Optical waveguide element, optical modulator using optical waveguide element, and optical transmission device
By coupling the first optical waveguide covered with a low refractive index layer and the second substrate with electro-optical effect in the optical waveguide element, and forming a convex portion at the interface, the small refractive index difference between the SiN waveguide and the TFLN rib optical waveguide is solved. It achieves low-loss light transfer and productivity improvement due to the difficult problem of light transfer.
Patent Information
- Application Number
- CN202311394746.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2023-03-30
- Filing Date
- 2023-10-25
- Publication Date
- 2024-10-01
AI Technical Summary
When the refractive index difference between the SiN waveguide and the TFLN rib optical waveguide is reduced, it is difficult to achieve low-loss light transfer, and the dry etching processing technology of the SiN waveguide has problems of high cost and low yield.
Designing an optical waveguide element, wherein the first substrate has a first optical waveguide covered with a low refractive index layer, and is optically coupled with a second substrate having an electro-optical effect, and the second substrate forms a convex portion at the interface to reduce light loss, And optimize light transfer by adjusting the width and thickness of the optical waveguide.
It achieves low-loss light transfer with a small refractive index difference, reduces light loss, and improves productivity and yield.
Smart Images

Figure CN118732154A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to an optical waveguide element, an optical modulation device and an optical transmitting device using the optical waveguide element, and more particularly to an optical waveguide element in which a first substrate having a first optical waveguide formed thereon and a second substrate having a rib-type optical waveguide formed thereon as a second optical waveguide are bonded together to optically couple the first optical waveguide and the second optical waveguide to each other, an optical modulation device and an optical transmitting device using the optical waveguide element. Background Art
[0002] In recent years, when making optical waveguide elements for optical communication, Si waveguides are used in optical waveguides (see Non-Patent Document 1). Since Si waveguides use CMOS (Complementary Metal Oxide Semiconductor) technology, they are scalable and excellent in terms of low cost, and can also be equipped with Ge / Si-based light-receiving elements. On the other hand, as a disadvantage, they cannot be used in the visible light region, and phase modulation makes it difficult to control the current flowing into the Si waveguide.
[0003] Therefore, as an alternative technology, silicon nitride (SiN), Thin Film LiNbO 3 (TFLN, thin film LN) is a new platform for optical waveguide cores (see non-patent literature 2, 3). In order to integrate optical functions, light source, phase modulation, reception, light synthesis / separation (power synthesis / branching, wavelength synthesis / separation, polarization wave synthesis / separation, etc.) are required. The most suitable materials for these structures are different, so methods for integrating heterogeneous materials are being developed.
[0004] In the case of heterogeneous material bonding, epitaxy can also be used. In recent years, direct bonding methods that bond flattened materials have been used to achieve optical functional integration using a combination of materials that cannot be grown epitaxially. Among them, an element that integrates light synthesis / separation and phase modulation has been developed by integrating silicon nitride (SiN) waveguides with TFLN.
[0005] In non-patent document 4, a SiN waveguide is formed on TFLN, thereby realizing phase modulation without processing LN into a waveguide. Compared with the monolithic TFLN modulator (see non-patent document 2), this method has a relatively large bending radius of several hundred μm and a large driving voltage (Vπ) because the light confinement of the optical waveguide is weak. However, LiNbO, which is a difficult material to process (difficult to dry-etch), has not been studied. 3 By processing (LN) and easily processed SiN, productivity is ensured.
[0006] On the other hand, it is proposed to replace the phase modulation part of the optical modulator using Si with phase modulation using the electro-optical effect of LN, etc., thereby achieving the same phase modulation as the previous LN and the easy processing, mass production, and miniaturization of Si waveguides (see non-patent document 5). The refractive index of Si is about 3.45, which is much higher than about 2.14 of LN. When the size of the Si waveguide is increased, as an optical waveguide, the light confinement effect is higher, and the light distribution can be biased only inside the Si waveguide, and it is difficult to be affected by light scattering caused by structural changes of other materials near the Si waveguide. As a result, it is possible to suppress the light loss at the end of the TFLN substrate arranged on the substrate containing the Si waveguide.
[0007] Figure 1 It is a plan view showing an example in which a second substrate 2 such as TFLN including a second optical waveguide 20 is arranged in a superimposed manner on a first substrate 1 including a first optical waveguide 10 such as a Si waveguide. Figure 2 (a) to (c) indicate Figure 1 The first optical waveguide 10 is a cross-sectional view at the dot-dash lines AA, BB, and CC. It should be noted that the first optical waveguide 10 is a core portion, and is covered by a low refractive index layer 11 (cladding portion) composed of a material having a lower refractive index than the material constituting the optical waveguide. In addition, in order to maintain mechanical strength, the first optical waveguide is supported by a holding substrate 12 as needed. The second optical waveguide 20 uses a rib-type optical waveguide in which a portion of the second substrate is higher than its periphery.
[0008] In such Figure 1 When the optical waveguide element is viewed from above, a portion 100 that widens the width of the first optical waveguide is provided at the boundary where the first optical waveguide 10 overlaps with the second substrate 2 (the edge of the second substrate), thereby enhancing the light confinement effect and suppressing light loss caused by the influence of the edge of the second substrate 2.
[0009] In addition, the light transfer between the Si waveguide and the TFLN waveguide is performed by reducing the cross-sectional size of the Si waveguide on the high refractive index side to expand the light distribution and transfer the light wave to the TFLN waveguide. As a result, the light transfer between the Si waveguide and the TFLN waveguide can be made low-loss (see Non-Patent Document 6). Therefore, the first optical waveguide 101 entering the lower side of the second substrate is as shown in FIG. Figure 1 As shown, the width of the optical waveguide is narrowed in a tapered shape at a position overlapping with the second optical waveguide 20 .
[0010] The problem with Si waveguides is that they are not transparent at wavelengths below 1.1 μm, so they may not be usable. In addition, they may also cause phenomena such as two-photon absorption, so they cannot input high-intensity light.
[0011] Therefore, by combining SiN waveguide and TFLN, it is possible to provide an optical waveguide element that can be used in the visible range and can perform phase modulation based on the change of electric field intensity used in the LN optical modulator. Of course, the dry etching processing technology of SiN is also established, so the productivity is high like that of Si waveguide.
[0012] However, the refractive index of SiN is about 2.00, which is also close to the refractive index of LN (about 2.14). Therefore, even if the size of the SiN waveguide as the first optical waveguide is increased at the edge of the TFLN, it will be affected by the TFLN. Moreover, it is difficult to simply apply the structure used for the Si waveguide to the light transfer between the SiN waveguide as the first optical waveguide and the rib-type optical waveguide 20 of the TFLN as the second optical waveguide. For example, a method of removing as much as possible around the rib-type optical waveguide 20 to make it thinner, or narrowing the width dimension of the second substrate 2 can also be considered, but high processing accuracy is required, which will increase the cost involved in manufacturing and reduce the yield rate.
[0013] Moreover, in order to Figure 2 As shown in (c), a rib-type optical waveguide 20 is formed on the first substrate 1 and on the TFLN as the second substrate, as shown in FIG. Figure 3 As shown in (a), after the first substrate 1 is bonded to the second substrate 2, as shown in Figure 3 As in (b), the resist pattern PR1 is formed so as to cover the position where the second optical waveguide is to be formed and the portion of the first substrate 1 that is not to be etched.
[0014] In particular, the resist material is arranged to cover (overhang) the edge of the TFLN near the first optical waveguide. If a portion of the Si waveguide or SiN waveguide serving as the first optical waveguide is damaged by etching, a large optical loss will occur.
[0015] As a result, if Figure 3 As shown in (c) , a convex portion 22 having the same height as the rib-type optical waveguide 20 is formed at the edge of the TFLN. Figure 4 This is a plan view, and the protrusion 22 is formed on the edge portion of the second substrate 2 including the boundary portion with the first optical waveguide 10 ( 100 ). Figure 5 yes Figure 4 Cross-sectional view at the single-dot chain line DD.
[0016] Regarding the influence of the protrusion 22, when the first optical waveguide is a Si waveguide, the light confinement effect can be improved and the light loss can be suppressed by widening the structure of the portion 100 with the width of the optical waveguide. However, when the first optical waveguide is a SiN waveguide, it is difficult to eliminate this problem by simply widening the structure of the portion 100 with the width.
[0017] Prior Art Literature
[0018] Non-patent literature
[0019] Non-patent document 1: Yikai Su et al., "Silicon Photonic Platform for Passive Waveguide Devices: Materials, Fabrication, and Applications", Advanced Materials Technologies. 1901153 (2020)
[0020] Non-patent document 2: Abdul Rahim et al., "Expanding the Silicon Photonics Portfolio With Silicom Nitride Photonic Integrated Circuits", Journal of Lightwave Technology, Vol. 35, No. 4, pp639 (February 15, 2017)
[0021] Non-patent document 3: Mian Zhang et al., "Integrated Lithium Niobate Electro-optic Modulators: When performance meets scalability", Optica, Vol. 8, No. 5, pp652 (2021)
[0022] Non-Patent Document 4: Sean Nelan et al., "Ultra-high Extinction Dual-output Thin-film Lithium Niobate Intensity Modulator", arXiv:2207.02608v1 (July 6, 2022)
[0023] Non-patent document 5: Shihao Sun et al., "Hybrid Silicon and Lithium Niobate Modulator", IEEE Journal of selected topics in Quantum Electronics, Vol. 27, No. 3, pp3300112 (May / June 2021)
[0024] Non-Patent Document 6: Peter O. Weigel et al., "Bonded Thin Film Lithium Niobate Modulator on a Silicon Photonics Platform Exceeding 100GHz3-dB Electrical Modulation Bandwidth", Optics Express, Vol. 26, No. 18, pp. 23728 (September 3, 2018) Summary of the invention
[0025] Problems to be solved by the invention
[0026] The problem to be solved by the present invention is to provide an optical waveguide element that can solve the above-mentioned problem and transfer light between the two with low loss even when the refractive index difference between the two is reduced, such as in the case of SiN waveguide and TFLN rib-type optical waveguide. Furthermore, an optical modulation device and an optical transmission device using the optical waveguide element are provided.
[0027] Solutions to Solve Problems
[0028] In order to solve the above-mentioned problems, an optical waveguide element, an optical modulation device using the optical waveguide element, and an optical transmission device according to the present invention have the following technical features.
[0029] (1) An optical waveguide element comprising: a first substrate having a first optical waveguide and a low refractive index layer, the low refractive index layer covering the first optical waveguide and being made of a material having a lower refractive index than the first optical waveguide; and a second substrate bonded to the first substrate and made of a material having an electro-optical effect and having a rib-type optical waveguide as a second optical waveguide, the first optical waveguide and the second optical waveguide having a portion optically coupled to each other, wherein the optical waveguide element is characterized in that, when the optical waveguide element is viewed from above, a convex portion is formed on the second substrate at a boundary portion where the first optical waveguide and the second substrate overlap, and a thickness of the second substrate at the convex portion is thinner than a thickness of the second substrate at the second optical waveguide.
[0030] (2) In the optical waveguide element described in (1) above, a length of the first optical waveguide at the convex portion in the propagation direction of the light wave is 2 μm or less.
[0031] (3) In the optical waveguide element described in (1) above, the width of the first optical waveguide at the boundary portion is set to be wider than the width of the first optical waveguide located in a front section or a rear section of the boundary portion.
[0032] (4) In the optical waveguide element described in (1) above, a difference in refractive index between the first optical waveguide and the second optical waveguide is 0.8 or less.
[0033] (5) In the optical waveguide element described in (4) above, the first optical waveguide is made of SiN and the second substrate is made of lithium niobate.
[0034] (6) An optical modulator, characterized in that the optical waveguide element described in any one of (1) to (5) above is accommodated in a housing, wherein the optical modulator includes an optical fiber that inputs or outputs a light wave to or from the first optical waveguide.
[0035] (7) In the optical modulator described in (6) above, the second substrate has a modulation electrode for modulating the light wave propagating in the second optical waveguide, and the shell has an electronic circuit inside which amplifies the modulation signal input to the modulation electrode.
[0036] (8) An optical transmitting device, characterized in that it comprises: the optical modulator described in (7) above; a light source for inputting light waves to the optical modulator; and an electronic circuit for outputting modulated signals to the optical modulator.
[0037] Effects of the Invention
[0038] The present invention comprises a first substrate and a second substrate, wherein the first substrate comprises a first optical waveguide and a low refractive index layer, the low refractive index layer covers the first optical waveguide and is made of a material having a lower refractive index than the first optical waveguide, the second substrate is bonded to the first substrate and is made of a material having an electro-optical effect, and comprises a rib-type optical waveguide as a second optical waveguide, the first optical waveguide and the second optical waveguide have a mutually optically coupled portion, wherein, when the optical waveguide element is viewed from above, a convex portion is formed on the second substrate at a boundary portion where the first optical waveguide and the second substrate overlap, and the thickness of the second substrate at the convex portion is thinner than the thickness of the second substrate at the second optical waveguide, thereby suppressing the optical loss of the first optical waveguide caused by the edge portion of the second substrate. Thus, an optical waveguide element capable of transferring light between the two with low loss can be provided even when the difference in refractive index between the two is small, such as a SiN waveguide or a TFLN rib-type optical waveguide, and further, an optical modulation device and an optical transmission device using the optical waveguide element can be provided. BRIEF DESCRIPTION OF THE DRAWINGS
[0039] Figure 1 It is a top view showing an example of an optical waveguide element.
[0040] Figure 2 yes Figure 1 A cross-sectional view of an optical waveguide element. Figure 2(a) is a cross-sectional view taken along the dashed line AA, (b) is a cross-sectional view taken along the dashed line BB, and (c) is a cross-sectional view taken along the dashed line CC.
[0041] Figure 3 This is a diagram showing a part of the manufacturing process of the optical waveguide element, and particularly shows a state where the protrusions 22 are formed on the second substrate 2 .
[0042] Figure 4 yes Figure 3 (c) is a top view of the optical waveguide element shown.
[0043] Figure 5 yes Figure 4 Cross-sectional view at the single-dot chain line DD.
[0044] Figure 6 It is a plan view showing an example of the optical waveguide element of the present invention.
[0045] Figure 7 yes Figure 6 Cross-sectional view at the single-dot chain line DD.
[0046] Figure 8 This is a diagram showing a part (part 1) of the manufacturing process related to the optical waveguide element of the present invention.
[0047] Fig. 9 This is a diagram showing a part (part 2) of the manufacturing process related to the optical waveguide element of the present invention.
[0048] Fig.10 This is a diagram for explaining an example of optically coupling two optical waveguides in the optical waveguide element of the present invention.
[0049] Fig.11 This is a diagram showing an example of changes in the effective refractive index in two optical waveguides in the light propagation direction.
[0050] Fig.12 This is a diagram for explaining a simulation model when TFLN is mounted on the upper side of a SiN waveguide.
[0051] Fig.13 It is a graph showing the relationship between the width of the SiN waveguide and the thickness of the TFLN.
[0052] Fig.14 This is a diagram showing changes in overlap integral (Loss) due to changes in the distance between the SiN waveguide and the TFLN and the thickness of the TFLN when the height (thickness) of the SiN waveguide is kept constant.
[0053] Fig.15 FIG. 1 is a diagram illustrating a simulation model of light transfer between a SiN waveguide and a rib-type light waveguide (TFLN).
[0054] Fig.16 It is a graph showing the change of light loss when the wavelength changes.
[0055] Fig.17 It is a diagram for explaining a simulation model for evaluating the influence of the convex portion of the edge portion of TFLN.
[0056] Fig.18 It is a diagram showing the influence of the convex part of TFLN.
[0057] Fig.19 This is a diagram for explaining a part of a manufacturing process using a wafer for constituting a plurality of optical waveguide elements (chips).
[0058] Fig. 20 This is a diagram for explaining a part of the manufacturing process of an optical waveguide element using a second substrate (TFLN) in the action portion of the optical modulator.
[0059] Fig.21 This is a diagram showing an example of an optical transmission device according to the present invention.
[0060] Description of symbols
[0061] 1First substrate
[0062] 10First optical waveguide (SiN)
[0063] 11 Low refractive index layer
[0064] 12. Hold the substrate
[0065] 2 Second substrate (TFLN)
[0066] 20 Second optical waveguide (rib type optical waveguide)
[0067] 23 convex part
[0068] 24 Peeling Layer
[0069] 25. Retaining member
[0070] F Fiber Optic
[0071] LD Light Source
[0072] CA Housing
[0073] MD Optical Modulation Devices
[0074] DRV drive circuit
[0075] DSP Digital Signal Processor
[0076] OTA optical transmitter DETAILED DESCRIPTION
[0077] Hereinafter, the optical waveguide element of the present invention will be described in detail using preferred examples.
[0078] like Figure 6 and 7 As shown, the optical waveguide element of the present invention comprises: a first substrate 1 having a first optical waveguide 10 and a low refractive index layer 11, the low refractive index layer 11 covering the first optical waveguide 10 and being made of a material having a lower refractive index than the first optical waveguide; and a second substrate 2 bonded to the first substrate 1, being made of a material having an electro-optical effect and having a rib-type optical waveguide 20 as a second optical waveguide, the optical waveguide element having a portion where the first optical waveguide 10 and the second optical waveguide 20 are optically coupled to each other, characterized in that, when the optical waveguide element is viewed from above, a convex portion 23 is formed on the second substrate at a boundary portion where the first optical waveguide and the second substrate overlap, and the thickness of the second substrate 2 at the convex portion 23 is thinner than the thickness of the second substrate 2 at the second optical waveguide 20.
[0079] In the optical waveguide element of the present invention, the first optical waveguide is described mainly with SiN waveguide, and the second substrate is described mainly with TFLN, but the present invention is not limited to these materials. For example, Si waveguide can also be used as the first optical waveguide. However, the optical waveguide element of the present invention can be more preferably used in the case where the refractive index difference between the material used for the first optical waveguide and the material used for the second optical waveguide is small. For example, when considering the case where the refractive index of SiN is in the range of 1.5 to 2.0 and the refractive index of LN is 2.1 to 2.3, it is more preferable to use the present invention when the refractive index difference is 0.8 or less. The following description will focus on the case where SiN is used, but in the case of pure SiN, the refractive index can be adjusted to 1.5 to 2.0 according to the density, but the refractive index of a sparsely dense film is easily changed due to the mixing of water. Therefore, the SiN of the present invention may also contain silicon oxynitride (SiON) whose composition can be adjusted.
[0080] Figure 6 is a plan view showing an example of the optical waveguide element of the present invention, Figure 7 yes Figure 6 When the first optical waveguide 10 is formed by a SiN waveguide, SiN is arranged on the first optical waveguide (core), and a cladding portion is formed by a material having a lower refractive index than the SiN of the core so as to cover the periphery. For example, the first substrate 1 is formed by forming the core of the optical waveguide by SiN, and the cladding portion is formed by forming the cladding portion by a material having a lower refractive index than the SiN of the core. 2 A cladding portion 11 is formed to cover the core portion 10. The cladding portion 11 is referred to as a low-refractive index layer.
[0081] In the present invention, the substrate including the first optical waveguide 10 is referred to as the first substrate 1. However, the first substrate includes not only the first optical waveguide 10 and the low refractive index layer 11 covering the first optical waveguide 10, but also a holding substrate 12 for improving the mechanical strength of the entire substrate. As the holding substrate, Si, SiO 2 .
[0082] The second substrate 2 bonded to the first substrate 1 is made of a thin plate of a material having an electro-optical effect, such as lithium niobate (LN), lithium tantalate (LT), or PLZT (lead lanthanum zirconate titanate). Hereinafter, the description will focus on TFLN.
[0083] A rib-type optical waveguide 20 is formed on the surface of the second substrate 2 as a second optical waveguide. The first optical waveguide 10 and the second optical waveguide have the following structure: Figure 6 The overlapping portion shown in the top view is used to transfer light waves between the first optical waveguide and the second optical waveguide. The shape of the overlapping portion will be described in detail later.
[0084] As a feature of the optical waveguide element of the present invention, Figure 6 As shown in FIG. 1 , when the optical waveguide element is viewed from above, a convex portion 23 is formed on the second substrate 2 at the boundary where the first optical waveguide 10 overlaps the second substrate 2. Figure 7 As shown in FIG. 1 , the thickness of the second substrate 2 at the protrusion 23 is thinner than the thickness of the second substrate 2 at the second optical waveguide 20. Figure 6 In the embodiment, the convex portion 23 is formed only at the edge of the second substrate near the first optical waveguide 10, but the present invention is not limited thereto. For example, the convex portion 23 may be formed as follows: Fig.10 As shown, a protrusion 23 is integrally formed on the edge of the second substrate.
[0085] In the optical waveguide element of the present invention, the height of the convex portion 23 is lowered to suppress the scattering of the light waves propagating in the first optical waveguide 10 due to the convex portion 23. By setting it at least lower than the height of the second optical waveguide 20, the generation of light loss is suppressed. In addition, as for a part of the first optical waveguide 10 and a portion arranged on the lower side of the convex portion 23, the effective refractive index is increased compared with other portions, and light confinement is enhanced, thereby reducing the scattering of light waves caused by the convex portion. Specifically, as Figure 6 The width of the optical waveguide is set wide as indicated by reference numeral 100. In this specification, reference numeral 10 denotes the first optical waveguide, reference numeral 100 denotes the portion that becomes wider near the edge of the second substrate, and reference numeral 101 denotes the portion of the first optical waveguide located below the second substrate.
[0086] Furthermore, regarding the shape of the convex portion 23, the length of the first optical waveguide 10 in the propagation direction of the light wave at the convex portion 23 is preferably set to 2 μm or less. By setting it within such a range, the light loss can be further suppressed. The details will be described later.
[0087] Next, use Figure 8 and Fig. 9 , the manufacturing process of the optical waveguide element of the present invention is described. It should be noted that the following optical waveguide element uses SiN waveguide and TFLN.
[0088] (Step 1)
[0089] Prepare Figure 8 The lower side of (a) shows a first substrate 1 including a SiN waveguide. The SiN 101 is covered with a low refractive index layer 11 and supported by a holding substrate 12 .
[0090] (Step 2)
[0091] TFLN having a thickness of about 0.5 μm is prepared as the second substrate 2. TFLN is bonded to the holding member 25 via a release layer 24. Specific examples of the material of the release layer include WOx and the like.
[0092] (Step 3)
[0093] The SiN waveguide (first substrate) is bonded to the TFLN (second substrate) (refer to Figure 8 (a) and (b)). The joining method can be direct joining or resin bonding, but Figure 8 In (b), it is described as direct bonding. Direct bonding is also described in Non-Patent Document 6.
[0094] (Step 4)
[0095] The peeling layer 24 is side-etched by using an appropriate chemical solution or the like (see Figure 8 (c)). When the WOx is side-etched by a chemical solution, the etching solution is preferably a mixture of ammonia water and hydrogen peroxide water. Moreover, when the side etching is performed by dry etching, a fluorine-based gas such as SF6 or XeF2 can also be used as an etching gas. At this time, the amount of side etching is arbitrary, but it is preferably greater than the thickness of the peeling layer 24.
[0096] (Step 5)
[0097] On the above sample, an appropriate processing inhibition film PR2 (refer to Fig. 9(d)). Matters required for film formation require a film forming method with step coverage. Specifically, it is sputtering film forming, and "step coverage = thinnest part film thickness / flat part film thickness" (the ratio of the film thickness of the thinnest part to the film thickness of the flat part) is set to about 0.5. Usually, the step coverage of vacuum evaporation is around 0, but the step coverage can be improved by increasing the pressure during film formation. When the material with high dry etching resistance described later is used for film formation, the step coverage is preferably less than 0.5.
[0098] Among the materials used for the processing inhibition film PR2, there can be cited materials that can obtain an appropriate selectivity during TFLN processing and materials that will not be removed simultaneously when the stripping layer is side-etched. Specifically, when the stripping layer is WOx, Cr or the like is preferably used. Moreover, after TFLN processing, commercialization can also be performed while the processing inhibition film is still retained. In this case, as a film material, the condition that no light absorption occurs and the condition that the refractive index is lower than that of SiN and LN become additional conditions. As a specific material for the processing inhibition film, Al 2 O 3 、SiO 2 , HfO 2 ,GeO 2 etc. However, the material of the processing inhibition film varies depending on the dry etching conditions of TFLN, so it is not limited to the above materials. The thickness of the processing inhibition film PR2 needs to be the thickness inside the range that is not processed to include not only the SiN waveguide (SiN) but also a part of the low refractive index layer 11 with SiN as the core and functioning as the cladding part during the processing when the TFLN waveguide is formed. The thickness of the processing inhibition film PR2 on the upper part of the edge part with TFLN is sufficient, and it is preferred that the substrate 2 of TFLN is exposed after the TFLN waveguide is formed.
[0099] (Step 6)
[0100] The release layer 24 is removed by using an appropriate chemical solution or the like, and the holding member is peeled off (see Fig. 9 (e)). The peeling can also be performed by the chemical solution used in step 4.
[0101] (Step 7)
[0102] A resist is applied to a substrate "SiN waveguide substrate with TFLN" in which TFLN is bonded to a substrate (101, 11, 12) containing a SiN waveguide 101, to form a resist pattern PR3. The pattern is aligned with respect to the SiN waveguide 101. Here, the resist PR3 does not need to cover (overhang) the outer periphery of the TFLN (second substrate 2). The resist PR3 is a resist for protecting the TFLN and is a resist for forming the rib-type optical waveguide 20 on the TFLN (see Fig. 9(f)). For example, in Figure 3 When the optical waveguide element is suspended as in (b), the thickness of the second substrate under the resist PR3 is the same as the thickness of the second substrate at the rib type optical waveguide 20. It has been difficult to make the height of the convex portion of the edge of the second substrate lower than that of the rib type optical waveguide, which is a characteristic of the optical waveguide element of the present invention.
[0103] (Step 8)
[0104] The TFLN is dry-etched using the resist pattern PR3 as a mask, thereby forming a rib-type optical waveguide 20 on the TFLN (see Fig. 9 (g)). The thickness of the processing suppression film PR2 at the edge of the TFLN is thinner than the film thickness on the SiN waveguide, so after the TFLN waveguide is formed, the LN is sometimes exposed. This state forms a size relationship of "thickness of the TFLN rib-type optical waveguide 20" > "thickness of the TFLN convex portion 23" > "thickness of the TFLN processed portion 21", which is also a preferred state from the viewpoint of suppressing light loss in the optical waveguide.
[0105] Fig.10 (a) is a top view showing a portion of the optical waveguide element made by the above-mentioned manufacturing process. The processing inhibition film PR2 is in a state where it remains outside the convex portion 23 of the TFLN. Moreover, the thickness of the convex portion 23 is thinner than the thickness of the rib-type optical waveguide 20, and thicker than the processed portion 21 that is mainly processed. Furthermore, even when using the SiN waveguide 10 with weak light confinement, the light scattering near the edge of the TFLN is the same as that of the Si waveguide. Therefore, a portion of the SiN waveguide 10 uses a waveguide width (100) with strong light confinement.
[0106] The light transfer from the SiN waveguide 10 to the TFLN rib-type optical waveguide 20 is performed by lowering the effective refractive index by setting the SiN waveguide width to a continuously narrowing tapered shape 10A, and increasing the effective refractive index by setting the other TFLN rib-type optical waveguide 20 to a continuously widening tapered shape 20A. The effective refractive indexes of both are equal, thereby performing the light transfer.
[0107] exist Fig.10 In the embodiment (b), the manufacturing tolerance is taken into consideration, and stable light transfer can be performed even when the mutual positional relationship between the SiN waveguide 10 and the rib type optical waveguide 20 is slightly deviated in the left-right direction of the drawing. Fig.11 The specific change of the width of the optical waveguide is shown in FIG. Fig.11 Thus, at the tapered portion 20B of the TFLN rib-type optical waveguide 20, the SiN waveguide 10 is an optical waveguide 10B of a constant width whose effective refractive index does not change, and by crossing the effective refractive indexes of the waveguides, low-loss light transfer and manufacturing tolerance can be ensured.
[0108] The following describes specific design conditions for achieving low-loss light transfer between the SiN waveguide and the TFLN rib-type optical waveguide.
[0109] First, if Fig.12 As shown in (a), a structure in which TFLN2 is mounted on the SiN waveguide 10 from the middle can be considered. When light is incident on the SiN waveguide, the refractive index changes sharply at the edge of TFLN2, so the light is scattered. The loss at this time is based on Fig.12 (b) and Fig.12 The refractive distribution of (c) can be calculated by the overlap integral of the light in the waveguide.
[0110] The SiN waveguide thickness (h) was fixed at 0.5 μm, and the SiN waveguide width (w), the distance between the SiN waveguide and the TFLN (d), and the TFLN thickness (t) were set as parameters varying within the following numerical ranges. The optical loss caused by TFLN loading was calculated. Fig.13 The calculation was performed at a wavelength of 1.55 μm and TE mode.
[0111] w=0.4~1.6μm
[0112] d=0.1~0.5μm
[0113] t=0.05~0.25μm
[0114] according to Fig.13 The larger the distance d between the SiN waveguide and the TFLN, the smaller the interaction between the SiN waveguide and the TFLN, and thus the smaller the optical loss. Similarly, the smaller the thickness t of the TFLN, the smaller the optical loss. It should be noted that when the SiN waveguide width w is increased, the optical loss decreases, and when it becomes 1.2μm or more, it becomes a constant value.
[0115] therefore, Fig.14 The figure shows the contour lines of light loss (overlap integral) when the SiN waveguide width w is fixed at 1.4 μm and t and d are used as parameters.
[0116] When the optical loss caused by TFLN loading is set to less than 0.1 dB, the linear approximation is Fig.14 If the 0.1dB line is obtained, the following relationship holds true.
[0117] t≤0.29d+0.072
[0118] Among them, the SiN film is set as a non-stoichiometric composition (SiNx, x≠1.33), or the refractive index can be changed by changing the density. Furthermore, LN can not only be a non-stoichiometric composition, but also the refractive index can be adjusted by impurity doping (Mg, Zn, etc.). Therefore, the condition for the above formula to be established is that the SiN film is a stoichiometric composition and LN is only a consistent melting composition.
[0119] Next, a state where a rib-type structure is added to TFLN is considered. A case where a directional coupler is used for optical connection between the SiN waveguide 10 and the rib-type optical waveguide 20 of TFLN will be described.
[0120] Fig.15 (a) shows a perspective view of the simulated structure. Fig.15 (b) is a top view of the structure, which also records the size marks of each waveguide. The width of the light incident part of the SiN waveguide is fixed to SiN_w1 = 0.8μm, and the width of the SiN waveguide at the edge of the loaded TFLN is thickened to SiN_w2 = 1.4μm. This is to suppress the light loss at the edge of the TFLN. Since the width of the SiN waveguide on the inner side of the TFLN is narrowed to SiN_w3, the light propagating in the SiN waveguide is affected by the TFLN.
[0121] Regarding the upper TFLN rib waveguide 20, the length of the region interacting with the SiN waveguide 10 (101) is DC_L, and the width of the rib waveguide is LN_w1. Then, the width of the rib waveguide 20 is increased to LN_w2 = 1.0 μm to confine light within the waveguide. Fig.15 (c) and (d) show Fig.15 (b) is a cross-sectional view at the dashed lines EE and FF. The thickness of the SiN waveguide is fixed at h = 0.5 μm, and the thickness of the upper cladding is set to d. The thickness of the TFLN LN_t = 0.5 μm corresponds to the thickness of the rib-type structure core.
[0122] In addition, the remaining thickness of TFLN in the portion processed into the rib-shaped structure is t.
[0123] In this structure, Fig.16 (a) shows the result of calculation with DC_L as the parameter while SiN_w3=1.0 μm, LN_w1=0.75 μm, d=0.3 μm, t=0.1 μm. The parameters used in the calculation are shown in Table 1.
[0124]
Table 1
[0125] Parameter Table
[0126] symbol value meaning SiN_w1 0.8μm Incident SiN waveguide width SiN_w2 1.4μm SiN waveguide width at the TFLN loading interface SiN_w3 1.0μm Width of SiN waveguide in directional coupling section DC_L 8.0μm Coupling length of directional coupler LN_w1 0.75μm Width of TFLN rib waveguide in directional coupling section LN_w2 1.0μm Width of TFLN rib waveguide at output side d 0.3μm The gap between SiN waveguide and TFLN rib waveguide width h 0.5μm SiN waveguide thickness LN_t 0.5μm TFLN rib waveguide thickness t 0.1μm TFLN rib waveguide residual film thickness
[0127] Fig.16 The vertical axis of (a) is the value of the outgoing light amount (the amount of outgoing light emitted from the TFLN rib-type optical waveguide) divided by the incident light amount (the amount of incident light incident on the SiN waveguide). The coupling length is set to DC_L = 8.0μm, from which it can be seen that the transmittance becomes 95% (0.2dB). For reference, Fig.16 (b) shows the wavelength dependence (1500 to 1600 nm) when the coupling length DC_L=8.0 μm.
[0128] Furthermore, it is conceivable that a convex portion is formed on the edge of the TFLN. Fig.17 (a) shows a stereogram of the simulated structure, Fig.17 (b) shows a top view, Fig.17 (c) shows a cross-sectional view taken along the dashed line GG in the top view. Fig.15 The size symbols used are Fig.17 The same is true in FIG. 1 , except that the convex portion 23 at the edge of TFLN is different. Fig.17 As described in (c), it is described by the length LN_L in the direction of light propagation and the thickness LN_h.
[0129] Fig.18 In this structure, Fig.15 The parameters used (Table 1) are fixed, and the optical loss is calculated using LN_h and LN_L as parameters. When the upper limit of the optical loss is set to 0.5 dB, LN_h < 0.17 μm or LN_L < 1.2 μm. Furthermore, when the upper limit of the optical loss is 1.0 dB, LN_h < 0.21 μm or LN_L < 2.0 μm. That is, the length of the light wave propagation direction of the SiN waveguide at the protrusion 23 is preferably 2 μm or less.
[0130] The above description describes the bonding of SiN waveguide and TFLN at the chip level. The manufacturing process used in the present invention can also be implemented at the wafer level. It should be noted that the numbers of the following steps are the same as Figure 8 and 9 The number of the manufacturing process step is associated with the manufacturing process step.
[0131] (Step 1)
[0132] Prepare a substrate containing a SiN waveguide.
[0133] (Step 2-1)
[0134] like Fig.19 As in (a), TFLN2 with a release layer 24 is prepared.
[0135] (Step 2-2)
[0136] like Fig.19 As in (b), a through hole is formed in a portion of the TFLN that will become an edge. Si deep drilling processing, laser processing, etc. used in MEMS are preferred.
[0137] (Step 2-3)
[0138] like Fig.19 As in (c), unnecessary portions of the holding member 25 supporting the TFLN 2 are removed by an appropriate method (mechanical processing such as dry etching, laser processing, and cutting).
[0139] (Step 3)
[0140] like Fig.19 After cleaning the wafer, the wafer with the SiN waveguide is bonded to the wafer. At this time, the edge of the TFLN is adjusted to the wide part of the SiN waveguide (refer to Figure 6 100).
[0141] (Step 4)
[0142] like Fig.19 As in (e), the peeling layer 24 is side-etched through the through hole.
[0143] (Step 5)
[0144] The processing inhibition film PR2 is formed. (Refer to Fig. 9 (d)
[0145] (Step 6)
[0146] The peeling layer 24 is completely peeled off. Fig. 9 (e)
[0147] (Steps 7 and 8)
[0148] The difficult-to-process part PR3 is formed into a film, and the rib-type optical waveguide 20, the convex part 23, etc. are processed (refer to Fig. 9 (f) and (g)). Then, electrode formation is performed.
[0149] According to the above-mentioned manufacturing process, it can be seen that the optical waveguide element of the present invention can be manufactured at the wafer level.
[0150] Next, a method of using TFLN only in the action portion of the Mach-Zehnder optical waveguide (the portion where the electric field of the electrode acts on the optical waveguide) when the optical waveguide element of the present invention is used as an optical modulator will be described.
[0151] (Step 1)
[0152] like Fig. 20 As in (a), a SiN waveguide 10 is prepared.
[0153] (Steps 2, 3)
[0154] like Fig. 20 As in (b), the substrate with TFLN 2 (including the holding member and the peeling layer, referred to as "substrate with TFLN") is bonded to the substrate with SiN waveguide 10 formed thereon (including the low refractive index layer 11). At this time, the length of the wide portion 100 of the SiN waveguide becomes the manufacturing tolerance with respect to the "dimensions of the substrate with TFLN" and the "bonding accuracy".
[0155] (Steps 4, 5, 6)
[0156] The release layer is side-etched, e.g. Fig. 20 The processing inhibiting film PR2 is formed as in (c). The release layer is removed and the holding member is peeled off.
[0157] (Step 7)
[0158] like Fig. 20 As in (d) of FIG. 1 , the resist (difficult-to-process material) PR3 is patterned. Positioning during patterning is performed on the formation position of the rib-type optical waveguide and the portion to be protected by the substrate on which the SiN waveguide is formed.
[0159] (Step 8)
[0160] like Fig. 20 As in (e), the TFLN is processed to remove the processing inhibiting film PR2 and the difficult-to-process material PR3. Although the state where the recessed portions RC are formed above and below the MZ structure is described, there is no problem even if these portions are processed because there is no waveguide.
[0161] Then, electrodes and the like are formed.
[0162] Next, an example of applying the optical waveguide element of the present invention to an optical modulator and an optical transmitter is described. Below, an example of a high bandwidth coherent driver modulator (HB-CDM) is used for description, but the present invention is not limited to this, and can also be applied to an optical phase modulator, an optical modulator with a polarization wave synthesis function, an optical waveguide element integrating more or less Mach-Zehnder optical waveguides, a junction device that is joined to an optical waveguide element made of other materials such as silicon, a device for sensor use, and the like.
[0163] like Fig.21As shown, the optical waveguide element has an optical waveguide composed of a SiN waveguide 10 and a rib-type optical waveguide 20, and a control electrode (not shown) such as a modulation electrode for modulating the light wave propagating in the rib-type optical waveguide 20, which is accommodated in a housing CA. Furthermore, by providing an optical fiber (F) for inputting and outputting light waves with respect to the optical waveguide, an optical modulation device MD can be formed. Fig.21 In the optical fiber F, an optical block having an optical lens, a lens barrel, a polarization combining unit OB, etc. are used to optically couple with the SiN waveguide 10 in the optical waveguide element. Not limited to this, the optical fiber can be introduced into the housing through a through hole penetrating the side wall of the housing, and the optical component or substrate can be directly joined to the optical fiber, or the optical fiber having a lens function at the end of the optical fiber can be optically coupled to the optical waveguide in the optical waveguide element. Moreover, in order to stably perform the connection with the optical fiber and the optical block, a reinforcing member (not shown) can be overlapped and arranged along the end face of the substrate (including the low refractive index layer 11) containing the SiN waveguide. The polarization combining unit OB can replace the space system with a waveguide by applying the waveguide structure described in non-patent document 3 to the SiN waveguide, and can suppress the manufacturing and component costs.
[0164] By connecting an electronic circuit (digital signal processor DSP) that outputs a modulation signal So that causes the optical modulator MD to perform a modulation operation to the optical modulator MD, an optical transmitter OTA can be constructed. In order to obtain the modulation signal S applied to the optical waveguide element, it is necessary to amplify the modulation signal So output from the digital signal processor DSP. Fig.21 In the embodiment, the drive circuit DRV is used to amplify the modulated signal. The drive circuit DRV and the digital signal processor DSP can be configured outside the housing CA or inside the housing CA. In particular, by configuring the drive circuit DRV inside the housing, the propagation loss of the modulated signal from the drive circuit can be further reduced.
[0165] The input light L1 to the optical modulation device MD may be supplied from outside the optical transmission device OTA, but may also be supplied as follows. Fig.21 As shown, a semiconductor laser (LD) is used as a light source. Output light L2 modulated by the light modulator MD is output to the outside through an optical fiber F.
[0166] Industrial Applicability
[0167] As described above, according to the present invention, it is possible to provide an optical waveguide element capable of transferring light between the two with low loss even when the difference in refractive index between the two is reduced, such as in the case of SiN waveguides and TFLN rib-type optical waveguides. Furthermore, it is possible to provide an optical modulation device and an optical transmission device using the optical waveguide element.
Claims
1. An optical waveguide component, comprising: A first substrate having a first optical waveguide and a low refractive index layer, wherein the low refractive index layer covers the first optical waveguide and is made of a material with a lower refractive index than the first optical waveguide; and The second substrate is bonded to the first substrate and is made of a material having an electro-optical effect and has a rib-type optical waveguide as a second optical waveguide. The first optical waveguide and the second optical waveguide have portions that are optically coupled to each other, and the optical waveguide element is characterized in that: When the optical waveguide element is viewed from above, a convex portion is formed on the second substrate at a boundary portion where the first optical waveguide overlaps the second substrate, and the thickness of the second substrate at the convex portion is thinner than the thickness of the second substrate at the second optical waveguide.
2. The optical waveguide element according to claim 1, wherein The length of the first optical waveguide at the convex portion in the propagation direction of the light wave is 2 μm or less.
3. The optical waveguide element according to claim 1, wherein: The width of the first optical waveguide at the boundary portion is set to be wider than the width of the first optical waveguide located in the front section or the rear section of the boundary portion.
4. The optical waveguide element according to claim 1, wherein A difference in refractive index between the first optical waveguide and the second optical waveguide is 0.8 or less.
5. The optical waveguide element according to claim 4, characterized in that The first optical waveguide is made of SiN, and the second substrate is made of lithium niobate.
6. An optical modulation device, characterized in that: The optical waveguide element according to any one of claims 1 to 5 is housed in a housing, The optical modulation device includes an optical fiber that inputs or outputs a light wave with respect to the first optical waveguide.
7. The optical modulation device according to claim 6, characterized in that: The second substrate has a modulation electrode, the modulation electrode is used to modulate the light wave propagating in the second optical waveguide, An electronic circuit is provided inside the housing, and the electronic circuit amplifies a modulation signal input to the modulation electrode.
8. An optical transmission device, characterized in that: have: The light modulation device according to claim 7; a light source for inputting light waves into the light modulation device; and The electronic circuit outputs a modulation signal to the optical modulation device.