Laminated structure, semiconductor element, and semiconductor device

By constructing a laminated structure with a linear expansion coefficient difference of less than 2.0 ppm/K between the semiconductor film and the conductive substrate, the problem of warping and cracking of the semiconductor film at high temperatures is solved, and the heat resistance and stability of the semiconductor element are improved.

CN118743031APending Publication Date: 2024-10-01FLOSFIA
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380018924.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-01-31
Filing Date
2023-01-27
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

In the laminated structure of a semiconductor film and a supporting substrate used in power devices, etc., degradation problems such as warping and cracking are prone to occur at high temperatures, resulting in reduced device performance.

Method used

Adopt a stacked structure of a crystalline oxide semiconductor layer with a specific linear expansion coefficient difference of less than 2.0ppm/K and a conductive substrate to ensure that the stacking direction is parallel or approximately parallel to the crystal axis of the semiconductor layer to reduce thermal stress caused by high temperatures. crack.

Benefits of technology

It effectively reduces the degradation of the semiconductor layer under high temperature conditions, improves the heat resistance and stability of semiconductor components, and is suitable for power device applications in high temperature environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118743031A_ABST
    Figure CN118743031A_ABST
Patent Text Reader

Abstract

Provided are a laminated structure, a semiconductor element, and a semiconductor device which are particularly useful in power devices and which reduce deterioration at high temperatures. This laminated structure is provided with at least a semiconductor layer containing a crystalline oxide semiconductor as a main component, and a conductive substrate laminated on the semiconductor layer. The laminated structure has a first direction in a plane perpendicular to a lamination direction of the laminated structure and a second direction perpendicular or substantially perpendicular to the first direction. A first linear expansion coefficient, which is a linear expansion coefficient of the conductive substrate in a first direction, is smaller than a second linear expansion coefficient, which is a linear expansion coefficient of the conductive substrate in a second direction. And a third linear expansion coefficient, which is a linear expansion coefficient of the semiconductor layer in the first direction, is smaller than a fourth linear expansion coefficient, which is a linear expansion coefficient of the semiconductor layer in the second direction.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a stacked structure, a semiconductor element, and a semiconductor device which are useful as a power device or the like. Background Art

[0002] As a next-generation switching element that can achieve high withstand voltage, low loss and high heat resistance, semiconductor devices using gallium oxide (Ga2O3) with a large band gap have attracted attention, and are expected to be used in power semiconductor devices such as inverters. In addition, due to its wide band gap, it is also expected to be used as a light-emitting device such as LEDs and sensors. According to Patent Document 1, the gallium oxide can control the band gap by mixing with indium and aluminum separately or in combination, and construct a very attractive material system as an InAlGaO-based semiconductor. Here, InAlGaO-based semiconductor refers to In X Al Y Ga Z O3 (0≤X≤2, 0≤Y≤2, 0≤Z≤2, X+Y+Z=1.5~2.5) can be regarded as the same material system containing gallium oxide.

[0003] Patent document 2 states that a semiconductor film having a corundum crystal structure and composed of α-Ga2O3 or α-Ga2O3 solid solution formed on a film-forming base substrate can be transferred to a substrate composed of a Cu-Mo composite material. In addition, in Patent document 3, metals such as Al, nitrides such as AlN, SiN, and GaN, oxides such as SiO2 and Al2O3, SiC, Si, GaAs, and diamond are described as materials for the supporting substrate of the β-Ga2O3 film. However, in the stacked structure of such a semiconductor film and a heterogeneous substrate as a supporting substrate, there are degradation problems caused by warping at high temperatures and cracks caused by stress, especially in the case of application to power devices and the like and during heating in the manufacturing process.

[0004] Patent Document 1: Japanese Patent No. 5343224

[0005] Patent Document 2: Japanese Patent No. 6784870

[0006] Patent Document 3: Japanese Patent Publication No. 2019-12836 Summary of the invention

[0007] One of the objects of the present invention is to provide a stacked structure, a semiconductor element, and a semiconductor device in which degradation at high temperatures is reduced.

[0008] As a result of intensive research conducted by the present inventors to achieve the above-mentioned object, it has been found that the following stacked structure can reduce degradation at high temperatures and solve the above-mentioned conventional problems: the stacked structure comprises at least a semiconductor layer containing a crystalline oxide semiconductor as a main component and a conductive substrate stacked on the semiconductor layer, wherein the stacked structure has a first direction and a second direction perpendicular or substantially perpendicular to the first direction in a plane perpendicular to the stacking direction of the stacked structure, a first linear expansion coefficient which is a linear expansion coefficient of the conductive substrate in the first direction is smaller than a second linear expansion coefficient which is a linear expansion coefficient of the conductive substrate in the second direction, and a third linear expansion coefficient which is a linear expansion coefficient of the semiconductor layer in the first direction is smaller than a fourth linear expansion coefficient which is a linear expansion coefficient of the semiconductor layer in the second direction. In addition, the stacked structure has been found to be particularly useful in semiconductor elements and semiconductor devices such as power devices.

[0009] Furthermore, after obtaining the above-mentioned knowledge, the present inventors further conducted repeated studies and finally completed the present invention.

[0010] That is, the present invention relates to the following technical solutions.

[0011] [1] A stacked structure comprising at least a semiconductor layer containing a crystalline oxide semiconductor as a main component and a conductive substrate stacked on the semiconductor layer, characterized in that the stacked structure has a first direction and a second direction perpendicular or substantially perpendicular to the first direction in a plane perpendicular to the stacking direction of the stacked structure, a first linear expansion coefficient which is the linear expansion coefficient of the conductive substrate in the first direction is smaller than a second linear expansion coefficient which is the linear expansion coefficient of the conductive substrate in the second direction, and a third linear expansion coefficient which is the linear expansion coefficient of the semiconductor layer in the first direction is smaller than a fourth linear expansion coefficient which is the linear expansion coefficient of the semiconductor layer in the second direction.

[0012] [2] The laminated structure according to [1] above, wherein a difference between the first linear expansion coefficient and the second linear expansion coefficient is 2.0 ppm / K or less.

[0013] [3] The laminated structure according to [1] or [2] above, wherein the second linear expansion coefficient is 10 ppm / K or less.

[0014] [4] A stacked structure according to any one of the above [1] to [3], wherein the crystalline oxide semiconductor includes at least a first crystal axis and a second crystal axis, and the linear expansion coefficient in the direction of the first crystal axis is smaller than the linear expansion coefficient in the direction of the second crystal axis, and the stacking direction of the stacked structure is parallel or approximately parallel to the first crystal axis.

[0015] [5] The stacked structure according to [4] above, wherein the crystalline oxide semiconductor has a corundum structure.

[0016] [6] The stacked structure according to [5] above, wherein the first crystal axis is the m-axis.

[0017] [7] The stacked structure according to [1] or [6] above, wherein the first direction of the semiconductor layer is an a-axis direction, and the second direction of the semiconductor layer is a c-axis direction.

[0018] [8] The stacked structure according to any one of [1] to [7] above, wherein the crystalline oxide semiconductor contains at least one metal selected from aluminum, indium, and gallium.

[0019] [9] The stacked structure according to any one of [1] to [8] above, wherein the crystalline oxide semiconductor contains at least gallium.

[0020]

[10] The laminated structure according to any one of [1] to [9] above, wherein the conductive substrate has a thickness of 200 μm or less.

[0021]

[11] A semiconductor device comprising at least: the stacked structure according to any one of [1] to

[10] above; and an electrode.

[0022]

[12] A semiconductor device comprising at least a semiconductor element bonded to a lead frame, a circuit substrate, or a heat dissipation substrate via a bonding component, wherein the semiconductor element is the semiconductor element described in

[11] .

[0023]

[13] A power conversion device using the semiconductor device described in

[12] .

[0024]

[14] A control system using the semiconductor device described in

[12] .

[0025] The laminated structure, semiconductor element and semiconductor device of the present invention improve degradation at high temperatures. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 This is a diagram showing an example of a laminate used in the embodiment of the present invention.

[0027] Figure 2 This is a diagram showing an example of an adhesive laminate used in the embodiment of the present invention.

[0028] Figure 3A diagram showing an example of a semiconductor structure used in an embodiment of the present invention.

[0029] Figure 4 This is a diagram schematically showing a suitable embodiment of the Schottky barrier diode (SBD) of the present invention.

[0030] Figure 5 This is a diagram schematically showing a suitable embodiment of the Schottky barrier diode (SBD) of the present invention.

[0031] Figure 6 This is a diagram schematically showing a suitable example of the metal oxide semiconductor field effect transistor (MOSFET) of the present invention.

[0032] Figure 7 For illustration Figure 6 Schematic diagram of a portion of a manufacturing process for a metal oxide semiconductor field effect transistor (MOSFET).

[0033] Figure 8 This is a diagram schematically showing a suitable example of the static induction transistor (SIT) of the present invention.

[0034] Fig. 9 This is a diagram schematically showing a suitable example of the Schottky barrier diode (SBD) of the present invention.

[0035] Fig.10 This is a diagram schematically showing a suitable example of the metal oxide semiconductor field effect transistor (MOSFET) of the present invention.

[0036] Fig.11 This is a diagram schematically showing a suitable example of the junction field effect transistor (JFET) of the present invention.

[0037] Fig.12 FIG. 4 is a structural diagram of an atomization CVD device used in an embodiment of the present invention.

[0038] Fig.13 A diagram schematically showing a suitable example of a semiconductor device.

[0039] Fig.14 These are images of the surfaces of the semiconductor layers after heating in Examples and Comparative Examples.

[0040] Fig.15 It is a block diagram showing an example of a control system using a semiconductor device according to an embodiment of the present invention.

[0041] Fig.16 1 is a circuit diagram showing an example of a control system using a semiconductor device according to an embodiment of the present invention.

[0042] Fig.17 It is a block diagram showing an example of a control system using a semiconductor device according to an embodiment of the present invention.

[0043] Fig.18 1 is a circuit diagram showing an example of a control system using a semiconductor device according to an embodiment of the present invention.

[0044] Fig.19 It is a figure which shows typically the upper surface of the conductive substrate concerning embodiment of this invention.

[0045] Fig. 20 It is a perspective view schematically showing a conductive substrate according to an embodiment of the present invention. DETAILED DESCRIPTION

[0046] The stacked structure of the present invention comprises at least a semiconductor layer containing a crystalline oxide semiconductor as a main component and a conductive substrate stacked on the semiconductor layer, and is characterized in that:

[0047] The stacked structure has a first direction and a second direction perpendicular or approximately perpendicular to the first direction in a plane perpendicular to the stacking direction of the stacked structure, a first linear expansion coefficient which is the linear expansion coefficient of the conductive substrate in the first direction is smaller than a second linear expansion coefficient which is the linear expansion coefficient of the conductive substrate in the second direction, and a third linear expansion coefficient which is the linear expansion coefficient of the semiconductor layer in the first direction is smaller than a fourth linear expansion coefficient which is the linear thermal expansion coefficient of the semiconductor layer in the second direction.

[0048] In an embodiment of the present invention, for example, the stacked structure can be appropriately manufactured by the following manufacturing method, the manufacturing method comprising: (1) a process of stacking the semiconductor layer directly or via other layers on a base substrate; and (3) a process of stacking the conductive substrate on the semiconductor layer via an electrode layer and / or a conductive adhesive layer as required, and removing the base substrate using a known method. Below, taking the main processes (1) to (3) of manufacturing the stacked structure as an example, a more detailed description is given using the accompanying drawings in an embodiment of the present invention.

[0049] In process (1), the semiconductor layer is stacked directly on the base substrate or with other layers interposed therebetween. By process (1), for example, Figure 1 The stack shown. Figure 1 The stacked body shown has a semiconductor layer 101 stacked on a base substrate 108. In the present invention, the crystalline semiconductor film 101 obtained in process (1) can be used as the semiconductor layer (hereinafter also referred to as "semiconductor film"). Next, process (1) is described.

[0050] (Base substrate)

[0051] The base substrate is not particularly limited as long as it is plate-shaped and is a substrate that serves as a support for the semiconductor film. It may be an insulating substrate, a semiconductor substrate, a metal substrate, or a conductive substrate, but the base substrate is preferably an insulating substrate, and is also preferably a substrate having a metal film on the surface. As the base substrate, for example, a base substrate containing a substrate material having a corundum structure as the main component, a base substrate containing a substrate material having a β-gallia structure as the main component, or a base substrate containing a substrate material having a hexagonal crystal structure as the main component can be cited. Here, the so-called "main component" means that relative to the total components of the substrate material, in terms of atomic ratio, it is preferably composed of more than 50% of the substrate material having a specific crystal structure, more preferably more than 70%, and further preferably more than 90%. The content of the substrate material having a specific crystal structure may also be 100%.

[0052] The substrate material is not particularly limited as long as it does not impair the purpose of the present invention, and can be a known material. As the substrate material having a corundum structure, for example, α-Al2O3 (sapphire substrate) or α-Ga2O3 can be appropriately listed, and a-plane sapphire substrate, m-plane sapphire substrate, r-plane sapphire substrate, c-plane sapphire substrate and α-type gallium oxide substrate (a-plane, m-plane or r-plane) can be listed as more appropriate examples. As a base substrate with a substrate material having a β-gallia structure as the main component, for example, a β-Ga2O3 substrate, or a mixed crystal substrate containing Ga2O3 and Al2O3 and Al2O3 more than 0wt% and less than 60wt%, etc. can be listed. In addition, as a base substrate with a substrate material having a hexagonal crystal structure as the main component, for example, a SiC substrate, a ZnO substrate, a GaN substrate, etc. can be listed.

[0053] The semiconductor layer is not particularly limited as long as it contains a crystalline oxide semiconductor as a main component and the linear expansion coefficient in the first direction (hereinafter also referred to as the "third linear expansion coefficient") is less than the linear expansion coefficient in the second direction (hereinafter also referred to as the "fourth linear expansion coefficient"). Here, the so-called "linear expansion coefficient" refers to the linear expansion coefficient measured according to JIS R3102 (1995). The crystal structure of the crystalline oxide semiconductor is also not particularly limited as long as it does not impair the purpose of the present invention. As the crystal structure of the crystalline oxide semiconductor, for example, a corundum structure, a β-gallia structure, a hexagonal structure (for example, an ε-type structure, etc.), a right-angle structure (for example, a κ-type structure, etc.), a cubic structure or a tetragonal structure, etc. can be listed. In an embodiment of the present invention, the crystalline oxide semiconductor preferably has a corundum structure, a β-gallia structure or a hexagonal structure (for example, an ε-type structure, etc.), and more preferably has a corundum structure. As the crystalline oxide semiconductor, for example, metal oxides containing one or more metals selected from aluminum, gallium, indium, iron, chromium, vanadium, titanium, rhodium, nickel, cobalt and iridium can be listed. In an embodiment of the present invention, the oxide semiconductor preferably contains at least one metal selected from aluminum, indium and gallium, more preferably contains at least gallium, and is preferably α-Ga2O3 or a mixed crystal thereof. It should be noted that the so-called "main component" means that the crystalline oxide semiconductor is contained in the semiconductor layer at a ratio of 0.5 or more of the atomic ratio of gallium in all the metal elements contained in the semiconductor layer. In an embodiment of the present invention, the atomic ratio of gallium in all the metal elements in the semiconductor layer is preferably 0.7 or more, more preferably 0.9 or more. In an embodiment of the present invention, it is also preferred that the crystalline oxide semiconductor contains at least a first crystal axis and a second crystal axis perpendicular or substantially perpendicular to the first crystal axis, and the linear expansion coefficient in the direction of the first crystal axis is smaller than the linear expansion coefficient in the direction of the second crystal axis, and the stacking direction of the stacked structure is parallel or substantially parallel to the first crystal axis. Here, "substantially parallel" is not limited to, for example, the case where the stacking direction of the stacked structure is parallel to the first crystal axis direction, but also includes the case where the angle formed by the stacking direction and the first crystal axis direction is less than ±10°. In addition, when the crystalline oxide semiconductor has a corundum structure, the first crystal axis is preferably the m-axis or the a-axis, and more preferably the m-axis. In addition, in this case, it is preferred that the first direction is the a-axis direction, and the second direction is the c-axis direction. It should be noted that, for example, "the first direction is the a-axis direction" is not limited to the case where the first direction is parallel to the a-axis direction, but also includes the case where the angle formed by the first direction and the a-axis direction is less than ±10°.

[0054] In addition, the thickness of the semiconductor layer is not particularly limited and may be 1 μm or less or 1 μm or more, but in the embodiment of the present invention, it is preferably 1 μm or more. In addition, the upper limit of the thickness of the semiconductor layer is not particularly limited as long as it does not impair the purpose of the present invention, but is preferably 30 μm or less. The surface area of ​​the semiconductor layer is not particularly limited and may be 1 mm 2 Above, also 1mm 2 Below, but preferably 10mm 2 ~300cm 2 , more preferably 10 mm 2 ~100cm 2 . In addition, the semiconductor layer is usually single crystal, but may also be polycrystalline. In addition, when the semiconductor layer is a multilayer film including at least a first semiconductor layer and a second semiconductor layer and a Schottky electrode is provided on the first semiconductor layer, the semiconductor layer is also preferably a multilayer film in which the carrier density of the first semiconductor layer is less than the carrier density of the second semiconductor layer. It should be noted that in this case, the second semiconductor layer usually contains a dopant, and the carrier density of the semiconductor layer can be appropriately set by adjusting the doping amount.

[0055] Fig. 20 : is a perspective view schematically showing a stacked structure including at least the conductive substrate and the semiconductor layer. Fig. 20 Although the conductive adhesive layer and the electrode layer are not shown in the figure, Fig. 20 The case where the laminated structure further includes the conductive adhesive layer and the electrode layer is also included in the embodiment of the present invention. Fig. 20 The Z direction in represents the stacking direction of the stacked structure. Fig. 20 The X direction and the Y direction in the figure represent the first direction and the second direction, respectively. In addition, the first crystal axis direction (for example, the m-axis direction or the a-axis direction) of the crystalline oxide semiconductor described above is Fig. 20 The Z direction (stacking direction) in the embodiment of the present invention is parallel or substantially parallel, and the second crystal axis direction (for example, the c-axis direction) of the crystalline oxide semiconductor is, for example, parallel to the Z direction (stacking direction) in the embodiment of the present invention. Fig. 20 The Y-axis direction is parallel or approximately parallel.

[0056] The semiconductor layer preferably contains a dopant. The dopant is not particularly limited and may be a known dopant. Examples of the dopant include n-type dopants such as tin, germanium, silicon, titanium, zirconium, vanadium or niobium, and p-type dopants such as magnesium, calcium, zinc, etc. In an embodiment of the present invention, the n-type dopant is preferably Sn, Ge or Si. In the composition of the semiconductor layer, the content of the dopant is preferably 0.00001 atomic % or more, more preferably 0.00001 atomic % to 20 atomic %, and most preferably 0.00001 atomic % to 10 atomic %. More specifically, the concentration of the dopant may generally be about 1×10 16 / cm 3 ~1×10 22 / cm 3 , and the concentration of the dopant can also be set to about 1×10 17 / cm 3 In addition, according to the present invention, it is also possible to use about 1×10 19 / cm 3 In the embodiment of the present invention, it is preferred to use 1×10 17 / cm 3 The above carrier concentrations include dopants.

[0057] The semiconductor layer may be formed by a known method. Examples of the method for forming the semiconductor layer include CVD, MOCVD, MOVPE, atomized CVD, atomized epitaxy, MBE, HVPE, pulsed growth, or ALD. In an embodiment of the present invention, the semiconductor layer is preferably formed by atomized CVD or atomized epitaxy. In the atomized CVD or atomized epitaxy, for example, Fig.12 The atomized CVD device shown atomizes the raw material solution (atomization process) to make the droplets float, and after atomization, the obtained atomized droplets are transported to the substrate by a carrier gas (transportation process), and then the atomized droplets are subjected to a thermal reaction in the film forming chamber to stack a semiconductor film containing a crystalline oxide semiconductor as a main component on the substrate (film forming process), thereby forming the semiconductor layer.

[0058] (Atomization process)

[0059] The raw material solution is atomized in the atomization process. The atomization method of the raw material solution is not particularly limited as long as it can atomize the raw material solution. It may be a known method, but in an embodiment of the present invention, an atomization method using ultrasound is preferred. The initial velocity of the atomized droplets obtained using ultrasound is zero, and they float in the air, so it is preferred. Since it is not blown like a spray, for example, but can float in space and be transported as a gas, there is no damage caused by impact energy, which is very suitable. The droplet size is not particularly limited, and may be a droplet of about several millimeters, but is preferably less than 50 μm, and more preferably 100 nm to 10 μm.

[0060] (Raw material solution)

[0061] The raw material solution is not particularly limited as long as it can be atomized or dropletized and contains a raw material capable of forming a semiconductor film, and the raw material solution may be an inorganic material or an organic material. In an embodiment of the present invention, the raw material is preferably a metal or a metal compound, and more preferably contains one or more metals selected from aluminum, gallium, indium, iron, chromium, vanadium, titanium, rhodium, nickel, cobalt and iridium.

[0062] In an embodiment of the present invention, as the raw material solution, a solution in which the metal is dissolved or dispersed in an organic solvent or water in the form of a complex or a salt can be appropriately used. As the form of the complex, for example, acetylacetone complex, carbonyl complex, amine complex, hydride complex, etc. can be listed. As the form of the salt, for example, organic metal salts (for example, metal acetates, metal oxalates, metal citrates, etc.), sulfide metal salts, nitrated metal salts, phosphated metal salts, halogenated metal salts (for example, chloride metal salts, bromide metal salts, iodide metal salts, etc.) can be listed.

[0063] In addition, it is preferred to mix additives such as hydrohalic acid and oxidizing agent in the raw material solution. As the hydrohalic acid, for example, hydrobromic acid, hydrochloric acid, hydroiodic acid, etc. can be listed, but hydrobromic acid or hydroiodic acid is preferred because they can more effectively suppress the generation of abnormal particles. As the oxidizing agent, for example, peroxides such as hydrogen peroxide (H2O2), sodium peroxide (Na2O2), barium peroxide (BaO2), benzoyl peroxide ((C6H5CO)2O2), etc., organic peroxides such as hypochlorous acid (HClO), perchloric acid, nitric acid, ozone water, peracetic acid or nitrobenzene, etc. can be listed.

[0064] The raw material solution may contain a dopant. By containing a dopant in the raw material solution, doping can be performed well. The dopant is not particularly limited as long as it does not impair the purpose of the present invention. As the dopant, for example, n-type dopants such as tin, germanium, silicon, titanium, zirconium, vanadium or niobium can be listed; or p-type dopants such as Mg, H, Li, Na, K, Rb, Cs, Fr, Be, Ca, Sr, Ba, Ra, Mn, Fe, Co, Ni, Pd, Cu, Ag, Au, Zn, Cd, Hg, Ti, Pb, N or P can be listed. The content of the dopant is appropriately set by using a calibration line that represents the relationship between the concentration of the dopant in the raw material and the desired carrier density.

[0065] The solvent of the raw material solution is not particularly limited, and may be an inorganic solvent such as water, an organic solvent such as alcohol, or a mixed solvent of an inorganic solvent and an organic solvent. In an embodiment of the present invention, the solvent preferably includes water.

[0066] (Transportation process)

[0067] In the transport process, the atomized droplets are transported into the film forming chamber by a carrier gas. As the carrier gas, there is no particular limitation as long as it does not impair the purpose of the present invention. As appropriate examples, for example, inert gases such as oxygen, ozone, nitrogen or argon can be cited; or reducing gases such as hydrogen or synthetic gas can be cited. In addition, the type of carrier gas can be one, but it can also be two or more, and a dilution gas with a reduced flow rate (for example, a 10-fold dilution gas, etc.) can be further used as a second carrier gas. In addition, the supply point of the carrier gas can also be two or more places, not just one place. Although the flow rate of the carrier gas is not particularly limited, it is preferably 0.01 to 20 L / min, and more preferably 1 to 10 L / min. In the case of a dilution gas, the flow rate of the dilution gas is preferably 0.001 to 5 L / min, and more preferably 0.1 to 3 L / min.

[0068] (Film Forming Process)

[0069] In the film forming process, the semiconductor film is formed on the substrate by causing the atomized droplets to react thermally in the film forming chamber. For the thermal reaction, as long as the atomized droplets are reacted by heat, and as long as the purpose of the present invention is not impaired, the reaction conditions are not particularly limited. In this process, the thermal reaction is usually carried out at a temperature above the evaporation temperature of the solvent, but preferably below a temperature not too high (e.g., 1000°C), more preferably below 650°C, and preferably at 300°C to 650°C. In addition, as long as the thermal reaction does not impair the purpose of the present invention, it can be carried out in any of the atmospheres of vacuum, non-oxygen atmosphere (e.g., inert gas atmosphere, etc.), reducing gas atmosphere, and oxygen atmosphere, but it is preferably carried out in an inert gas atmosphere or oxygen atmosphere. In addition, it can be carried out under any of the conditions of atmospheric pressure, pressurization, and reduced pressure, but in an embodiment of the present invention, it is preferably carried out under atmospheric pressure. It should be noted that the film thickness can be set by adjusting the film forming time.

[0070] In an embodiment of the present invention, the film forming process may be followed by an annealing treatment. The annealing temperature is not particularly limited as long as it does not impair the purpose of the present invention, and is generally 300°C to 650°C, preferably 350°C to 550°C. In addition, the annealing time is generally 1 minute to 48 hours, preferably 10 minutes to 24 hours, and more preferably 30 minutes to 12 hours. It should be noted that the annealing treatment may be carried out in any atmosphere as long as it does not impair the purpose of the present invention. It may be carried out in a non-oxygen atmosphere or in an oxygen atmosphere. As a non-oxygen atmosphere, for example, an inert gas atmosphere (for example, a nitrogen atmosphere) or a reducing gas atmosphere may be cited, but in an embodiment of the present invention, an inert gas atmosphere is preferably used, and a nitrogen atmosphere is more preferably used.

[0071] In addition, in an embodiment of the present invention, the semiconductor film may be directly disposed on the base substrate, or the semiconductor film may be disposed via other layers such as a stress relaxation layer (e.g., a buffer layer, an ELO layer, etc.), a stripping sacrificial layer, etc. The formation method of each layer is not particularly limited and may be a known method, but in an embodiment of the present invention, an atomized CVD method is preferably used.

[0072] In process (2), as required, an electrode layer 105b is formed on the semiconductor layer 101. Through process (2), for example, Figure 2 The stack shown. Figure 2 The stacked body is composed of a base substrate 108, a semiconductor layer 101 and an electrode layer 105b.

[0073] The electrode layer is not particularly limited as long as it has conductivity and does not impair the purpose of the present invention. The constituent material of the electrode layer may be a conductive inorganic material or a conductive organic material. In an embodiment of the present invention, the material of the electrode is preferably a metal. As the metal, for example, at least one metal selected from Groups 4 to 10 of the periodic table can be appropriately listed. As metals of Group 4 of the periodic table, for example, titanium (Ti), zirconium (Zr), hafnium (Hf), etc. can be listed. As metals of Group 5 of the periodic table, for example, vanadium (V), niobium (Nb), tantalum (Ta), etc. can be listed. As metals of Group 6 of the periodic table, for example, chromium (Cr), molybdenum (Mo), and tungsten (W) can be listed. As metals of Group 7 of the periodic table, for example, manganese (Mn), technetium (Tc), rhenium (Re), etc. can be listed. As metals of Group 8 of the periodic table, for example, iron (Fe), ruthenium (Ru), osmium (Os), etc. can be listed. As metals of Group 9 of the periodic table, for example, cobalt (Co), rhodium (Rh), iridium (Ir), etc. can be cited. As metals of Group 10 of the periodic table, for example, nickel (Ni), palladium (Pd), platinum (Pt), etc. can be cited. In an embodiment of the present invention, the electrode layer preferably contains at least one metal selected from Group 4 and Group 9 of the periodic table, and more preferably contains a metal of Group 9 of the periodic table. The thickness of the electrode layer is not particularly limited, but is preferably 0.1nm to 10μm, more preferably 5nm to 500nm, and most preferably 10nm to 200nm. In addition, in an embodiment of the present invention, the electrode layer may be composed of two or more layers with different compositions.

[0074] The method for forming the electrode layer is not particularly limited and can be a known method. As the method for forming the electrode layer or the other electrode layer, specifically, for example, a dry method and a wet method can be cited. As the dry method, for example, sputtering, vacuum evaporation, CVD, etc. can be cited. As the wet method, for example, screen printing and die coating can be cited.

[0075] In process (3), the conductive substrate is stacked on the electrode layer via a conductive adhesive layer as required, and the base substrate is removed by a known method. Figure 3 A laminate as shown. Figure 3The laminate shown has an electrode layer 105b bonded to a conductive substrate 107 via a conductive adhesive layer 106, and a semiconductor layer 101 is stacked on the electrode layer 105b. Examples of methods for removing the base substrate include a method of removing by applying a mechanical impact, a method of removing by applying heat and utilizing thermal stress, a method of removing by applying vibrations such as ultrasonic waves, a method of removing by etching, a method of removing by grinding, a method of removing by heat treatment after ion implantation such as smart cutting, a method of removing by laser lift-off, and a method of combining these methods.

[0076] The conductive adhesive layer is not particularly limited as long as it can bond the electrode layer and the conductive substrate. As the constituent material of the conductive adhesive layer, for example, metals selected from at least one of Al, Au, Pt, Ag, Ti, Ni, Bi, Cu, Ga, In, Pb, Sn and Zn and their metal oxides, eutectic materials (for example, Au-Sn, etc.) and the like can be cited. In an embodiment of the present invention, the conductive adhesive layer preferably has a porous structure. In addition, when the conductive adhesive layer has a porous structure, the conductive adhesive layer preferably contains metal particles, more preferably contains metal particles containing at least one metal selected from Au, Pt, Ag, Ti, Ni, Bi, Cu, Ga, In, Pb, Sn and Zn, and preferably contains metal particles containing precious metals. As the precious metal, for example, at least one metal selected from Au, Ag, Pt, Pd, Rh, Ir, Ru and Os can be cited, but in an embodiment of the present invention, the precious metal is preferably Ag. In addition, in an embodiment of the present invention, the conductive adhesive layer preferably contains a metal particle sintered body, and more preferably contains a silver particle sintered body. By using this preferred conductive adhesive layer, the adhesion between the electrode layer and the conductive substrate can be made better without damaging the electrical properties of the semiconductor element. In addition, the conductive adhesive layer may be a single layer or a multilayer. In addition, the thickness of the conductive adhesive layer is not particularly limited as long as it does not damage the purpose of the present invention, but is preferably 10nm to 200μm, and more preferably 10nm to 50μm. In addition, the conductive adhesive layer is usually amorphous, but may also contain accessory components such as crystals. It should be noted that the method for forming the conductive adhesive layer is not particularly limited and may be a known coating method.

[0077] The conductive substrate is not particularly limited as long as it has conductivity and can support the semiconductor layer, and the linear expansion coefficient in the first direction (hereinafter, also referred to as the "first linear expansion coefficient") is smaller than the linear expansion coefficient in the second direction (hereinafter, also referred to as the "second linear expansion coefficient"). In an embodiment of the present invention, the conductive substrate preferably includes at least a first metal and a second metal different from the first metal. Fig.19 The figure schematically shows the upper surface of the conductive substrate. Fig.19 The conductive substrate 107 has a first direction ( Fig.19 and a second direction perpendicular or substantially perpendicular to the first direction ( Fig.19 Y direction in the drawing). Here, the term "substantially vertical" also includes, for example, the case where the angle formed by the first direction and the second direction is 90°±10°. Here, the term "linear expansion coefficient" refers to the linear expansion coefficient measured according to JISR 3102 (1995). The difference between the first linear expansion coefficient and the second linear expansion coefficient is not particularly limited as long as it does not impair the purpose of the present invention. In an embodiment of the present invention, the difference between the first linear expansion coefficient and the second linear expansion coefficient is preferably 3.0ppm / K or less, and more preferably 2.0ppm / K or less. It should be noted that the upper limit of the second linear expansion coefficient is also not particularly limited as long as it does not impair the purpose of the present invention. The upper limit of the second linear expansion coefficient is generally 12ppm / K or less, and preferably 10ppm / K or less. By setting such a preferred configuration, even in the case where there is a difference in linear expansion coefficient between the conductive substrate and the semiconductor layer, the degradation of the semiconductor layer at high temperature can be better reduced. It should be noted that in Fig. 20 In the stacked structure shown in FIG. 1 , the first linear expansion coefficient of the conductive substrate 107 is Fig. 20 The linear expansion coefficient in the X direction, the second linear expansion coefficient of the conductive substrate 107 is Fig. 20 The linear expansion coefficient in the Y direction.

[0078] The first metal and / or the second metal are not particularly limited as long as they do not damage the purpose of the present invention. In an embodiment of the present invention, it is preferred to include a first metal and a second metal having a Young's modulus greater than the Young's modulus of the first metal, and the mass ratio of the second metal in the conductive substrate is greater than the mass ratio of the first metal. By setting it as such a preferred configuration, for example, even if there is a difference in linear expansion coefficient between the semiconductor layer and the conductive substrate, the degradation (cracks, etc.) of the semiconductor layer at high temperatures can be more effectively reduced. As a combination of the first metal and the second metal in the conductive substrate, for example, copper (Cu)-tungsten (W), copper (Cu)-molybdenum (Mo), lanthanum (La)-molybdenum (Mo), yttrium (Y)-molybdenum (Mo), rhenium (Re)-molybdenum (Mo), molybdenum (Mo)-tungsten (W), niobium (Nb)-molybdenum (Mo), tantalum (Ta)-molybdenum (Mo), etc. can be listed. In an embodiment of the present invention, it is preferred that the first metal and / or the second metal is at least one metal selected from metals of Group 6 of the periodic table and metals of Group 11 of the periodic table. As metals of the 6th group of the periodic table, for example, chromium (Cr), molybdenum (Mo) and tungsten (W) can be listed. As metals of the 11th group of the periodic table, for example, copper (Cu), silver (Ag), and gold (Au) can be listed. In an embodiment of the present invention, it is preferred that the first metal is a metal of the 11th group of the periodic table (for example, copper, etc.), and the second metal is a metal of the 6th group of the periodic table (for example, molybdenum, etc.). By setting the first metal and the second metal to this preferred combination, it is possible to better suppress degradation at high temperatures while maintaining the heat dissipation of the stacked structure or the semiconductor element. It should be noted that in an embodiment of the present invention, when the conductive substrate contains molybdenum and copper, as the conductive substrate, it is preferred to use a Cu-Mo composite substrate (hereinafter, also referred to as "Cu-Mo composite substrate") obtained by an impregnation method of impregnating copper in a molybdenum blank. In addition, in the present invention, it is also preferred that the first direction of the conductive substrate is a rolling direction.

[0079] The Young's modulus of the first metal is not particularly limited as long as it does not impair the purpose of the present invention. The Young's modulus of the first metal is generally 200 GPa or less, and is, for example, 150 GPa or less. The lower limit of the Young's modulus of the first metal is not particularly limited. In an embodiment of the present invention, the Young's modulus of the first metal is preferably 100 GPa or more. In addition, the Young's modulus of the second metal is not particularly limited as long as it does not impair the purpose of the present invention. The appropriate Young's modulus of the second metal is, for example, 300 GPa or more. The appropriate Young's modulus of the conductive substrate is, for example, 200 GPa or more. By setting this preferred configuration, even in the case where the linear expansion coefficient of the semiconductor layer and the linear expansion coefficient of the conductive substrate are different, the degradation of the semiconductor layer at high temperature can be improved more well. The mass ratio of the first metal and the second metal in the conductive substrate is not particularly limited as long as it does not impair the purpose of the present invention. In an embodiment of the present invention, the mass ratio of the second metal is preferably 60 mass % or more. The upper limit of the mass ratio of the second metal is also not particularly limited, but in an embodiment of the present invention, it is preferably 85 mass % or less, more preferably 70 mass % or less. It should be noted that the mass ratio of the first metal in the conductive substrate is usually, for example, 40% by mass or less, preferably 30% by mass or less. The lower limit of the mass ratio of the first metal is also not particularly limited. In an embodiment of the present invention, the mass ratio of the first metal is 10% by mass or more and 15% by mass or more. By setting it to such a preferred ratio, it is possible to better reduce degradation at high temperatures while maintaining heat dissipation. It should be noted that in an embodiment of the present invention, a metal film may also be provided on the surface of the conductive substrate. As the constituent metal of the metal film, for example, one or more metals selected from gallium, iron, indium, aluminum, copper, vanadium, titanium, chromium, rhodium, nickel, cobalt, zinc, magnesium, calcium, silicon, yttrium, strontium and barium can be listed. In addition, the thickness of the conductive substrate is not particularly limited, but is preferably 200 μm or less, which can give better heat dissipation without damaging the electrical characteristics of the semiconductor element, so it is preferred. In addition, the area of ​​the conductive substrate is not particularly limited, but in an embodiment of the present invention, it is preferably substantially the same as the area of ​​the semiconductor layer. It should be noted that the term “substantially the same” includes, for example, a case where the area of ​​the conductive substrate is the same as the area of ​​the semiconductor layer, and also includes a case where the ratio of the area of ​​the conductive substrate to the area of ​​the semiconductor layer is in the range of 0.9 to 1.4.

[0080] In addition, in an embodiment of the present invention, it is also preferred that a copper-containing layer is formed on the uppermost layer and the lowermost layer of the conductive substrate, respectively. By setting the conductive substrate to such a preferred configuration, the heat dissipation and mounting properties of the stacked structure when used for a semiconductor element can be further improved. In addition, when a metal of Group 11 of the periodic table is contained in the uppermost layer and / or the lowermost layer of the stacked structure, the electrode layer and the conductive substrate can be joined without using the conductive adhesive layer, and the warping and thermal resistance of the semiconductor element can be more effectively improved. In this case, for example, the copper-containing layer on the outermost surface of the electrode layer on the conductive substrate side and the copper-containing layer on the outermost surface of the conductive substrate on the electrode layer side in the stacked structure can be diffused and bonded, so that the electrode layer and the conductive substrate can be joined in an industrially advantageous manner without using the conductive adhesive layer.

[0081] In an embodiment of the present invention, after process (3), the crystal of the crystalline semiconductor film can be regrown, and a different semiconductor layer, another electrode layer, etc. can be provided on the semiconductor layer.

[0082] In an embodiment of the present invention, when the stacked structure is used in a semiconductor element, it is preferred that another electrode layer is further provided on the surface of the semiconductor layer opposite to the surface on which the electrode layer is stacked. In this way, by setting a stacked structure in which the conductive substrate, the conductive adhesive layer, the electrode layer, the semiconductor layer and the other electrode layer are stacked in sequence, the forward characteristics of the semiconductor element as a vertical device in which current flows in the thickness direction of the semiconductor layer can be made more excellent. The other electrode layer is not particularly limited as long as it has conductivity and does not impair the purpose of the present invention. The constituent material of the other electrode layer may be a conductive inorganic material or a conductive organic material. In an embodiment of the present invention, the material of the other electrode is preferably a metal. As suitable metals, for example, at least one metal selected from Groups 8 to 13 of the periodic table can be listed. As metals of Groups 8 to 10 of the periodic table, metals exemplified as metals of Groups 8 to 10 of the periodic table in the description of the electrode layer can be listed. As metals of Group 11 of the periodic table, for example, copper (Cu), silver (Ag), gold (Au), etc. can be listed. As metals of Group 12 of the periodic table, for example, zinc (Zn), cadmium (Cd), etc. can be listed. In addition, as metals of Group 13 of the periodic table, for example, aluminum (Al), gallium (Ga), indium (In), etc. can be listed. In an embodiment of the present invention, the other electrode layer preferably includes at least one metal selected from the metals of Groups 11 and 13 of the periodic table, and more preferably includes at least one metal selected from silver, copper, gold and aluminum. It should be noted that the thickness of the other electrode layer is not particularly limited, but is preferably 1 nm to 500 μm, more preferably 10 nm to 100 μm, and preferably 0.5 μm to 10 μm.

[0083] The method for forming the other electrode layer is not particularly limited and can be a known method. As the method for forming the electrode layer or the other electrode layer, specifically, for example, a dry method and a wet method can be cited. As the dry method, for example, sputtering, vacuum evaporation, CVD, etc. can be cited. As the wet method, for example, screen printing and die coating can be cited.

[0084] The stacked structure and semiconductor element of the present invention are useful in various semiconductor elements, especially in power devices. In addition, semiconductor elements can be classified into: lateral elements (lateral devices), electrodes are formed on one side of the semiconductor layer, and current flows in a direction perpendicular to the film thickness direction of the semiconductor layer; and vertical elements (vertical devices), electrodes are provided on both sides of the semiconductor layer, and current flows in the film thickness direction of the semiconductor layer. In an embodiment of the present invention, the semiconductor element can be appropriately used for lateral devices and vertical devices, but it is preferably used for vertical devices. As the semiconductor element, for example, Schottky barrier diodes (SBD), metal semiconductor field effect transistors (MESFET), high electron mobility transistors (HEMT), metal oxide film semiconductor field effect transistors (MOSFET), electrostatic induction transistors (SIT), junction field effect transistors (JFET), insulated gate bipolar transistors (IGBT) or light emitting diodes can be listed. In an embodiment of the present invention, the semiconductor element is preferably SBD, MOSFET, SIT, JFET or IGBT, more preferably SBD, MOSFET or SIT, and preferably SBD.

[0085] Below, the stacked structure is used for a semiconductor element. Suitable examples are described using the accompanying drawings, but the present invention is not limited to these embodiments. It should be noted that in the semiconductor element illustrated below, other layers (such as an insulator layer, a semi-insulator layer, a conductor layer, a semiconductor layer, a damping layer or other intermediate layer, etc.) may be further included as long as the purpose of the present invention is not impaired, and the damping layer (buffer layer) may be appropriately omitted.

[0086] (SBD)

[0087] Figure 4 An example of the Schottky barrier diode (SBD) according to the present invention is shown. Figure 4 The SBD includes an n-type semiconductor layer 101a, an n+type semiconductor layer 101b, a conductive adhesive layer 106, a conductive substrate 107, a Schottky electrode 105a, and an ohmic electrode 105b.

[0088] The materials of the Schottky electrode and the ohmic electrode may be known electrode materials, and examples of the electrode materials include: metals such as Al, Mo, Co, Zr, Sn, Nb, Fe, Cr, Ta, Ti, Au, Pt, V, Mn, Ni, Cu, Hf, W, Ir, Zn, In, Pd, Nd or Ag or their alloys; metal oxide conductive films such as tin oxide, zinc oxide, indium oxide, indium tin oxide (ITO), indium zinc oxide (IZO); organic conductive compounds such as polyaniline, polythiophene or polypyrrole; or mixtures thereof, etc. The Schottky electrode and the ohmic electrode may be formed, for example, by known methods such as vacuum evaporation or sputtering.

[0089] In an embodiment of the present invention, as the conductive substrate 107, the conductive substrate involved in the above-mentioned embodiment of the present invention is used. That is, a conductive substrate containing copper and molybdenum and having a first linear expansion coefficient that is smaller than a second linear expansion coefficient is used. In addition, the conductive substrate is stacked on the semiconductor layer in such a manner that the third linear expansion coefficient of the semiconductor layer is smaller than the fourth linear expansion coefficient. By using a conductive substrate of such a preferred structure, even when the linear expansion coefficient of the semiconductor layer in the first direction and the second direction is anisotropic, degradation of the semiconductor layer at high temperature can be reduced. In order to confirm the effect of the embodiment of the present invention, a conductive substrate 107 is prepared according to the above process. Figure 4 The structure corresponding to the semiconductor element shown is used, and a heating test is performed. Here, the following stacked structure is used in the embodiment: the stacked structure is formed by using a substrate containing a first metal (Cu) and a second metal (Mo) as a conductive substrate, and stacking a semiconductor layer whose main surface is an m-plane and the conductive substrate in such a manner that the first linear expansion coefficient is smaller than the second linear expansion coefficient and the third linear expansion coefficient is smaller than the fourth linear expansion coefficient. In addition, the following stacked structure is used in the comparative example: the stacked structure is made in the same manner as the embodiment, except that the conductive substrate is stacked on the semiconductor layer in such a manner that the first linear expansion coefficient is smaller than the second linear expansion coefficient and the third linear expansion coefficient is larger than the fourth linear expansion coefficient. The thickness of the conductive substrate is 200μm. In addition, in both the embodiment and the comparative example, the m-plane α-Ga2O3 layer is used as the semiconductor layer. The crack detection device (manufactured by SoftWorks) was used to detect the number of cracks generated in the examples and comparative examples after heating at 450°C for 60 minutes. The number of cracks generated in the comparative example was 86 more than that in the examples. It should be noted that the number of cracks generated was calculated by dividing the surface of the semiconductor layer into 289 regions and counting the number of cracks in each region as 1. Fig.142 shows images of the surface of the semiconductor layer after heating, which were taken by a crack inspection device (manufactured by SoftWorks) in the laminated structures produced under the conditions of the examples and comparative examples. Fig.14 (a) is the result corresponding to the embodiment, Fig.14 (b) is the result corresponding to the comparative example. Fig.14 It is clear that according to the embodiment of the present invention, degradation (crack generation) of the semiconductor layer at high temperature can be reduced favorably.

[0090] Figure 5 An example of the Schottky barrier diode (SBD) according to the present invention is shown. Figure 5 The SBD Figure 4 The SBD structure further includes an insulator layer 104. More specifically, it includes an n-type semiconductor layer 101a, an n+ type semiconductor layer 101b, a conductive adhesive layer 106, a conductive substrate 107, a Schottky electrode 105a, an ohmic electrode 105b, and an insulator layer 104.

[0091] As the material of the insulator layer 104, for example, GaO, AlGaO, InAlGaO, AlInZnGaO4, AlN, Hf2O3, SiN, SiON, Al2O3, MgO, GdO, SiO2 or Si3N4 etc. can be listed, but in the embodiment of the present invention, the material with corundum structure is preferably used. By using an insulator with a corundum structure for the insulator layer, the function of the semiconductor characteristics in the interface can be well exerted. The insulator layer 104 is arranged between the n-type semiconductor layer 101 and the Schottky electrode 105a. The formation of the insulator layer can be carried out by a known method such as sputtering, vacuum evaporation or CVD.

[0092] Regarding the formation and materials of Schottky electrodes and ohmic electrodes, Figure 4 The same is true for the case of SBDs. For example, known methods such as sputtering, vacuum evaporation, compression bonding, and CVD can be used to form electrodes composed of, for example, metals such as Al, Mo, Co, Zr, Sn, Nb, Fe, Cr, Ta, Ti, Au, Pt, V, Mn, Ni, Cu, Hf, W, Ir, Zn, In, Pd, Nd, or Ag, or alloys thereof; metal oxide conductive films such as tin oxide, zinc oxide, indium oxide, indium tin oxide (ITO), or indium zinc oxide (IZO); organic conductive compounds such as polyaniline, polythiophene, or polypyrrole; or mixtures thereof.

[0093] Figure 5 SBD and Figure 4 Compared with SBDs, it has better insulation properties and higher current controllability.

[0094] (MOSFET)

[0095] exist Figure 6 2 shows an example in which the semiconductor element of the present invention is a MOSFET. Figure 6 The MOSFET is a trench MOSFET, and includes an n-type semiconductor layer 131a, n+ type semiconductor layers 131b and 131c, a conductive adhesive layer 136, a conductive substrate 137, a gate insulating film 134, a gate electrode 135a, a source electrode 135b and a drain electrode 135c.

[0096] A conductive adhesive layer 136 having a thickness of, for example, 50 nm to 50 μm is formed on a conductive substrate 137. A drain electrode 135c is formed on the conductive adhesive layer 136. An n+ type semiconductor layer 131b having a thickness of, for example, 100 nm to 100 μm is formed on the drain electrode 135c, and an n- type semiconductor layer 131a having a thickness of, for example, 100 nm to 100 μm is formed on the n+ type semiconductor layer 131b. Then, an n+ type semiconductor layer 131c is further formed on the n- type semiconductor layer 131a, and a source electrode 135b is formed on the n+ type semiconductor layer 131c.

[0097] In addition, a plurality of trenches penetrating the n+ type semiconductor layer 131c and reaching the middle of the n- type semiconductor layer 131a are formed in the n- type semiconductor layer 131a and the n+ type semiconductor layer 131c. A gate electrode 135a is embedded in the trench via a gate insulating film 134 having a thickness of, for example, 10 nm to 1 μm.

[0098] When Figure 6 When the MOSFET is in the on state, a voltage is applied between the source electrode 135b and the drain electrode 135c, and a positive voltage relative to the source electrode 135b is applied to the gate electrode 135a, a channel layer is formed on the side of the n-type semiconductor layer 131a, and electrons are injected into the n-type semiconductor layer, thereby being turned on. In the off state, the voltage of the gate electrode is set to 0V, so that a channel layer cannot be formed, and the n-type semiconductor layer 131a is filled with a depletion layer, thereby being turned off.

[0099] Figure 7 express Figure 6 part of the MOSFET manufacturing process. For example, using Figure 7 The stacked body shown in (a) is formed, and an etching mask is set in a predetermined region of the n-type semiconductor layer 131a and the n+ type semiconductor layer 131c, and the etching mask is used as a mask to further perform anisotropic etching by a reactive ion etching method, such as Figure 7As shown in (b), a trench having a depth from the surface of the n+ type semiconductor layer 131c to the middle of the n- type semiconductor layer 131a is formed. Figure 7 As shown in (c), after forming a gate insulating film 134 with a thickness of, for example, 50 nm to 1 μm on the side and bottom of the groove using a well-known method such as thermal oxidation, vacuum evaporation, sputtering, or CVD, a gate electrode material such as polycrystalline silicon with a thickness less than that of the n-type semiconductor layer is formed in the groove using CVD, vacuum evaporation, sputtering, or the like.

[0100] Then, a source electrode 135b can be formed on the n+ type semiconductor layer 131c, and a drain electrode 135c can be formed on the n+ type semiconductor layer 131b by using a known method such as vacuum evaporation, sputtering, or CVD to manufacture a power MOSFET. It should be noted that the electrode materials of the source electrode and the drain electrode can be known electrode materials, and examples of the electrode materials include: metals such as Al, Mo, Co, Zr, Sn, Nb, Fe, Cr, Ta, Ti, Au, Pt, V, Mn, Ni, Cu, Hf, W, Ir, Zn, In, Pd, Nd, or Ag, or alloys thereof; metal oxide conductive films such as tin oxide, zinc oxide, indium oxide, indium tin oxide (ITO), and indium zinc oxide (IZO); organic conductive compounds such as polyaniline, polythiophene, or polypyrrole; or mixtures thereof.

[0101] The MOSFET obtained in this way has a better withstand voltage than the conventional trench MOSFET. Figure 6 , an example of a trench-type vertical MOSFET is shown, but the present invention is not limited thereto and can be applied to various MOSFET forms. Figure 6 The depth of the trench is dug downward until its depth reaches the bottom surface of the n-type semiconductor layer 131a, thereby reducing the series resistance.

[0102] (SIT)

[0103] Figure 8 An example in which the semiconductor element of the present invention is a SIT is shown. Figure 8 The SIT includes an n-type semiconductor layer 141a, n+type semiconductor layers 141b and 141c, a conductive adhesive layer 146, a conductive substrate 147, a gate electrode 145a, a source electrode 145b, and a drain electrode 145c.

[0104] A conductive support layer 147 having a thickness of, for example, 100 nm to 100 μm is formed on the drain electrode 145c, and a conductive adhesive layer 146 having a thickness of, for example, 50 nm to 50 μm is formed on the conductive support layer 147. In addition, an n+ type semiconductor layer 141b having a thickness of, for example, 100 nm to 100 μm is formed on the conductive adhesive layer 146, and an n- type semiconductor layer 141a having a thickness of, for example, 100 nm to 100 μm is formed on the n+ type semiconductor layer 141b. Then, an n+ type semiconductor layer 141c is further formed on the n- type semiconductor layer 141a, and a source electrode 145b is formed on the n+ type semiconductor layer 141c.

[0105] In addition, a plurality of trenches are formed in the n-type semiconductor layer 141a, penetrating the n+ semiconductor layer 131c and reaching the middle of the n-type semiconductor layer 131a. A gate electrode 145a is formed on the n-type semiconductor layer in the trench. Figure 8 In the on state of the SIT, a voltage is applied between the source electrode 145b and the drain electrode 145c, and a positive voltage relative to the source electrode 145b is applied to the gate electrode 145a, a channel layer is formed in the n-type semiconductor layer 141a, and electrons are injected into the n-type semiconductor layer, thereby being turned on. In the off state, the voltage of the gate electrode is set to 0V, so that a channel layer cannot be formed, and the n-type semiconductor layer is filled with a depletion layer, thereby being turned off.

[0106] In an embodiment of the present invention, Figure 7 MOSFETs are manufactured in the same way Figure 8SIT. More specifically, for example, an etching mask is set in a specified area of ​​the n-type semiconductor layer 141a and the n+ type semiconductor layer 141c, and the etching mask is used as a mask to perform anisotropic etching, for example, by reactive ion etching, to form a groove with a depth from the surface of the n+ type semiconductor layer 141c to the middle of the n-type semiconductor layer. Next, a gate electrode material such as polycrystalline silicon is formed in the groove with a thickness less than the thickness of the n-type semiconductor layer by CVD, vacuum evaporation, sputtering, etc. In addition, the SIT can be manufactured by forming a source electrode 145b on the n+ type semiconductor layer 141c and a drain electrode 145c on the n+ type semiconductor layer 141b using a known method such as vacuum evaporation, sputtering, and CVD. It should be noted that the electrode materials of the source electrode and the drain electrode can be respectively known electrode materials. Examples of the electrode materials include: metals such as Al, Mo, Co, Zr, Sn, Nb, Fe, Cr, Ta, Ti, Au, Pt, V, Mn, Ni, Cu, Hf, W, Ir, Zn, In, Pd, Nd or Ag or their alloys; metal oxide conductive films such as tin oxide, zinc oxide, indium oxide, indium tin oxide (ITO), indium zinc oxide (IZO); organic conductive compounds such as polyaniline, polythiophene or polypyrrole; or mixtures thereof, etc.

[0107] In the above example, a p-type semiconductor is not used, but the present invention is not limited to this, and a p-type semiconductor may also be used. Figures 9 to 11 Examples of using p-type semiconductors are shown in FIG. These semiconductor elements can be manufactured in the same manner as the manufacturing method of the above examples. It should be noted that the p-type semiconductor may be the same material as the n-type semiconductor and contain a p-type dopant, or may be a different p-type semiconductor.

[0108] It should be noted that a plurality of embodiments of the present invention described above may be combined, or some structural elements may be applied to other embodiments, and such forms also belong to the embodiments of the present invention.

[0109] The semiconductor element is particularly useful in power devices. As the semiconductor element, for example, a diode (for example, a PN diode, a Schottky barrier diode, a junction barrier Schottky diode, etc.) or a transistor (for example, a MESFET, etc.) can be listed, but a diode is preferred, and a Schottky barrier diode (SBD) is more preferred.

[0110] The semiconductor element involved in the embodiment of the present invention is further bonded to a lead frame, a circuit substrate, a heat dissipation substrate, etc. by a bonding component based on the above content and conventional methods and is appropriately used as a semiconductor device, especially as a power module, an inverter or a converter, and is further appropriately used in a semiconductor system using a power supply device, etc. Fig.13 A suitable example of the semiconductor device is shown in FIG. Fig.13 In the semiconductor device, both sides of the semiconductor element 500 are bonded to the lead frame, the circuit substrate or the heat dissipation substrate 502 by solder 501. With such a structure, a semiconductor device with excellent heat dissipation can be formed. It should be noted that in the embodiment of the present invention, the surroundings of the bonding parts such as solder are preferably sealed with resin.

[0111] The semiconductor element or semiconductor device of the present invention can be applied to power conversion devices such as inverters and converters to achieve the above functions. More specifically, it can be applied to diodes built into inverters and converters, thyristors as switching elements, power transistors, IGBTs (Insulated Gate Bipolar Transistors), MOSFETs (Metal-Oxide-Semiconductor Field Effect Transistors), etc. Fig.15 1 is a block diagram showing an example of a control system using a semiconductor element or a semiconductor device according to an embodiment of the present invention. Fig.16 The circuit diagram of the control system is particularly suitable for a control system installed in an electric vehicle.

[0112] like Fig.15 As shown, the control system 500 includes a battery (power source) 501, a boost converter 502, a buck converter 503, an inverter 504, a motor (driven object) 505, and a drive control unit 506, which are mounted on an electric vehicle. The battery 501 is composed of a storage battery such as a nickel-hydrogen battery and a lithium-ion battery, and can store power through charging at a charging station or regenerative energy during deceleration, and output a DC voltage required for the operation of the driving system and electrical system of the electric vehicle. The boost converter 502 is, for example, a voltage conversion device equipped with a chopper circuit, and can boost a DC voltage of, for example, 200V supplied from the battery 501 to, for example, 650V through the switching operation of the chopper circuit, and output it to the driving system such as the motor. The buck converter 503 is also a voltage conversion device equipped with a chopper circuit, but can output the DC voltage of, for example, 200V supplied from the battery 501 to, for example, about 12V, and then output it to the electric window and electric steering system or the electrical system including the on-board electrical equipment.

[0113] The inverter 504 converts the DC voltage supplied from the boost converter 502 into a three-phase AC voltage by switching operation and outputs it to the motor 505. The motor 505 is a three-phase AC motor constituting the driving system of the electric vehicle, and is rotationally driven by the three-phase AC voltage output from the inverter 504, and its rotational driving force is transmitted to the wheels of the electric vehicle through a transmission, etc., not shown.

[0114] On the other hand, various sensors not shown are used to measure the measured values ​​of the rotation speed and torque of the wheels, the amount of accelerator pedal (acceleration), etc. from the running electric vehicle, and these measurement signals are input to the drive control unit 506. In addition, the output voltage value of the inverter 504 is also input to the drive control unit 506 at the same time. The drive control unit 506 has the function of a controller having a computing unit such as a CPU (Central Processing Unit) and a data storage unit such as a memory, so a control signal is generated by using the input measurement signal, and it is output to the inverter 504 as a feedback signal, thereby controlling the switching operation of the switching element. As a result, the AC voltage provided by the inverter 504 to the motor 505 can be corrected in real time, so as to correctly perform the operation control of the electric vehicle and realize the safe and comfortable operation of the electric vehicle. It should be noted that the voltage output to the inverter 504 can also be controlled by providing the feedback signal from the drive control unit 506 to the boost converter 502.

[0115] Fig.16 To indicate removal Fig.15 The circuit structure after the buck converter 503 in the figure is a circuit structure that only shows the structure for driving the motor 505. As shown in the figure, the semiconductor device of the present invention is applied to the boost converter 502 and the inverter 504 as a Schottky barrier diode, for example, for switching control. In the boost converter 502, it is incorporated into the chopper circuit for chopping control, and in the inverter 504, it is incorporated into the switching circuit including the IGBT for switching control. It should be noted that the current is stabilized by providing an inductor (coil, etc.) at the output end of the battery 501, and the voltage is stabilized by providing a capacitor (electrolytic capacitor, etc.) between the battery 501, the boost converter 502, and the inverter 504.

[0116] In addition, as in Fig.16As shown by the dotted line in the figure, a calculation unit 507 composed of a CPU (Central Processing Unit) and a storage unit 508 composed of a non-volatile memory are provided in the drive control unit 506. The signal input to the drive control unit 506 is provided to the calculation unit 507, and the required calculation is performed to generate a feedback signal for each semiconductor element. In addition, the storage unit 508 temporarily holds the calculation results of the calculation unit 507, accumulates the physical constants and functions required for the drive control in a table form, and outputs them to the calculation unit 507 as appropriate. The calculation unit 507 and the storage unit 508 can adopt a known structure, and their processing capabilities can also be arbitrarily selected.

[0117] like Fig.15 and Fig.16 As shown, in the control system 500, diodes and thyristors, power transistors, IGBTs, MOSFETs, etc. as switching elements are used for the switching operations of the boost converter 502, the buck converter 503, and the inverter 504. By using gallium oxide (Ga2O3), especially corundum gallium oxide (α-Ga2O3) as its material in these semiconductor elements, the switching characteristics are greatly improved. Furthermore, by applying the semiconductor device involved in the present invention, etc., extremely good switching characteristics can be expected, and further miniaturization and cost reduction of the control system 500 can be achieved. That is, the boost converter 502, the buck converter 503, and the inverter 504 can each expect the effect of the present invention, and any one of them, or a combination of any two or more, or a form that also includes a drive control unit 506 can expect the effect of the present invention.

[0118] It should be noted that the control system 500 can be applied not only to the semiconductor device of the present invention in the control system of an electric vehicle, but also to control systems for all purposes such as stepping up and down the voltage of power from a DC power source or converting power from DC to AC. In addition, a power source such as a solar cell can be used as a battery.

[0119] Fig.17 FIG. 2 is a block diagram showing another example of a control system using a semiconductor element or a semiconductor device according to an embodiment of the present invention. Fig.18 The following is a circuit diagram of the control system, which is suitable for being installed in infrastructure equipment and home appliances that are operated by power from an AC power source.

[0120] like Fig.17As shown, the control system 600 is used to input power supplied from the outside, such as a three-phase AC power supply (power supply) 601, and has an AC / DC converter 602, an inverter 604, a motor (driven object) 605 and a drive control unit 606, which can be mounted on various devices (described later). The three-phase AC power supply 601 is, for example, a power generation facility (thermal power plant, hydroelectric power plant, geothermal power plant, atomic power plant, etc.) of an electric power company, and its output is supplied as an AC voltage while being stepped down by a substation. In addition, the three-phase AC power supply 601 is also installed in a building and nearby facilities in the form of a private generator, for example, and is supplied with power through a cable. The AC / DC converter 602 is a voltage conversion device that converts an AC voltage into a DC voltage, and is used to convert the AC voltage of 100V and 200V supplied from the three-phase AC power supply 601 into a specified DC voltage. Specifically, it is converted into a commonly used desired DC voltage such as 3.3V, 5V or 12V by voltage conversion. In the case where the driven object is a motor, it is converted to 12V. It should be noted that a single-phase AC power supply may be used instead of a three-phase AC power supply. In this case, if the AC / DC converter is set to a single-phase input, the same system configuration can be constructed.

[0121] The inverter 604 converts the DC voltage supplied from the AC / DC converter 602 into a three-phase AC voltage by switching operation and outputs it to the motor 605. The motor 604 has a different form depending on the control object, but it is a three-phase AC motor that drives wheels when the control object is a train, drives pumps and various power sources when the control object is factory equipment, and drives compressors and the like when the control object is a household appliance. The motor 605 is rotationally driven by the three-phase AC voltage output from the inverter 604, and its rotational driving force is transmitted to a driving object not shown.

[0122] It should be noted that, for example, there are many driven objects in household appliances that can directly receive the DC voltage output from the AC / DC converter 302 (such as personal computers, LED lighting equipment, video equipment, audio equipment, etc.). In this case, the control system 600 does not need the inverter 604. Fig.17 As shown in , a DC voltage is supplied to the driven object from the AC / DC converter 602. In this case, for example, a 3.3V DC voltage is supplied to a personal computer or the like, and a 5V DC voltage is supplied to an LED lighting device or the like.

[0123] On the other hand, various sensors not shown are used to measure the measured values ​​of the rotation speed and torque of the driven object or the temperature and flow rate of the surrounding environment of the driven object, and these measurement signals are input to the drive control unit 606. In addition, the output voltage value of the inverter 604 is also input to the drive control unit 606 at the same time. Based on these measurement signals, the drive control unit 606 provides a feedback signal to the inverter 604 to control the switching operation of the switching element. Thus, the AC voltage provided by the inverter 604 to the motor 605 can be corrected in real time, so as to correctly perform the operation control of the driven object and realize the stable operation of the driven object. In addition, as mentioned above, in the case where the driven object can be driven by a DC voltage, it is also possible to replace the feedback to the inverter and perform feedback control on the AC / DC converter 602.

[0124] Fig.18 To express Fig.17 A diagram of a circuit structure. As shown in the figure, the semiconductor device of the present invention is applied to an AC / DC converter 602 and an inverter 604 as, for example, a Schottky barrier diode, and is used for switching control. As the AC / DC converter 602, a converter is used in which, for example, a circuit of a Schottky barrier diode is configured in a bridge shape, and a DC conversion is performed by converting the negative voltage portion of the input voltage into a positive voltage and rectifying it. In addition, the switching control is performed by incorporating an IGBT switching circuit in the inverter 604. It should be noted that the current is stabilized by providing an inductor (coil, etc.) between the three-phase AC power supply 601 and the AC / DC converter 602, and the voltage is stabilized by providing a capacitor (electrolytic capacitor, etc.) between the AC / DC converter 602 and the inverter 604.

[0125] In addition, as in Fig.18 As shown by the dotted line in the figure, a calculation unit 607 composed of a CPU and a storage unit 608 composed of a non-volatile memory are provided in the drive control unit 606. The signal input to the drive control unit 606 is provided to the calculation unit 607, and the required calculation is performed to generate a feedback signal for each semiconductor element. In addition, the storage unit 608 temporarily holds the calculation results of the calculation unit 607, accumulates the physical constants and functions required for the drive control in a table form, and outputs them to the calculation unit 607 as appropriate. The calculation unit 607 and the storage unit 608 can adopt a known structure, and their processing capabilities can also be arbitrarily selected.

[0126] In such a control system 600, Fig.15 and Fig.16The control system 500 shown in the figure similarly uses diodes and thyristors, power transistors, IGBTs, MOSFETs, etc. as switching elements in the rectification operation and switching operation of the AC / DC converter 602 and the inverter 604. By using gallium oxide (Ga2O3), especially corundum gallium oxide (α-Ga2O3) as its material in these semiconductor elements, the switching characteristics are greatly improved. Furthermore, by applying the semiconductor elements and semiconductor devices involved in the present invention, extremely good switching characteristics can be expected, and further miniaturization and cost reduction of the control system 600 can be achieved. That is, the AC / DC converter 602 and the inverter 604 can each expect the effect of the present invention, and any one or combination of them, or the form that also includes the drive control unit 606 can expect the effect of the present invention.

[0127] It should be noted that Fig.17 and Fig.18 The motor 605 is exemplified as a driven object, but the driven object is not necessarily limited to an object that is mechanically operated, and many devices that require AC voltage can be used as the object. For the control system 600, as long as power is input from an AC power supply to drive the driven object, it can be applied, and can be installed to drive and control such devices as basic equipment (for example, power equipment in buildings and factories, communication equipment, traffic control equipment, water treatment equipment, system equipment, labor-saving equipment, trams, etc.) and household appliances (for example, refrigerators, washing machines, personal computers, LED lighting equipment, video equipment, audio equipment, etc.).

[0128] The semiconductor element of the present invention can be used in all fields such as semiconductors (such as compound semiconductor electronic devices), electronic components and electrical equipment components, optical and electrophotographic related devices, industrial components, etc., and is particularly useful for power devices.

[0129] Description of Reference Numerals

[0130] 1. Film forming device (atomization CVD device)

[0131] 2a Carrier gas source

[0132] 2b Carrier gas (dilution) source

[0133] 3a flow control valve

[0134] 3b flow control valve

[0135] 4 Fog Sources

[0136] 4a Raw material solution

[0137] 4b Raw material particles

[0138] 5 Containers

[0139] 5a Water

[0140] 6 Ultrasonic vibrator

[0141] 7 Film Forming Room

[0142] 8 Heating Plate

[0143] 9 Supply pipe

[0144] 10 substrates

[0145] 101 semiconductor layer

[0146] 101a n-type semiconductor layer

[0147] 101b n+ type semiconductor layer

[0148] 102 p-type semiconductor layer

[0149] 103 Metal Layer

[0150] 104 Insulator layer

[0151] 105 electrode layer

[0152] 105a Schottky electrode (other electrode layers)

[0153] 105b Ohm electrode (electrode layer)

[0154] 106 conductive adhesive layer

[0155] 107 Conductive substrate

[0156] 108 Base substrate

[0157] 131a n-type semiconductor layer

[0158] 131b first n+ type semiconductor layer

[0159] 131c second n+ type semiconductor layer

[0160] 132 p-type semiconductor layer

[0161] 134 Gate insulation film

[0162] 135a Gate electrode

[0163] 135b Source electrode

[0164] 135c Drain electrode

[0165] 136 Conductive adhesive layer

[0166] 137 Conductive substrate

[0167] 141a n-type semiconductor layer

[0168] 141b first n+ type semiconductor layer

[0169] 141c second n+ type semiconductor layer

[0170] 142 p-type semiconductor layer

[0171] 145a Gate electrode

[0172] 145b Source electrode

[0173] 145c Drain electrode

[0174] 146 Conductive adhesive layer

[0175] 147 Conductive substrate

[0176] 400 Semiconductor components

[0177] 401 solder

[0178] 402 circuit substrate (heat dissipation substrate)

[0179] 500 control system

[0180] 501 battery (power source)

[0181] 502 Boost Converter

[0182] 503 Buck Converter

[0183] 504 Inverter

[0184] 505 motor (driving object)

[0185] 506 Drive control unit

[0186] 507 Operation Department

[0187] 508 Storage

[0188] 600 Control System

[0189] 601 three-phase AC power supply (power supply)

[0190] 602AC / DC Converter

[0191] 604 Inverter

[0192] 605 motor (driven object)

[0193] 606 Drive Control Unit

[0194] 607 Operation Department

[0195] 608 Storage Department

Claims

1. A stacked structure comprising at least a semiconductor layer containing a crystalline oxide semiconductor as a main component and a conductive substrate stacked on the semiconductor layer, characterized in that: The stacked structure has a first direction and a second direction perpendicular or substantially perpendicular to the first direction in a plane perpendicular to the stacking direction of the stacked structure. The first linear expansion coefficient, which is the linear expansion coefficient of the conductive substrate in the first direction, is smaller than the second linear expansion coefficient, which is the linear expansion coefficient of the conductive substrate in the second direction, and the third linear expansion coefficient, which is the linear expansion coefficient of the semiconductor layer in the first direction, is smaller than the fourth linear expansion coefficient, which is the linear expansion coefficient of the semiconductor layer in the second direction.

2. The laminated structure according to claim 1, wherein A difference between the first linear expansion coefficient and the second linear expansion coefficient is 2.0 ppm / K or less.

3. The laminated structure according to claim 1 or 2, wherein: The second linear expansion coefficient is 10 ppm / K or less.

4. The laminated structure according to any one of claims 1 to 3, wherein: The crystalline oxide semiconductor includes at least a first crystal axis and a second crystal axis, and the linear expansion coefficient in the direction of the first crystal axis is smaller than the linear expansion coefficient in the direction of the second crystal axis. The stacking direction of the stacked structure is parallel or substantially parallel to the first crystal axis.

5. The laminated structure according to claim 4, wherein: The crystalline oxide semiconductor has a corundum structure.

6. The laminated structure according to claim 5, wherein: The first crystal axis is the m-axis.

7. The laminated structure according to claim 5 or 6, wherein: The first direction of the semiconductor layer is an a-axis direction, and the second direction of the semiconductor layer is a c-axis direction.

8. The laminated structure according to any one of claims 1 to 7, wherein: The crystalline oxide semiconductor includes at least one metal selected from aluminum, indium, and gallium.

9. The laminated structure according to any one of claims 1 to 8, wherein: The crystalline oxide semiconductor includes at least gallium.

10. The laminated structure according to any one of claims 1 to 9, wherein: The conductive substrate has a thickness of 200 μm or less.

11. A semiconductor element, characterized in that: The invention comprises at least: the stacked structure according to any one of claims 1 to 10; and an electrode.

12. A semiconductor device, wherein at least a semiconductor element is bonded to a lead frame, a circuit substrate or a heat dissipation substrate via a bonding member, wherein: The semiconductor element is the semiconductor element according to claim 11.

13. A power conversion device using the semiconductor device according to claim 12.

14. A control system using the semiconductor device according to claim 12.