Method for manufacturing solder mask ink for packaging substrate and packaging substrate

By optimizing the coating and vacuum flattening parameters, combining the replacement of the coating wheel and the use of specific leveling agents, the problem of color difference in the anti-welding ink of the packaging substrate is solved, and product quality and production efficiency are improved and costs are reduced.

CN118741890BActive Publication Date: 2024-12-03SHENZHEN HEMEIJINGYI TECH CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411187763.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-28
Publication Date
2024-12-03
Estimated Expiration
2044-08-28

AI Technical Summary

Technical Problem

In the prior art, the welding-proof ink of the packaging substrate is prone to color aberration problems during the production process, resulting in product scrapping and production costs.

Method used

By optimizing the coating pressure, coating speed and vacuum flattening parameters, combined with the replacement of the coating wheel, the copper surface leveling agent of sodium persulfate-sulfuric acid and super-coarse micro-etching agent are used to perform ink plug holes and vacuum flattening. Ensure uniformity and quality of the ink layer.

Benefits of technology

It effectively avoids the color difference problem of the ink layer, improves product yield, reduces production costs, and ensures uniformity of the coating effect.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118741890B_ABST
    Figure CN118741890B_ABST
Patent Text Reader

Abstract

The present invention discloses a method for making solder mask ink for a packaging substrate and a packaging substrate, and relates to the technical field of packaging substrates. The method comprises: obtaining a packaging substrate to be solder masked; after leveling the copper surface, roughening the copper surface, and plugging the holes with ink; coating the packaging substrate to be solder masked with a first coating wheel, performing a pre-bake after the first coating, and then coating the substrate with a second coating wheel in two stages, and performing a pre-bake after the second coating; vacuum flattening with a vacuum press, exposing and developing after vacuum flattening; baking and ultraviolet irradiation of the ink layer; detecting the thickness difference between the two end parts and the middle part of the first coating wheel or the second coating wheel, and when the thickness difference reaches a preset thickness, or when the frequency of use of the first coating wheel or the second coating wheel reaches a preset frequency, replacing the first coating wheel or the second coating wheel. The method according to the embodiment of the present invention can improve the problem of color difference in solder mask ink.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of packaging substrates, and in particular to a method for manufacturing solder mask ink for a packaging substrate and the packaging substrate. Background Art

[0002] Solder mask inks are divided into green paint and black paint, and solder mask processes are divided into dry and wet types. The dry ink process uses dry film solder mask, while the wet ink process uses liquid ink. For the wet ink process, there is often a risk of ink color difference on the substrate during the production process. The color difference of green paint is relatively obvious, while the color difference of black paint is relatively small. In the actual production process, it is found that there is a color difference on the substrate surface of a single product, or there is a color difference in the solder mask ink between different batches of products, or there is a color difference in the solder mask ink between strips of the same batch of products. These solder mask color difference problems may cause product scrapping, reduce product yield, and increase product production costs. Summary of the invention

[0003] The present invention aims to solve at least one of the technical problems existing in the prior art. To this end, the present invention provides a method for preparing solder mask ink for a packaging substrate and a packaging substrate, which can improve the problem of color difference of the solder mask ink.

[0004] On the one hand, a method for manufacturing a solder mask ink for a package substrate according to an embodiment of the present invention comprises the following steps:

[0005] Obtain the package substrate to be solder-proofed;

[0006] After the copper surface of the package substrate to be solder-proof is leveled, the copper surface is roughened;

[0007] Performing ink plugging on the holes of the package substrate to be solder-proofed;

[0008] According to the preset ink thickness, the first coating wheel is used to coat the package substrate to be solder-proof at a first coating pressure and a first coating speed, and the package substrate to be solder-proof is pre-baked for a period of time after the first coating period. The second coating wheel is used to coat the package substrate to be solder-proof at a second coating pressure and a second coating speed, and the package substrate to be solder-proof is pre-baked for a period of time after the second coating period. The mesh number of the first coating wheel is greater than the mesh number of the second coating wheel, and the material of the two end portions of the first coating wheel and the second coating wheel is different from that of the middle portion, and the wear resistance of the two end portions of the first coating wheel and the second coating wheel is higher than that of the middle portion. The first coating pressure is less than the second coating pressure, and the first coating speed is less than the second coating speed.

[0009] Determine vacuum flattening parameters according to the preset ink thickness, and vacuum flatten the solder mask package substrate after the second stage pre-baking according to the vacuum flattening parameters by a vacuum press;

[0010] Exposing and developing the to-be-solder-resist package substrate after vacuum flattening to form ink layers on both sides of the to-be-solder-resist package substrate;

[0011] The ink layer is baked and irradiated with ultraviolet rays to form a solder mask layer of the solder mask packaging substrate;

[0012] Detect the thickness difference between the two end portions and the middle portion of the first coating wheel or the second coating wheel, and replace the first coating wheel or the second coating wheel when the thickness difference reaches a preset thickness or when the use frequency of the first coating wheel or the second coating wheel reaches a preset frequency.

[0013] According to some embodiments of the present invention, the step of roughening the copper surface after leveling the copper surface of the package substrate to be solder-proof includes:

[0014] Using a copper surface leveler of sodium persulfate-sulfuric acid to level the copper surface of the anti-solder packaging substrate to reduce the copper surface height difference;

[0015] An ultra-roughening micro-etching agent is used to form a microscopic rough copper surface on the flattened copper surface, and the anti-soldering packaging substrate is pickled. The ultra-roughening micro-etching agent includes formic acid, sulfuric acid, copper compounds and persulfate.

[0016] According to some embodiments of the present invention, the step of plugging the holes of the package substrate to be solder-proof with ink comprises:

[0017] Performing ink plugging on the holes of the package substrate to be solder-proofed;

[0018] The anti-solder packaging substrate to be prepared after the ink plugging holes is subjected to tunnel pre-baking, and is left to stand for a preset time after tunnel pre-baking to discharge the gas in the holes; wherein the tunnel pre-baking temperature is 75°C-85°C, the tunnel pre-baking time is 10-25 minutes, and the preset time is 45-75 minutes.

[0019] According to some embodiments of the present invention, the mesh number of the first coating wheel is 500P, and the mesh number of the second coating wheel is 300P.

[0020] According to some embodiments of the present invention, the step of exposing and developing the vacuum flattened package substrate to be solder-resistant and forming an ink layer on both sides of the package substrate to be solder-resistant includes:

[0021] Exposing the light-curable ink on both sides of the solder mask packaging substrate after vacuum flattening to cure the light-curable ink in the exposed part to form a polymer;

[0022] The solder mask packaging substrate is developed by using a developer to remove the unexposed portion of the light-curable ink.

[0023] According to some embodiments of the present invention, the step of baking and ultraviolet irradiation on the ink layer to form a solder mask layer of the package substrate to be solder-resistant comprises:

[0024] The ink layer is baked at a temperature of 150° C. to solidify the thermosetting resin component of the ink layer;

[0025] The ink layer is irradiated with ultraviolet rays; the energy of the ultraviolet rays is 1400-2200 MJ.

[0026] According to some embodiments of the present invention, the adjustment range of the vacuum flattening parameters is: vacuum temperature is 95±5°C, vacuum time is 15-30s, vacuum degree is 0.8-1.4hpa, flattening temperature is 100±5°C, flattening time is 25-50s, vacuum pressure is 0.4-1.6Mpa, and flattening pressure is 0.8-2.0Mpa. By adjusting the vacuum flattening parameters, the ink surface is flattened with an R value of ≤4um.

[0027] According to some embodiments of the present invention, the vacuum press includes an upper film pressing mechanism and a lower film pressing mechanism, the upper film pressing mechanism includes an upper roller and an upper hot plate, the lower film pressing mechanism includes a lower roller and a lower hot plate, the upper roller and the upper hot plate are at the same height in the horizontal direction, and the lower roller and the lower hot plate are at the same height in the horizontal direction; when the vacuum press performs vacuum flattening on the package substrate to be solder-proof, the package substrate to be solder-proof is placed between the upper film pressing mechanism and the lower film pressing mechanism, and a first flattening steel plate is arranged between the package substrate to be solder-proof and the upper film pressing mechanism, and a second flattening steel plate is arranged between the package substrate to be solder-proof and the lower film pressing mechanism.

[0028] According to some embodiments of the present invention, the package substrate to be solder-proofed after vacuum flattening is exposed by eight exposure lamp sources to improve exposure uniformity, so that the exposure uniformity is greater than 99.5%.

[0029] On the other hand, according to the packaging substrate of the embodiment of the present invention, solder resist ink is provided on both sides of the packaging substrate, and the solder resist ink is manufactured by the manufacturing method of the solder resist ink of the packaging substrate described in the above embodiment.

[0030] The method for preparing the solder mask ink for the packaging substrate and the packaging substrate according to the embodiments of the present invention have at least the following beneficial effects: by optimizing the coating pressure, coating speed and vacuum flattening parameters, the quality of the ink is improved, ensuring that there is no color difference in the ink layer on the surface of the packaging substrate, thereby ensuring the quality of the product, improving the product yield and reducing the production cost; at the same time, by optimizing and replacing the coating wheel, the coating effect of the coating wheel is guaranteed, making the coating effect more uniform and avoiding color difference.

[0031] Additional aspects and advantages of the present invention will be given in part in the following description and in part will be obvious from the following description, or will be learned through practice of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] The above and / or additional aspects and advantages of the present invention will become apparent and easily understood from the description of the embodiments in conjunction with the following drawings, in which:

[0033] Figure 1 A flowchart of the steps of a method for manufacturing solder mask ink for a packaging substrate according to an embodiment of the present invention;

[0034] Figure 2 A flowchart of some steps of a method for making solder mask ink for a package substrate according to an embodiment of the present invention;

[0035] Figure 3 A flowchart of some steps of a method for making solder mask ink for a package substrate according to an embodiment of the present invention;

[0036] Figure 4 The present invention is a flowchart of some steps of a method for manufacturing solder mask ink for a packaging substrate according to an embodiment of the present invention. DETAILED DESCRIPTION

[0037] Embodiments of the present invention are described in detail below, and examples of the embodiments are shown in the accompanying drawings, wherein the same or similar reference numerals throughout represent the same or similar elements or elements having the same or similar functions. The embodiments described below with reference to the accompanying drawings are exemplary and are only used to explain the present application, and are not to be construed as limitations on the present application. For the step numbers in the following embodiments, they are only provided for the convenience of explanation, and the order between the steps is not limited in any way, and the execution order of each step in the embodiment can be adaptively adjusted according to the understanding of those skilled in the art.

[0038] In the description of the present invention, it should be understood that descriptions involving orientations, such as up, down, front, back, left, right, etc., and orientations or positional relationships indicated are based on the orientations or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present invention and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as a limitation on the present invention.

[0039] The terms "first", "second", "third" and "fourth" etc. in the specification and claims of the present invention and the drawings are used to distinguish different objects, rather than to describe a specific order. In addition, the terms "including" and "having" and any variations thereof are intended to cover non-exclusive inclusions. For example, a process, method, system, product or device that includes a series of steps or units is not limited to the listed steps or units, but may optionally include steps or units that are not listed, or may optionally include other steps or units that are inherent to these processes, methods, products or devices.

[0040] Reference to "embodiments" in the present invention means that a particular feature, structure, or characteristic described in conjunction with the embodiments may be included in at least one embodiment of the present invention. The appearance of the phrase in various places in the specification does not necessarily refer to the same embodiment, nor is it an independent or alternative embodiment that is mutually exclusive with other embodiments. It is explicitly and implicitly understood by those skilled in the art that the embodiments described herein may be combined with other embodiments.

[0041] Solder mask inks are divided into green paint and black paint, and solder mask processes are divided into dry and wet types. The dry ink process uses dry film solder mask, while the wet ink process uses liquid ink. For the wet ink process, there is often a risk of ink color difference on the substrate during the production process. The color difference of green paint is relatively obvious, while the color difference of black paint is smaller. In the actual production process, it is found that there is a color difference on the substrate surface of a single product, or there is a color difference in the solder mask ink between different batches of products, or there is a color difference in the solder mask ink between strips of the same batch of products. These solder mask color difference problems may cause the product to be scrapped, reduce product yield, and increase product production costs.

[0042] To this end, an embodiment of the present invention provides a method for preparing a solder mask ink for a packaging substrate and a packaging substrate, which improves the quality of the ink by optimizing the coating pressure, coating speed and vacuum flattening parameters, ensures that there is no color difference in the ink layer on the surface of the packaging substrate, guarantees the quality of the product, improves the product yield and reduces the production cost; at the same time, by optimizing and replacing the coating wheel, the coating effect of the coating wheel is guaranteed, making the coating effect more uniform and avoiding color difference.

[0043] The following describes in detail a method for manufacturing solder mask ink for a packaging substrate and a packaging substrate according to an embodiment of the present invention in conjunction with the accompanying drawings.

[0044] On the one hand, the present invention provides a method for preparing a solder mask ink for a packaging substrate, such as Figure 1 As shown, the method comprises the following steps:

[0045] Step S100: obtaining a package substrate to be solder-proofed;

[0046] Among them, the packaging substrate to be solder-proof refers to the packaging substrate that has completed the production of inner and outer layer circuits, but has not yet produced the solder mask layer; generally speaking, after the existing packaging substrate / circuit board has completed the production of the circuit, it is necessary to produce a solder mask layer on both sides of the packaging substrate to play the role of solder resistance and protection; the solder mask layer is also called the green oil layer, which is the non-wiring layer of the packaging substrate. The solder mask is applied to the places where soldering is not required. This is because the solder is fluid at high temperature when soldering the packaging substrate, so a layer of solder mask must be applied to the places where soldering is not required to prevent the solder from flowing and overflowing and causing a short circuit.

[0047] Step S200: After the copper surface of the solder mask package substrate is leveled, the copper surface is roughened;

[0048] Before roughening the copper surface, it is necessary to level the copper surface first to reduce the copper surface height difference and improve the subsequent roughening effect and solder mask effect. Then, the copper surface is roughened again to generate a microscopic rough copper surface on the copper surface to improve the bonding strength between the copper surface and the ink.

[0049] Specifically, Figure 2 As shown, step S200 includes the following two steps:

[0050] Step S210: using a copper surface leveler of sodium persulfate-sulfuric acid to level the copper surface of the solder mask packaging substrate to reduce the copper surface height difference;

[0051] Step S220: using an ultra-roughening micro-etching agent to form a microscopic rough copper surface on the flattened copper surface, and pickling the solder mask packaging substrate, wherein the ultra-roughening micro-etching agent includes formic acid, sulfuric acid, copper compounds and persulfate.

[0052] By using a leveling agent of sodium persulfate-sulfuric acid, a good leveling effect is achieved, and the copper surface of the solder mask packaging substrate can be effectively leveled, thereby reducing the copper surface drop and improving the subsequent roughening effect and solder mask effect. By using an ultra-roughening micro-etching agent containing formic acid, sulfuric acid, copper compounds and persulfate, a good micro-etching effect is achieved, which can effectively form a microscopic rough copper surface on the leveled copper surface and improve the bonding force between the copper surface and the ink. After roughening, the solder mask packaging substrate needs to be pickled to remove copper surface oxides and residual roughening solutions to avoid affecting subsequent processes and product quality; 4±1% hydrochloric acid can be used for pickling.

[0053] Step S300: plugging holes of the solder mask packaging substrate with ink;

[0054] Before making ink layers on both sides of the solder mask packaging substrate, it is necessary to plug the solder mask packaging substrate with ink first. The purpose of ink plugging is to: prevent the tin from penetrating the component surface from the via hole during wave soldering to cause a short circuit; avoid flux residue in the via hole; prevent the surface solder paste from flowing into the hole to cause cold soldering and affect mounting; prevent the tin balls from popping out during wave soldering to cause a short circuit.

[0055] After the solder mask packaging substrate is plugged with ink, it is necessary to perform tunnel pre-baking on the solder mask packaging substrate. After tunnel pre-baking, let it stand for a preset time to discharge the gas in the hole; wherein, the temperature of the tunnel pre-baking is 75°C-85°C, the time of the tunnel pre-baking is 10-25 minutes, and the preset time is 45-75 minutes. The ink is solidified by tunnel pre-baking; after pre-baking, let it stand for 45-75 minutes to discharge the gas in the hole.

[0056] Step S400: According to the preset ink thickness, the first coating wheel is used to coat the substrate to be solder masked with a first coating pressure and a first coating speed, and the substrate to be solder masked with a first pre-bake is performed after the first coating. Then, the second coating wheel is used to coat the substrate to be solder masked with a second coating pressure and a second coating speed, and the substrate to be solder masked with a second pre-bake is performed after the second coating. The mesh number of the first coating wheel is greater than the mesh number of the second coating wheel, and the material of the two end parts of the first coating wheel and the second coating wheel is different from that of the middle part, and the wear resistance of the two end parts of the first coating wheel and the second coating wheel is higher than that of the middle part. The first coating pressure is less than the second coating pressure, and the first coating speed is less than the second coating speed.

[0057] In this example, the ink is applied on both sides of the solder mask packaging substrate to form an ink layer by coating; coating is to extrude the surface of the solder mask packaging substrate by a coating wheel, and the production is controlled by the amount of ink carried by the coating wheel, which is an automated coating production operation. It should be noted that for different ink thicknesses, the coating pressure and coating speed need to be adaptively adjusted so that the coating pressure and coating speed match the ink thickness to improve the coating effect and prevent the color difference of the green paint caused by the thin thickness of the solder mask ink in locations with higher pressure and faster speed. Therefore, it is necessary to test the influence of different coating pressures and coating speeds on the color difference of different ink thicknesses, so as to optimize the coating pressure and coating speed according to the required ink thickness. During the coating process, the coating is divided into two stages, wherein the first stage of coating is carried out by the first coating wheel at the first coating pressure and the first coating speed, and the second stage of coating is carried out by the second coating wheel at the second coating pressure and the second coating speed; it should be noted that the first stage of coating requires more ink, and the second stage of coating requires less ink, therefore, the first coating pressure and the first coating speed are both less than the second coating pressure and the second coating speed, so that the coating is more uniform, and the coating color difference is prevented. At the same time, during the coating process, the two ends of the coating wheel are obviously more severely worn than the middle, the two ends of the coating wheel are severely worn, and the lines on the coating wheel are worn, because the main function of the lines is to drive the ink to be coated on the substrate during printing. If the lines are worn, the ink coated on the substrate will become less, resulting in less ink on both sides of the substrate, and the paint surface is thin and presents color difference. To this end, in this example, the material of the two end parts of the first coating wheel and the second coating wheel is different from that of the middle part, so that the wear resistance of the two end parts of the first coating wheel and the second coating wheel is higher than that of the middle part, so that the wear degree of the two end parts of the first coating wheel and the second coating wheel is close to the wear degree of the middle part, avoiding the difference between the amount of ink on both sides of the substrate and the amount of ink in the middle during the coating process, thereby improving the problem of color difference. In addition, in this example, the mesh number of the first coating wheel is greater than the mesh number of the second coating wheel. For example, the mesh number of the first coating wheel is 500P, and the mesh number of the second coating wheel is 300P. The mesh number of the coating wheel refers to the number of grooves per inch on the wheel surface, usually expressed in LPI (lines per inch). The higher the mesh number, the denser the grooves, and the more notches on the coating wheel surface. The mesh number of the coating wheel has an important influence on the coating quality. First of all, a coating wheel with a high mesh number can provide a higher cutting force, so that the coating material is better attached to the wheel surface, thereby achieving a more uniform coating. Therefore, since the coating requirements of the first coating stage are higher, the mesh number of the first coating wheel is greater than the mesh number of the second coating wheel to ensure uniform coating.

[0058] After the first stage of coating, tunnel pre-baking is required. The pre-baking temperature is about 80℃ and the pre-baking time is 10-25min. After the second stage of coating, tunnel pre-baking is required. The pre-baking temperature is about 80℃ and the second stage of baking time is 50-80min. The second stage of baking time is much longer than the first stage, so that all the ink after coating can be initially solidified.

[0059] Step S500: determining vacuum flattening parameters according to a preset ink thickness, and vacuum flattening the solder mask package substrate after the second stage pre-baking according to the vacuum flattening parameters by a vacuum press;

[0060] During vacuum flattening, the vacuum flattening parameters are optimized according to different board thicknesses and ink thicknesses to make the surface more uniform after coating and improve the color difference of the green paint after vacuum flattening. In order to obtain suitable vacuum flattening parameters, multiple tests can be conducted for different board thicknesses and ink thicknesses to determine the optimal vacuum parameters corresponding to each board thickness and ink thickness. During vacuum flattening, the vacuum press uses a release film for flattening. For different release films, the surface roughness of the film is different, and the glossiness of the pressed ink surface is different. The best release film can be selected, and vacuum pressing can be performed by pressurizing and heating, thereby improving the flatness and glossiness of the ink and reducing the color difference of the green paint caused by the ink thickness R value.

[0061] In addition, the vacuum flattening technology is optimized. The vacuum press includes an upper film pressing mechanism and a lower film pressing mechanism. The upper film pressing mechanism includes an upper roller and an upper hot plate. The lower film pressing mechanism includes a lower roller and a lower hot plate. The upper roller and the upper hot plate have the same height in the horizontal direction, and the lower roller and the lower hot plate have the same height in the horizontal direction. When the vacuum press performs vacuum flattening on the anti-solder packaging substrate, the anti-solder packaging substrate is placed between the upper film pressing mechanism and the lower film pressing mechanism, and a first flattening steel plate is arranged between the anti-solder packaging substrate and the upper film pressing mechanism, and a second flattening steel plate is arranged between the anti-solder packaging substrate and the lower film pressing mechanism. Among them, the upper roller and the lower roller are used for film pressing, and the upper hot plate and the lower hot plate are used for heating during the flattening process to ensure the effect of vacuum flattening. A high-flatness flattening steel plate is used, and the parallelism of the flattening roller is adjusted. The upper and lower side rollers are embedded above and below the axis, and the rollers are adjusted horizontally to the same height as the upper and lower hot plates, thereby further improving the effect of vacuum flattening. The carrier film (PE film) is driven by the upper and lower rollers of the vacuum flattening machine. The first stage is heated and pressurized under vacuum to fill the gaps between the patterns and obtain a substrate with no bubbles and good filling condition. Then, the concave and convex substrate is reheated in the second stage to make the ink flow and pressurize to flatten the surface.

[0062] In this example, the vacuum flattening parameters are adjusted accordingly according to different ink thicknesses. The adjustment range of the vacuum flattening parameters is: vacuum temperature is 95±5℃, vacuum time is 15-30s, vacuum degree is 0.8-1.4hpa, flattening temperature is 100±5℃, flattening time is 25-50s, vacuum pressure is 0.4-1.6Mpa, and flattening pressure is 0.8-2.0Mpa. By adjusting the vacuum flattening parameters, the ink surface is flattened with an R value of ≤4um.

[0063] Step S600: exposing and developing the package substrate to be solder masked after vacuum flattening to form ink layers on both sides of the package substrate to be solder masked;

[0064] After vacuum flattening, the solder mask package substrate is exposed and developed to solidify the light-curable ink in the exposed part to form a polymer and fade the ink in the unexposed part.

[0065] Specifically, Figure 3 As shown, in this example, step S600 includes the following two steps:

[0066] Step S610: exposing the light-curable ink on both sides of the solder mask package substrate to be flattened by vacuum to cure the light-curable ink in the exposed part to form a polymer;

[0067] Step S620: Develop the solder mask packaging substrate with a developer to remove the unexposed portion of the light-curable ink.

[0068] Among them, the developer can use sodium carbonate or the like to wash the ink and dissolve the unexposed ink, thereby removing the unexposed ink. During exposure, the vacuum flattened solder mask package substrate is exposed through eight exposure light sources to improve the exposure uniformity, making the exposure uniformity greater than 99.5%, and improving the uniformity of 90% to more than 99.5%. By controlling the illuminance value of the eight exposure light sources, the effect of the solder mask exposure light energy on the color difference of the green paint illumination appearance is solved.

[0069] Step S700: baking and irradiating the ink layer with ultraviolet light to form a solder mask layer of the package substrate to be solder masked.

[0070] After exposure and development, the ink layer of the anti-solder packaging substrate is baked to solidify the resin of the ink layer, and then the ink is irradiated with ultraviolet rays to increase the curing degree of the ink, so that the ink forms a solder mask layer of the anti-solder packaging substrate.

[0071] Specifically, Figure 4 As shown, in this example, step S700 includes the following two steps:

[0072] Step S710: baking the ink layer at a temperature of 150° C. to solidify the thermosetting resin component of the ink layer;

[0073] Step S720: irradiate the ink layer with ultraviolet light; the energy of the ultraviolet light is 1400-2200 MJ.

[0074] At a high temperature of 150°C, after a long period of baking, the resin of the ink layer will slowly harden and cure, and then the ink is irradiated with ultraviolet light, the energy of which is 1400-2200MJ, thereby increasing the degree of curing of the ink.

[0075] Step S800: Detect the thickness difference between the two end portions and the middle portion of the first coating wheel or the second coating wheel. When the thickness difference reaches a preset thickness, or when the usage frequency of the first coating wheel or the second coating wheel reaches a preset frequency, replace the first coating wheel or the second coating wheel.

[0076] In the case where the first coating wheel and the second coating wheel are used more frequently, there may be a certain thickness difference between the two end parts and the middle part of the first coating wheel and the second coating wheel. When the thickness difference reaches the preset thickness, it will affect the coating uniformity and cause the paint color difference. Therefore, when the thickness difference reaches the preset thickness, the first coating wheel or the second coating wheel needs to be replaced. At the same time, when the frequency of use of the first coating wheel or the second coating wheel reaches the preset frequency, at this time, the overall degree of wear is heavy, and the first coating wheel and the second coating wheel need to be replaced in time to ensure the coating effect. In this example, when the frequency of use of the coating wheel reaches 13000PNL, the coating wheel is replaced once, that is, the coating wheel needs to be replaced every time it coats 13,000 substrates. In addition, after the first coating wheel and the second coating wheel are used a certain number of times (less than 13000PNL), their coating pressure and coating speed can be optimized according to their wear degree to ensure that the packaging substrates of the same batch of products do not have color difference.

[0077] Therefore, according to the method for preparing the solder mask ink for the packaging substrate of the embodiment of the present invention, the coating pressure, coating speed and vacuum flattening parameters are optimized to improve the quality of the ink, ensure that there is no color difference in the ink layer on the surface of the packaging substrate, ensure the quality of the product, improve the product yield and reduce the production cost; at the same time, by optimizing and replacing the coating wheel, the coating effect of the coating wheel is guaranteed, making the coating effect more uniform and avoiding color difference.

[0078] On the other hand, the present invention further proposes a packaging substrate, wherein solder resist ink is provided on both sides of the packaging substrate, and the solder resist ink is manufactured by the method for manufacturing the solder resist ink for the packaging substrate described in the above-mentioned embodiment.

[0079] On the other hand, an embodiment of the present invention further provides an electronic device, including:

[0080] A memory for storing program instructions;

[0081] The processor is used to call the program instructions stored in the memory and execute the method for making the solder resist ink of the packaging substrate according to the obtained program instructions.

[0082] The processor may be implemented by a general-purpose central processing unit (CPU), a microprocessor, an application-specific integrated circuit (ASIC), or one or more integrated circuits, and is used to execute relevant programs to implement the technical solutions provided in the embodiments of the present application;

[0083] The memory can be implemented in the form of a read-only memory (ROM), a static storage device, a dynamic storage device, or a random access memory (RAM). The memory can store an operating system and other applications. When the technical solution provided in the embodiments of this specification is implemented by software or firmware, the relevant program code is stored in the memory, and the processor calls and executes the method for making solder mask ink for a package substrate in the embodiments of this application; the memory and the processor can be connected through a bus or the like.

[0084] On the other hand, an embodiment of the present invention further provides a storage medium, which is a computer-readable storage medium and stores a computer program. When the computer program is executed by a processor, the method for manufacturing the solder mask ink for the packaging substrate is implemented.

[0085] As a non-transient computer-readable storage medium, the memory can be used to store non-transient software programs and non-transient computer executable programs. In addition, the memory may include a high-speed random access memory, and may also include a non-transient memory, such as at least one disk storage device, a flash memory device, or other non-transient solid-state storage devices. In some embodiments, the memory may optionally include a memory remotely arranged relative to the processor, and these remote memories may be connected to the processor via a network. Examples of the above-mentioned networks include, but are not limited to, the Internet, an intranet, a local area network, a mobile communication network, and a combination thereof. The device embodiments described above are merely schematic, wherein the units described as separate components may or may not be physically separated, and are implemented to be located in one place, or may also be distributed to multiple network units. Some or all of the modules may be selected according to actual needs to achieve the purpose of the present embodiment.

[0086] Although specific embodiments are described herein, those of ordinary skill in the art will recognize that many other modifications or alternative embodiments are also within the scope of the present disclosure. For example, any of the functions and / or processing capabilities described in conjunction with a particular device or component may be performed by any other device or component. In addition, although various exemplary implementations and architectures have been described according to embodiments of the present disclosure, those of ordinary skill in the art will recognize that many other modifications to the exemplary implementations and architectures described herein are also within the scope of the present disclosure.

[0087] Some aspects of the present disclosure are described above with reference to the block diagram and flow chart of the system, method, system and / or computer program product according to the exemplary embodiments.It should be understood that the combination of one or more blocks in the block diagram and the flow chart and the blocks in the block diagram and the flow chart can be realized by executing computer executable program instructions respectively.Equally, according to some embodiments, some blocks in the block diagram and the flow chart may not need to be executed in the order shown, or may not need to be executed in full.In addition, additional components and / or operations beyond those components and / or operations shown in the blocks in the block diagram and the flow chart may be present in certain embodiments.

[0088] Therefore, the blocks in the block diagrams and flow charts support the combination of devices for performing the specified functions, the combination of elements or steps for performing the specified functions, and the program instruction devices for performing the specified functions. It should also be understood that each block in the block diagrams and flow charts and the combination of blocks in the block diagrams and flow charts can be implemented by a special-purpose hardware computer system or a combination of special-purpose hardware and computer instructions that performs a specific function, element or step.

[0089] The program modules, applications, etc. described herein may include one or more software components, including, for example, software objects, methods, data structures, etc. Each such software component may include computer-executable instructions that, in response to execution, cause at least a portion of the functionality described herein (e.g., one or more operations of the illustrative methods described herein) to be performed.

[0090] Software components can be encoded with any of various programming languages. An exemplary programming language can be a low-level programming language, such as an assembly language associated with a specific hardware architecture and / or an operating system platform. The software component comprising assembly language instructions may need to be converted to executable machine code by an assembler before being executed by hardware architecture and / or platform. Another exemplary programming language can be a higher-level programming language, which can be transplanted across multiple architectures. The software component comprising a higher-level programming language may need to be converted to an intermediate representation by an interpreter or a compiler before execution. Other examples of programming languages ​​include but are not limited to macro languages, shells or command languages, job control languages, scripting languages, database queries or search languages ​​or report writing languages. In one or more exemplary embodiments, the software component comprising the instruction of one of the above-mentioned programming language examples can be directly executed by an operating system or other software components, without first being converted into another form.

[0091] Software components may be stored as files or other data storage structures. Software components of similar type or related functions may be stored together, such as in a specific directory, folder, or library. Software components may be static (e.g., preset or fixed) or dynamic (e.g., created or modified at execution time).

[0092] The embodiments of the present invention are described in detail above with reference to the accompanying drawings, but the present invention is not limited to the above embodiments, and various changes can be made within the knowledge scope of ordinary technicians in the relevant technical field without departing from the purpose of the present invention.

Claims

1. A method for preparing solder mask ink for a packaging substrate, characterized in that: The following steps are involved: Obtain the package substrate to be solder-proofed; After the copper surface of the package substrate to be solder-proof is leveled, the copper surface is roughened; Performing ink plugging on the holes of the package substrate to be solder-proofed; According to the preset ink thickness, the first coating wheel is used to coat the package substrate to be solder-proof at a first coating pressure and a first coating speed, and the package substrate to be solder-proof is pre-baked for a period of time after the first coating period. The second coating wheel is used to coat the package substrate to be solder-proof at a second coating pressure and a second coating speed, and the package substrate to be solder-proof is pre-baked for a period of time after the second coating period. The mesh number of the first coating wheel is greater than the mesh number of the second coating wheel, and the material of the two end portions of the first coating wheel and the second coating wheel is different from that of the middle portion, and the wear resistance of the two end portions of the first coating wheel and the second coating wheel is higher than that of the middle portion. The first coating pressure is less than the second coating pressure, and the first coating speed is less than the second coating speed. Determine vacuum flattening parameters according to the preset ink thickness, and vacuum flatten the solder mask package substrate after the second stage pre-baking according to the vacuum flattening parameters by a vacuum press; Exposing and developing the to-be-solder-resist package substrate after vacuum flattening to form ink layers on both sides of the to-be-solder-resist package substrate; The ink layer is baked and irradiated with ultraviolet rays to form a solder mask layer of the solder mask packaging substrate; Detect the thickness difference between the two end portions and the middle portion of the first coating wheel or the second coating wheel, and replace the first coating wheel or the second coating wheel when the thickness difference reaches a preset thickness or when the use frequency of the first coating wheel or the second coating wheel reaches a preset frequency.

2. The method for preparing the solder resist ink for the package substrate according to claim 1, characterized in that: After the copper surface of the solder mask package substrate is leveled, the step of roughening the copper surface comprises: Using a copper surface leveler of sodium persulfate-sulfuric acid to level the copper surface of the anti-solder packaging substrate to reduce the copper surface height difference; An ultra-roughening micro-etching agent is used to form a microscopic rough copper surface on the flattened copper surface, and the anti-soldering packaging substrate is pickled. The ultra-roughening micro-etching agent includes formic acid, sulfuric acid, copper compounds and persulfate.

3. The method for preparing the solder resist ink for the package substrate according to claim 1, characterized in that: The step of plugging the holes of the package substrate to be solder-proof with ink comprises: Performing ink plugging on the holes of the package substrate to be solder-proofed; The anti-solder packaging substrate to be prepared after the ink plugging holes is subjected to tunnel pre-baking, and is left to stand for a preset time after tunnel pre-baking to discharge the gas in the holes; wherein the tunnel pre-baking temperature is 75°C-85°C, the tunnel pre-baking time is 10-25 minutes, and the preset time is 45-75 minutes.

4. The method for preparing the solder resist ink for the package substrate according to claim 1, characterized in that: The mesh number of the first coating wheel is 500P, and the mesh number of the second coating wheel is 300P.

5. The method for preparing the solder resist ink for the package substrate according to claim 1, characterized in that: The step of exposing and developing the vacuum flattened package substrate to be solder masked and forming ink layers on both sides of the package substrate to be solder masked comprises: Exposing the light-curable ink on both sides of the solder mask packaging substrate after vacuum flattening to cure the light-curable ink in the exposed part to form a polymer; The solder mask packaging substrate is developed by using a developer to remove the unexposed portion of the light-curable ink.

6. The method for preparing the solder resist ink for the package substrate according to claim 1, characterized in that: The step of baking and ultraviolet irradiation on the ink layer to form a solder mask layer of the solder mask packaging substrate to be solder masked comprises: The ink layer is baked at a temperature of 150° C. to solidify the thermosetting resin component of the ink layer; The ink layer is irradiated with ultraviolet rays; the energy of the ultraviolet rays is 1400-2200 MJ.

7. The method for preparing solder mask ink for packaging substrate according to claim 1, characterized in that: The vacuum press includes an upper film pressing mechanism and a lower film pressing mechanism, the upper film pressing mechanism includes an upper roller and an upper heating plate, the lower film pressing mechanism includes a lower roller and a lower heating plate, the upper roller and the upper heating plate are at the same height in the horizontal direction, and the lower roller and the lower heating plate are at the same height in the horizontal direction; when the vacuum press performs vacuum flattening on the package substrate to be solder-proof, the package substrate to be solder-proof is placed between the upper film pressing mechanism and the lower film pressing mechanism, and a first flattening steel plate is arranged between the package substrate to be solder-proof and the upper film pressing mechanism, and a second flattening steel plate is arranged between the package substrate to be solder-proof and the lower film pressing mechanism.

8. The method for preparing solder mask ink for packaging substrate according to claim 1, characterized in that: The vacuum flattened package substrate to be solder-proof is exposed by eight exposure lamp sources to improve exposure uniformity, so that the exposure uniformity is greater than 99.5%.

9. A packaging substrate, characterized in that: Solder resist ink is provided on both sides of the packaging substrate, and the solder resist ink is manufactured by the method for manufacturing solder resist ink for a packaging substrate according to any one of claims 1 to 8.

Citation Information

Patent Citations

  • Solder mark coating wheel and solder mark coating machine

    CN109569952A

  • Method for improving thickness of printing ink at orifice of thin plate plug hole

    CN116546730A

  • Solder mask optimization method and device for substrate

    CN117202527A

  • A method of printing ink on a substrate

    KR1019990047917A