formation of the first element-containing layer, and the fourth gas that has not reacted or reacted with the by-product from the processing chamber 201.

[0095] [Step 3]

[0096] (Second gas supply)

[0097] After the residual gas is removed, the valve 334 is opened to flow the second gas as the reaction gas into the gas supply pipe 330. The second gas is flow-regulated by the MFC 332 and supplied from the gas supply hole 430a of the nozzle 430 into the processing chamber 201. At this time, the valve 534 is opened at the same time to flow an inactive gas such as N2 gas into the gas supply pipe 530. The N2 gas flowing in the gas supply pipe 530 is flow-regulated by the MFC 532 and supplied into the processing chamber 201 together with the second gas. At this time, the gas flowing into the processing chamber 201 is only the second gas and the N2 gas.

[0098] At this time, valves 514 and 524 are opened to supply N2 gas into the processing chamber 201 through gas supply pipes 510, 520, 310, 320 and nozzles 410 and 420. This prevents the second gas from entering the nozzles 410 and 420. That is, the second gas and N2 gas are supplied to the wafer 200.

[0099] At this time, the APC valve 243 is adjusted to set the pressure in the processing chamber 201 to a pressure in the range of, for example, 1 to 3990 Pa. The supply flow rate of the second gas controlled by the MFC 312 is set to a flow rate in the range of, for example, 0.1 to 2.0 slm. The supply flow rate of the N2 gas controlled by the MFCs 512, 522, and 532 and the temperature of the heater 207 are set in the same manner as when the first gas is supplied.

[0100] The second gas supplied into the processing chamber 201 reacts with at least a portion of the first element-containing layer on the wafer 200 . As a result, a layer containing the first element and the second element (first and second element-containing layer) is formed on the wafer 200 .

[0101] (Third gas supply)

[0102] After a predetermined time, for example, 0.01 to 5 seconds, has passed since the supply of the second gas began, the valve 324 is opened to allow the third gas, which is a reducing gas, to flow into the gas supply pipe 320. Here, the third gas is flow-regulated by the MFC 322 and is supplied from the gas supply hole 420a of the nozzle 420 into the processing chamber 201. At this time, the valve 524 is simultaneously opened to allow an inactive gas such as N2 gas to flow into the gas supply pipe 520. The N2 gas flowing in the gas supply pipe 520 is flow-regulated by the MFC 522 and is supplied to the processing chamber 201 together with the third gas.

[0103] At this time, the valve 514 is opened to supply the second gas and the third gas into the processing chamber 201 through the gas supply pipes 510 and 310 and the nozzle 410. This prevents the second gas and the third gas from entering the nozzle 410. That is, the second gas, the third gas and the N2 gas are supplied to the wafer 200.

[0104] At this time, the APC valve 243 is adjusted to set the pressure in the processing chamber 201 to a pressure in the range of, for example, 130 to 3990 Pa. By setting the pressure in such a range, a film that does not contain the third element can be formed. In addition, the supply flow rate of the third gas controlled by the MFC 322 is set to a flow rate in the range of, for example, 0.1 to 5 slm. The supply flow rate of the N2 gas controlled by the MFCs 512, 522, and 532 and the temperature of the heater 207 are set in the same manner as when the first gas is supplied.

[0105] After a predetermined time, for example, 0.01 to 60 seconds, has passed since the supply of the second gas started, the valve 334 of the gas supply pipe 330 is closed to stop the supply of the second gas. That is, the time for supplying the second gas to the wafer 200 is set to, for example, a time in the range of 0.01 to 10 seconds. At this time, in order to prevent the third gas from intruding into the nozzles 410 and 430, the valves 514 and 534 are opened to flow N2 gas into the gas supply pipes 510 and 530. At this time, the third gas and N2 gas are supplied to the wafer 200.

[0106] At this time, the APC valve 243 is adjusted to set the pressure in the processing chamber 201 to a pressure in the range of, for example, 130 to 3990 Pa. In addition, the supply flow rate of the third gas controlled by the MFC 322 is set to a flow rate in the range of, for example, 0.1 to 5 slm. The supply flow rate of the N2 gas controlled by the MFCs 512, 522, and 532 and the temperature of the heater 207 are set in the same manner as when the first gas is supplied.

[0107] In the third step, the supply of the third gas is started before the supply of the second gas is stopped, or Figure 4 As in the timing of gas supply shown in (B) of FIG. 1 (described later as a variation 1 of the embodiment), the supply of the third gas is started at the same time as the supply of the second gas is stopped. Thus, the process of supplying the second gas to the wafer 200 and the process of supplying the third gas to the wafer 200 are performed continuously. In other words, in the third process, a state in which at least one of the second gas and the third gas exists in the processing chamber 201 is maintained.

[0108] [Step 4]

[0109] (Residual gas removal)

[0110] After a predetermined time, for example, 0.01 to 10 seconds, has passed since the supply of the third gas started, the valve 324 is closed to stop the supply of the third gas. Then, the second gas remaining in the processing chamber 201 that has not reacted or has contributed to the formation of the first and second element-containing layer, the reaction byproducts, and the third gas that has not reacted or has reacted with the byproducts are removed from the processing chamber 201 through the same processing steps as the second step described above.

[0111] (Specified number of implementations)

[0112] The cycle of sequentially performing the first step to the fourth step is performed one or more times (predetermined number of times (n times)), thereby forming a film containing the first element and the second element with a predetermined thickness (for example, 0.5 to 5.0 nm) on the wafer 200. Preferably, the above cycle is repeated a plurality of times. At this time, by performing the first step and the third step under the above conditions, a film containing the first element and the second element but not containing the third element and / or the fourth element can be formed.

[0113] (Post-purge and atmospheric pressure recovery)

[0114] N2 gas is supplied to the processing chamber 201 from each of the gas supply pipes 510, 520, and 530, and exhausted from the exhaust pipe 231. The N2 gas acts as a purge gas, thereby purging the processing chamber 201 with an inert gas, and the gas and by-products remaining in the processing chamber 201 are removed from the processing chamber 201 (post-purge). After that, the atmosphere in the processing chamber 201 is replaced with an inert gas (inert gas replacement), and the pressure in the processing chamber 201 is restored to normal pressure (atmospheric pressure recovery).

[0115] (Wafer removal)

[0116] After that, the sealing cover 219 is lowered by the wafer boat elevator 115 to open the lower end of the reaction tube 203. Then, the processed wafers 200 are carried out from the lower end of the reaction tube 203 to the outside of the reaction tube 203 while being supported by the wafer boat 217 (wafer boat unloading). After that, the processed wafers 200 are taken out of the wafer boat 217 (wafer taking out).

[0117] When a substance containing a halogen element is used as the first gas, a byproduct containing a halogen element is generated when the first element-containing layer and / or the first and second element-containing layer are formed. In addition, for example, when the second gas contains H, a byproduct containing a halogen element, for example, a hydrogen halide is generated. Such a byproduct sometimes hinders the reaction between the first gas and / or the second gas and the surface of the wafer 200. That is, the more such a byproduct exists on the wafer 200 and in the processing chamber 201, the more it hinders the formation of the first element-containing layer and / or the first and second element-containing layer, and thus there is a tendency for the film formation rate to decrease.

[0118] In the first step, the fourth gas reacts with the byproduct generated when the layer containing the first element is formed (or the byproduct is reduced), and is discharged from the processing chamber 201 as the halogenated fourth element. In addition, the third gas in the third step reacts with the byproduct generated when the layer containing the first and second elements is formed (or the byproduct is reduced), and is discharged from the processing chamber 201 as the halogenated third element. As a result, the amount of byproducts existing on the wafer 200 and in the processing chamber 201 in the first and third steps is reduced, so that the film formation rate can be improved.

[0119] In the first step of the embodiment, the supply of the second gas and the supply of the third gas are performed continuously. In this case, compared with the case where the supply of the second gas and the supply of the third gas are performed discontinuously, the time from the generation of the by-product to the reaction with the third gas is shortened. As a result, the amount of by-product adsorbed on the surface of the wafer 200 is further reduced, so the film formation rate can be increased. Therefore, it is preferred that the purge based on the inert gas in the processing chamber 201 is not performed during the supply of the second gas and the supply of the third gas. In addition, it is preferred not to exhaust the processing chamber 201 in a state where the second gas or the third gas is not supplied to the wafer 200.

[0120] The same is true in the third step. That is, by continuously supplying the second gas and the third gas, the film forming rate can be increased. In addition, it is preferred that during the supply of the first gas and the supply of the fourth gas, the processing chamber 201 is not purged with an inert gas, or the processing chamber 201 is not exhausted in a state where the first gas or the fourth gas is not supplied to the wafer 200.

[0121] In the embodiment, the third element in the third gas supplied continuously with the second gas tends to be easily captured in the film compared to the fourth element in the fourth gas supplied continuously with the first gas. However, in the case where both the third gas and the fourth gas are made to be stable gases that are difficult to be captured in the film, although the third gas can be suppressed from being captured in the film, there is a tendency that the effect of removing byproducts when the first gas is supplied is reduced. Thus, in terms of forming a film containing the first element and the second element but not containing the third element, it is preferred that the third gas be a gas (stable gas, low-reactivity gas) having a higher decomposition temperature than the fourth gas. Thus, it is possible to make the third gas less likely to be captured in the film and to make the effect of removing byproducts when the first gas is supplied less likely to be reduced.

[0122] (3) Modification

[0123] Figure 4 (B) is a diagram showing the timing of gas supply in Modification 1 of the embodiment. Figure 4As shown in (B) in FIG. 1 , the supply of the third gas may be started at the same time as the supply of the second gas is finished. In this case, the film formation rate can be improved in the same manner as in the embodiment.

[0124] Here, there is a tendency that the longer the second gas and the third gas are supplied, the higher the content of the third element in the film. As described above, in order to increase the film formation rate, it is preferable to supply the second gas and the third gas continuously. Thus, by starting the supply of the third gas at the same time as the end of the supply of the second gas, it is easy to form a film containing the first element and the second element but not the third element at a good film formation rate.

[0125] In contrast, the fourth element in the fourth gas supplied continuously with the first gas tends to be difficult to be captured in the film compared to the third element in the third gas supplied continuously with the second gas. In addition, when the supply of the first gas and the supply of the fourth gas are at least partially performed simultaneously, the time from when the byproduct is generated by the reaction of the first gas to when it reacts with the fourth gas becomes longer than when the supply of the fourth gas is started simultaneously with the end of the supply of the first gas. Thus, by partially performing the supply of the first gas and the supply of the fourth gas simultaneously, it is easy to improve the film formation rate when forming a film containing the first element and the second element but not containing the fourth element.

[0126] Figure 4 (C) is a diagram showing the timing of gas supply in Modification 2 of the embodiment. Figure 4 As shown in (C) in FIG. 1 , the supply of the second gas may be started at the same time as the supply of the third gas is terminated. In addition, the supply of the third gas may be started during the supply of the second gas while the supply of the third gas is continuous. In these cases, the film forming rate can be improved in the same manner as in the embodiment.

[0127] In addition, the first element-containing layer before reacting with the second gas tends to react with the third gas more easily than after reacting with the second gas. Therefore, in Modification 2 in which the third gas reaches the first element-containing layer earlier than the second gas, the third element content of the film tends to be higher than that of Modification 1. That is, when forming a film containing the first element and the second element but not containing the third element, it is more preferable to start supplying the third gas after starting supplying the second gas as in the embodiment and Modification 1 than to start supplying the second gas after starting supplying the third gas as in Modification 2.

[0128] Experimental examples are described below, but the present invention is not limited to these experimental examples.

[0129] <Experimental example>

[0130] In this experimental example, a titanium nitride (TiN) film was formed under the conditions described below using the substrate processing apparatus 10 used in the above-mentioned embodiment. In this experimental example, a gas containing titanium (Ti) as a first element and a halogen element was set as the first gas, a N-containing gas containing nitrogen (N) as a second element was set as the second gas, a gas containing a Group 15 element having a reducing property as the third element was set as the third gas, and a gas containing a Group 14 element having a reducing property as the fourth element was set as the fourth gas.

[0131] Separately, in Condition 1, the Figure 4 The gas supply timing of (B) in Condition 2 is used as the modified example 2. Figure 4 In addition, as a comparative example 1, a TiN film was formed on the substrate by using the gas supply timing of (C). Figure 5 Specifically, in Comparative Example 1, a TiN film is formed on a substrate by performing a cycle of first gas supply, residual gas removal, second gas supply, and residual gas removal for a predetermined number of times. In addition, as Comparative Example 2, a TiN film is formed on a substrate by using a gas supply timing shown in (A). Figure 5 Specifically, in Comparative Example 2, a TiN film is formed on a substrate by supplying the first gas, supplying the first gas and the fourth gas simultaneously, supplying the fourth gas, removing the residual gas, supplying the second gas, and removing the residual gas for a predetermined number of times. In addition, as Comparative Example 3, a TiN film is formed on a substrate by supplying the first gas, supplying the first gas and the fourth gas simultaneously, supplying the fourth gas, removing the residual gas, and supplying the second gas. Figure 5 Specifically, in Comparative Example 3, the TiN film is formed on the substrate by performing a cycle of supplying the first gas, supplying the first gas and the third gas simultaneously, supplying the third gas, removing the residual gas, supplying the second gas, and removing the residual gas a predetermined number of times. In addition, the conditions other than the gas supply timing are performed within the range exemplified in the above-mentioned embodiment.

[0132] The results of X-ray diffraction (XRD) measurements of these TiN films are shown in Figure 7 .

[0133] In the TiN film of Comparative Example 1, the intensity of 111 diffraction becomes lower than the intensity of 200 diffraction of the TiN crystal. It can be seen from this that in the TiN film, the proportion of TiN grains growing toward the {111} plane in the direction perpendicular to the surface of the wafer 200 is greater than that of the {100} plane. That is, the {111} plane becomes the dominant crystal orientation. The TiN film in which the {111} plane is the dominant crystal orientation is prone to form gaps between the grains, and liquids, gases, etc. invade the gaps, thereby sometimes producing substances other than TiN such as oxides, etc., which leads to a decrease in film quality. Therefore, in such a TiN film, the film quality is likely to become lower and the resistance is likely to become higher. In other words, by making the planes other than the {111} plane the dominant crystal orientation, the film quality and resistance of the TiN film can be improved.

[0134] The intensity of the 200 diffraction line of the TiN film of Comparative Example 2 relative to the intensity of the 111 diffraction line is higher than that of the TiN film of Comparative Example 1. This shows that the number of TiN grains oriented along the {100} plane increases. Therefore, as in Comparative Example 2, by continuously supplying the first gas and the fourth gas, the film quality of the TiN film can be improved.

[0135] The TiN film of Comparative Example 3 also has a higher intensity of the 200 diffraction line relative to the 111 diffraction line than the TiN film of Comparative Example 1. That is, as in Comparative Example 3, by continuously supplying the first gas and the third gas, the film quality of the TiN film can be improved.

[0136] In addition, the intensity of the 200 diffraction line of the TiN film of Comparative Example 3 is higher relative to the intensity of the 111 diffraction line than that of the TiN film of Comparative Example 2. Therefore, compared with the case where the first gas supply and the fourth gas supply are continuously performed as in Comparative Example 2, the effect of improving the film quality of the TiN film is greater when the first gas supply and the third gas supply are continuously performed as in Comparative Example 3.

[0137] In addition, the intensity of the 200 diffraction line of the TiN film under Conditions 1 and 2 relative to the intensity of the 111 diffraction line is higher than that of the TiN film of Comparative Example 2. Therefore, as in Conditions 1 and 2, by continuously supplying the second gas and the third gas, and continuously supplying the second gas and the fourth gas, the film quality of the TiN film can be improved.

[0138] In addition, the intensity of the 200 diffraction line of the TiN film of condition 1 is higher than that of the 111 diffraction line of the TiN film of condition 2. Moreover, the width of the diffraction peak of the TiN film of condition 2 is larger than that of the TiN film of condition 2 in relation to the height. It can be seen from this that the TiN film of condition 2 is closer to an amorphous state than the TiN film of condition 1. In other words, it can be seen that the TiN film of condition 1 has better crystallinity than the TiN film of condition 2. Therefore, in the case of continuously supplying the second gas and the third gas, it is more preferable to start the supply of the third gas after starting the supply of the second gas as in condition 1 than to start the supply of the second gas after starting the supply of the third gas as in condition 2.

[0139] As can be seen from the above, in the process of forming the TiN film, the third gas and / or the fourth gas function as a modifying gas that increases the proportion of TiN grains oriented along a predetermined crystal plane in the formed TiN film. Therefore, the process of supplying the third gas and / or the fourth gas can also be regarded as a process of modifying the TiN film.

[0140] In the experimental example, as the first gas (raw gas) containing the first element and the halogen element, a gas containing the metal element Ti as the first element and the halogen element is used for explanation. However, the present invention is not limited to this. For example, as the first element, it can also be tantalum (Ta), tungsten (W), cobalt (Co), yttrium (Y), ruthenium (Ru), aluminum (Al), hafnium (Hf), zirconium (Zr), molybdenum (Mo), niobium (Nb), manganese (Mn), nickel (Ni), silicon (Si), etc. as metal elements. In addition, as the halogen element, fluorine (F), chlorine (Cl), bromine (Br), iodine (I), etc. can be used.

[0141] Regarding the gas containing a halogen element and a metal element as the first gas, for example, tantalum pentachloride (TaCl5), tantalum pentafluoride (TaF5), tungsten hexachloride (WCl6), tungsten hexafluoride (WF6), titanium tetrafluoride (TiF4), cobalt dichloride (CoCl2), cobalt dichloride (CoF2), yttrium trichloride (YCl3), yttrium trifluoride (YF3), ruthenium trichloride (RuCl3), ruthenium trifluoride (RuF3), aluminum trichloride (AlCl3), aluminum trifluoride (AlF3), hafnium tetrachloride (HfCl4) can be used. , hafnium tetrafluoride (HfF4), zirconium tetrachloride (ZrCl4), zirconium tetrafluoride (ZrF4)), molybdenum pentafluoride (MoF5), molybdenum pentachloride (MoCl5), niobium trifluoride (NbF3), niobium trichloride (NbCl3), manganese difluoride (MnF2), manganese dichloride (MnCl2), nickel difluoride (NiF2), nickel dichloride (NiCl2), tetrachlorosilane (SiCl4), dichlorosilane (SiH2Cl2), monochlorosilane (SiH3Cl), hexachlorodisilane (Si2Cl6) and other gases to form a film. As the first gas, one or more of them can be used.

[0142] In the experimental example, as the second gas (raw material gas), an N-containing gas (nitriding gas) containing N as the second element is used. However, the present invention is not limited to this. As the second element, for example, oxygen (O) which is a Group 16 element can be used. As the second gas, for example, an O-containing gas (oxidizing gas) containing O as the second element can be used.

[0143] Regarding the N-containing gas as the second gas, for example, a gas containing N and hydrogen (H), or a gas containing carbon (C) and N can be used. As a gas containing N and H, for example, a nitride-based gas containing an NH bond can be used. Specifically, ammonia (NH3), hydrazine (N2H4), diazene (N2H2), N3H8, etc. can be used. In addition, as a gas containing C and N, an amine-based gas or an organic hydrazine-based gas can be used. In addition, for example, monoethylamine (C2H5NH2), diethylamine ((C2H5)2NH), triethylamine ((C2H5)3N), monomethylamine (CH3NH2), dimethylamine ((CH3)2NH), trimethylamine ((CH3)3N), etc. can be used. In addition, for example, monomethylhydrazine ((CH3)HN2H2), dimethylhydrazine ((CH3)2N2H2), trimethylhydrazine ((CH3)2N2(CH3)H), etc. can be used. As the second gas, one or more of these can be used.

[0144] In addition, regarding the O-containing gas as the second gas, for example, oxygen (O2) gas, nitrous oxide (N2O) gas, nitric oxide (NO) gas, nitrogen dioxide (NO2) gas, ozone (O3) gas, water vapor (H2O gas), carbon monoxide (CO) gas, carbon dioxide (CO2) gas, O2 gas + hydrogen (H2) gas, O3 gas + H2 gas, H2O gas + H2 gas, etc. can be used. It should be noted that in this specification, the recording of two gases such as "O3 gas + H2 gas" refers to a mixed gas of O3 gas and H2 gas. As the second gas, one or more of them can be used.

[0145] In the experimental example, a reducing gas containing a Group 15 element as the third element is used as the third gas, and a reducing gas containing a Group 14 element as the fourth element is used as the fourth gas. However, the present invention is not limited thereto. For example, any one of a Group 13 element, a Group 14 element, and a Group 15 element can be used as the third element and / or the fourth element.

[0146] In addition, it is preferred to use the 15th group element as the 3rd element.Thus, the 3rd element can be made difficult to be captured in. In addition, it is further preferred to use P as the 15th group element as the 3rd element.Thus, the 3rd element can be further made difficult to be captured in the film. In addition, when using the 15th group element as the 3rd element, it is preferred to use the 14th group element as the 4th element.Thus, the 4th element can be further made difficult to be captured in the film.

[0147] As the 13th group element, for example, boron (B) can be used. As the 14th group element, for example, C, Si, and Ge can be used. As the 15th group element, for example, N and P can be used. Among them, when forming a film that does not contain the third element and / or the fourth element, it is preferable to use an element different from the first element and the second element as the third element and / or the fourth element.

[0148] In addition, even if a gas containing the third element and H or a gas containing the fourth element and H is used, the above effect can be obtained. As such a gas, for example, a gas containing a bond between the third element and hydrogen in one molecule or a gas containing a bond between the fourth element and hydrogen in one molecule can be used respectively. As such a gas, for example, a gas containing only the third element and hydrogen in one molecule or a gas containing a bond between the fourth element and hydrogen in one molecule can be used respectively. In the case of removing a byproduct containing a halogen element by the third gas and / or the fourth gas, it is preferable to use a gas not containing a halogen element.

[0149] As the above-mentioned gas, for example, one or more of borane (BH3), diborane (B2H6), methane (CH4), ethane (C2H6), monosilane (SiH4), disilane (Si2H6), germane (GeH4), digermane (Ge2H6), NH3, N2H4, phosphine (PH3), diphosphine (P2H4) and the like can be used as the third gas and the fourth gas. In addition, it is preferred to select one or more of these gases so that the third gas is a gas having a higher decomposition temperature than the fourth gas.

[0150] In addition, in the embodiments and their variations and experimental examples, the configuration of supplying the third gas and the fourth gas into the processing chamber 201 from the common nozzle 420 is described. However, the present invention is not limited thereto. The present invention can also be applied to the case where the third gas and the fourth gas are supplied into the processing chamber 201 from separate nozzles.

[0151] In addition, in the embodiments, variations, and experimental examples, a configuration for film formation using a batch-type substrate processing apparatus that processes a plurality of substrates at a time is described. However, the present invention is not limited thereto, and can also be appropriately applied to a case where film formation is performed using a substrate processing apparatus that processes one or more substrates at a time. In addition, in the above-mentioned embodiment, an example of film formation using a substrate processing apparatus having a hot-wall type processing furnace is described. The present invention is not limited to the above-mentioned embodiment, and can also be appropriately applied to a case where a film is formed using a substrate processing apparatus having a cold-wall type processing furnace.

[0152] When these substrate processing apparatuses are used, each process can be performed with the same processing steps and processing conditions as those in the above-mentioned embodiments, modified examples, and experimental examples, and the same effects as those in the above-mentioned embodiments, modified examples, and experimental examples can be obtained.

[0153] The embodiment and its Modification 1, Modification 2, Comparative Examples 1, 2, and 3 in the experimental examples have been described above. However, the present invention is not limited to these embodiments, and can be used in appropriate combination.

Claims

1. A substrate processing method, comprising the following steps: (a) a step of supplying a first gas containing a first element and a halogen element to a substrate; (b) supplying a second gas containing a second element different from the first element to the substrate; (c) a step of supplying a third gas containing a third element and having reducing properties to the substrate; and (d) a step of supplying a fourth gas containing a fourth element and having reducing properties, (a) and (d) are performed successively, and (b) and (c) are performed successively a predetermined number of times, thereby forming a film including the first element and the second element on the substrate.

2. The substrate processing method according to claim 1, wherein: The decomposition temperature of the third gas is higher than that of the fourth gas.

3. The substrate processing method according to claim 1, wherein: The film does not contain the third element and / or the fourth element.

4. The substrate processing method according to claim 1, wherein: During (b) and (c), a state in which at least one of the second gas and the third gas exists in the space where the substrate exists is maintained.

5. The substrate processing method according to claim 1, wherein: During (b) and (c), the space where the substrate is located is not purged.

6. The substrate processing method according to claim 1, wherein: During the period between (b) and (c), the space where the substrate exists is not vacuum-exhausted, and the supply of gas to the substrate is not being performed.

7. The substrate processing method according to claim 1, wherein: (c) starts after (b) starts.

8. The substrate processing method according to claim 7, wherein: (c) starts at the same time as (b) ends.

9. The substrate processing method according to claim 1, wherein: Start (b) after starting (c).

10. The substrate processing method according to claim 9, wherein: (b) starts at the same time as (c) ends.

11. The substrate processing method according to claim 9, wherein: (a) and (d) are performed at least partially simultaneously.

12. The substrate processing method according to claim 1, wherein: The third gas is a modifying gas that increases the ratio of crystal grains oriented along a predetermined crystal plane in the film.

13. The substrate processing method according to claim 1, wherein: The fourth gas is a modifying gas that increases the ratio of crystal grains oriented along a predetermined crystal plane in the film.

14. The substrate processing method according to any one of claims 1 to 11, wherein: The first element is a metal element, and the film is a metal element-containing film.

15. The substrate processing method according to any one of claims 1 to 11, wherein: The third element is any one of Group 13 elements, Group 14 elements, and Group 15 elements.

16. The substrate processing method according to any one of claims 1 to 11, wherein: The fourth element is any one of Group 13 elements, Group 14 elements, and Group 15 elements.

17. A method for manufacturing a semiconductor device, comprising the following steps: (a) a step of supplying a first gas containing a first element and a halogen element to a substrate; (b) supplying a second gas containing a second element different from the first element to the substrate; (c) a step of supplying a third gas containing a third element and having reducing properties to the substrate; and (d) a step of supplying a fourth gas containing a fourth element and having reducing properties, (a) and (d) are performed successively, and (b) and (c) are performed successively a predetermined number of times, thereby forming a film including the first element and the second element on the substrate.

18. A substrate processing apparatus comprising: a first gas supply system for supplying a first gas containing a first element and a halogen element to the substrate; a second gas supply system for supplying a second gas including a second element different from the first element to the substrate; a third gas supply system for supplying a third gas containing a third element and having reducing properties to the substrate; a fourth gas supply system for supplying a fourth gas containing a fourth element and having reducing properties to the substrate; and The control unit is configured to control the first gas supply system, the second gas supply system, and the third gas supply system to perform the following processing, the processing including: (a) supplying the first gas to the substrate; (b) supplying the second gas to the substrate; (c) a process of supplying the third gas to the substrate; and (d) supplying the fourth gas to the substrate, The process of forming a film including the first element and the second element on the substrate is performed by performing (a) and (d) successively and (b) and (c) successively a predetermined number of times.

19. A computer-readable recording medium having a program recorded thereon for causing a substrate processing apparatus to execute the following steps using a computer, the steps comprising: (a) supplying a first gas containing a first element and a halogen element to a substrate; (b) supplying a second gas containing a second element different from the first element to the substrate; (c) a step of supplying a third gas containing a third element and having reducing properties to the substrate; and (d) a step of supplying a fourth gas containing a fourth element and having reducing properties, (a) and (d) are performed successively, and (b) and (c) are performed successively a predetermined number of times, thereby forming a film including the first element and the second element on the substrate.

Citation Information

Patent Citations

  • Manufacturing method of semiconductor device, substrate processing device, and program

    WO2019058608A1

  • Method for producing semiconductor device, substrate processing apparatus, and program

    CN113227450A

  • Semiconductor device manufacturing method, substrate processing apparatus, and recording medium

    CN114250447A

  • Substrate processing method, semiconductor device manufacturing method, substrate processing apparatus, and recording medium

    CN114959639A

  • Substrate processing method, substrate processing apparatus, recording medium, and method of manufacturing semiconductor device