Instantaneous inoculant containing rare earth and its application in ductile iron

By using rare earth-containing instantaneous incubators in ductile iron, especially the combination of silicon, aluminum, calcium, zirconium and cerium, combined with in-pack effluent pretreatment and spheroidization, the interior of the integrated bridge shell casting in ductile iron is solved. The density and yield rate issues significantly improve the graphite spheroidization rate and density of the castings.

CN118768526BActive Publication Date: 2024-11-15ANHUI HELI CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202411259705.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-09-10
Publication Date
2024-11-15
Estimated Expiration
2044-09-10

AI Technical Summary

Technical Problem

In ductile iron, especially in the integrated bridge shell casting process, there are challenges of internal density problems and difficult to guarantee yield.

Method used

Use rare earth-containing instantaneous incubators, with specific ingredients including silicon, aluminum, calcium, zirconium and cerium. The mass percentage of zirconium does not exceed 3%, and the mass percentage of cerium does not less than 1%. By adding 0.1% to the iron solution The agent is poured instantaneous incubation treatment, and the in-pack effluent pretreatment and spheroidization treatment are carried out when necessary to further optimize the incubation effect.

Benefits of technology

It significantly improves the internal density and yield of ductile iron parts, especially when the amount of zirconium added is controlled within 1%. The increase of cerium significantly improves the graphite spheroidization effect and the density of the castings, ensuring more stable performance. .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118768526B_ABST
    Figure CN118768526B_ABST
Patent Text Reader

Abstract

The present invention discloses an instantaneous inoculant containing rare earth and its application in ductile iron, wherein the inoculant includes silicon, aluminum, calcium, zirconium and cerium, as well as iron and inevitable impurities, wherein the mass percentage of zirconium does not exceed 3%, and the mass percentage of cerium is not less than 1%. The inoculant of the present invention contains rare earth elements cerium and silicon, aluminum, calcium and iron, and when a small amount of zirconium is added, the internal density problem of the one-piece bridge housing ductile iron casting can be significantly improved, and a relatively stable yield rate can be achieved; in particular, when the addition amount of zirconium is controlled within 1%, as the addition amount of cerium increases, the graphite spheroidization effect and internal density improvement of the one-piece bridge housing ductile iron casting are further significantly improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of casting, and in particular relates to an instantaneous inoculant containing rare earth for casting and the application of the instantaneous inoculant in ductile iron. Background Art

[0002] Cast iron is generally produced in a cupola or induction furnace and generally contains 2 to 4% carbon. The carbon is intimately mixed with the iron, and the form that the carbon takes in the solidified cast iron is important to the characteristics and properties of the iron casting. If the carbon takes the form of iron carbide, the cast iron is called white cast iron and has hard and brittle physical properties, which are undesirable in certain applications. If the carbon takes the form of graphite, the cast iron is soft and machinable and is called gray cast iron.

[0003] Graphite can occur in cast iron in flake, vermicular or spherical form and variations thereof, with the spherical shape producing the strongest and most ductile type of cast iron.

[0004] The graphite can be controlled to obtain different shapes, sizes and number densities of graphite nodules by certain additives that promote graphite formation during the solidification of the cast iron, these additives are called inoculants, and the process by which they are added to the cast iron is called the inoculation process. In the casting of iron products from liquid iron, there is always a risk of the formation of iron carbides in thin sections of the casting. The formation of iron carbides is caused by the rapid cooling of the thin sections compared to the slower cooling of the thicker sections of the casting. The formation of iron carbides in the casting is known in the industry as "chill". The formation of chill is quantified by measuring the "chill depth", and the ability of an inoculant to prevent chill and reduce chill depth is a convenient way to measure and compare the ability of inoculants.

[0005] In cast irons containing spheroidal graphite, the ability of the inoculant is also generally tested by the number density of spheroidal graphite particles per unit area in the as-cast condition. A higher number density of graphite spheroids per unit area means that the ability of the inoculation process or graphite nucleation has been improved.

[0006] Therefore, there is a continuing need to find inoculants that reduce the depth of the chill and improve the machinability of gray cast iron and increase the number density of graphite nodules in ductile iron.

[0007] Since the exact chemistry and mechanism of the inoculation process and why the inoculants work as they do are not fully understood at this time, a great deal of research is being conducted to provide the industry with new and improved inoculants.

[0008] It is generally believed in the industry that calcium and certain other elements inhibit iron carbide formation and promote graphite formation, and therefore most inoculants contain calcium, and the addition of these iron carbide inhibitors is usually promoted by the addition of ferrosilicon alloys.

[0009] In recent years, the industry has found that the addition of rare earth elements can help improve the performance of inoculants to a certain extent.

[0010] Earlier, the patent application document with the publication number CN100408710C publicly recorded the inoculant product containing bismuth and rare earths, which contained 5~75% ferrosilicon-based A-type alloy, wherein Si / Fe>2, 0.005~3% by mass of rare earths, 0.005~3% bismuth, lead and / or antimony, and less than 3% calcium, wherein the (Bi+Pb+Sb) / RE ratio was 0.9~2.2; and contained at least one of 25~95% silicon-based or ferrosilicon-based B-type alloy, wherein Si / Fe>2 calculated based on silicon or ferrosilicon, and the calcium content was such that the total calcium content in the mixture accounted for 0.3~3%. The above mixture has good time stability of grains and can perform efficient inoculation treatment on castings, especially thin castings.

[0011] The patent application document with publication number CN116441496B also publicly records a high-efficiency inoculant for large-section ductile iron castings containing bismuth oxide, which includes 30-75% Si, 0-10% Sn, 0.5-10% Bi, 0.1-5.0% rare earth, 2.0-8.0% Ba, 0-5.0% O and impurities within 1% by mass, the balance is Fe, and the rare earth metal is lanthanum, cerium or yttrium. Pig iron, ferrosilicon, silicon-barium master alloy and rare earth metals are added to the medium frequency furnace for smelting in sequence. When the raw materials are completely melted and the molten iron forms a homogeneous molten state, slag is removed. The temperature of the molten iron needs to reach 1300~1350℃. Granular metal bismuth oxide and metal tin are added. The power of the medium frequency furnace is increased to rapidly raise the temperature in the furnace to about 1400℃. The power of the medium frequency furnace is reduced, and the molten iron is poured into the ingot plate. After natural cooling to room temperature, the molten iron is completely solidified. The ingot plate is tilted to manually demold into the iron trough. The thickness of the ingot plate is 30~70mm. The application of the above-prepared high-efficiency inoculant in ductile iron can obtain strong mechanical properties such as tensile strength, yield strength, elongation after fracture and cross-sectional shrinkage.

[0012] As an external protective structure of a driving component, the bridge housing, left and right connecting plates and left and right axle heads are usually cast separately and then assembled and fixed. Casting them as an integrated whole can reduce machining and assembly costs. However, when the casting is integrated and molded as a whole, there are multiple scattered isolated hot spots in the casting, and the yield rate of the casting is difficult to guarantee. It is also difficult to solve the internal density problem only from the riser shrinkage compensation design and the chiller design at the hot spot. Summary of the invention

[0013] In view of the above technical problems, the present application proposes an instantaneous inoculant containing rare earth and its application in ductile iron, aiming to improve the internal density problem in the casting process of the one-piece bridge housing.

[0014] The specific technical solutions are as follows:

[0015] In a first aspect, the present application provides a rare earth-containing instantaneous inoculant, which includes silicon, aluminum, calcium, zirconium and cerium, as well as iron and inevitable impurities, wherein the mass percentage of zirconium does not exceed 3%, and the mass percentage of cerium is not less than 1%.

[0016] In some preferred embodiments, the mass percentage of zirconium does not exceed 1%.

[0017] In some preferred embodiments, the mass percentage of cerium is 3-4%.

[0018] In some preferred embodiments, the mass percentage of zirconium is 0.7-1%.

[0019] In a second aspect, the present application provides an application of an instantaneous inoculant containing rare earth, wherein the above-mentioned inoculant is added in an amount of 0.1% of the total mass of the molten iron for pouring instantaneous inoculation treatment.

[0020] In some preferred embodiments, before the pouring instantaneous inoculation treatment, the molten iron is subjected to ladle water pretreatment and spheroidization treatment in sequence, wherein the ladle water pretreatment uses 0.2-1 mm particle size metallurgical grade silicon carbide accounting for 0.2% of the total mass of the molten iron.

[0021] In some preferred embodiments, after the spheroidization treatment and before the pouring instantaneous inoculation treatment, a secondary inoculation treatment is carried out using a barium-based inoculation wire with a concentration of 0.1% of the total mass of the molten iron.

[0022] In some preferred embodiments, the barium-based inoculated wire comprises, by mass percentage, 68-75% Si, 2-4% Ba, 1-2% Ca and no more than 1.5% Al.

[0023] The beneficial effects of the present invention are as follows: the inoculant of the present invention contains rare earth elements cerium and silicon, aluminum, calcium, and iron. When a small amount of zirconium is added, the internal density problem of the one-piece bridge housing ductile iron casting can be significantly improved, and a relatively stable yield rate can be achieved; in particular, when the amount of zirconium added is controlled within 1%, as the amount of cerium added increases, the graphite spheroidization effect and internal density improvement of the one-piece bridge housing ductile iron casting are further significantly improved. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 Shown is the structure of the ductile iron casting of the one-piece bridge housing;

[0025] Figure 2 Shown is a metallographic diagram of the application of Example 46;

[0026] Figure 3 Shown is a metallographic diagram of the application of Example 1. DETAILED DESCRIPTION

[0027] In order to make the purpose, technical solution and advantages of the embodiments of the present invention more clear, the technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments. Example 1

[0028] Preparation of inoculant

[0029] High-grade ferrosilicon and pig iron are selected as raw materials, mixed evenly in a mass ratio of 4:1, and then placed in a furnace to be smelted to 1300℃ to form a completely molten liquid alloy, and the slag is scraped off at the same time.

[0030] Silicon calcium alloy, silicon zirconium alloy and aluminum ingot are added into the furnace in sequence according to 5%, 3.5% and 1% of the mass percentage of the liquid alloy respectively, and then the temperature is rapidly raised and stirred evenly to form molten alloy liquid until the temperature of the molten metal in the furnace reaches 1380°C; during the process of being taken out of the furnace, rare earth ferrosilicon alloy particles are evenly sprinkled on the alloy liquid in a flowing manner according to 3.5% of the mass percentage of the liquid alloy liquid.

[0031] The alloy liquid is quickly cooled to a solid state (below 900°C) by a rapid cooling device, then placed in a graphite container and naturally cooled to room temperature, and finally crushed and screened into 0.2~0.8mm granular inoculant.

[0032] The measured composition is: 52.3% silicon, 0.94% aluminum, 1.58% calcium, 1.03% cerium, 1.14% zirconium, and the balance is iron. In this embodiment and subsequent embodiments, the composition contents are expressed in percentages by mass unless otherwise specified.

[0033] The method for preparing the inoculant in Example 1 was adopted to change the addition amount of each component to prepare the inoculants of Examples 2 to 10 respectively. The measured components of the inoculants prepared in each example are shown in Table 1.

[0034] Table 1: Measured composition of the inoculants of Examples 1 to 10

[0035]

[0036] Embodiment 11

[0037] Application of inoculant

[0038] The performance of the inoculants of Examples 1 to 10 on the ductile iron castings of the integrated bridge housing is shown in that the amount of the inoculant is 0.1% of the total mass of the molten iron, and the inoculant is used as a stream inoculant.

[0039] The one-piece bridge housing is characterized by integrating the bridge housing 100, the left and right connecting plates 200, and the left and right axle heads 300. The five parts are cast in one piece, and the weight of the casting is 74.2 kg. It is no longer necessary to form five parts separately and then assemble them, which greatly reduces the machining cost and assembly cost. Due to the high degree of integration of the castings, the one-piece molding, and the dispersion of isolated heat nodes, especially the ends of the connecting plates 200 and the axle heads 300 and the bridge housing 100, even if shrinkage is compensated by using hot risers, heat risers and side risers, and cold iron is used for quenching at the hot nodes, it is difficult to ensure the yield rate, and there will still be problems with internal density.

[0040] Ductile iron castings of integrated bridge housing Figure 1 As shown, the composition of the ductile iron castings of the integrated bridge housing is shown in Table 2.

[0041] Table 2: Composition of ductile iron castings for one-piece axle housing

[0042]

[0043] The performance parameters shown in Table 3 were obtained in the ductile iron castings of the integrated axle housing using the inoculants of Examples 1 to 10.

[0044] Table 3: Performance of the inoculants of Examples 1 to 10 in ductile iron castings of an integrated axle housing

[0045]

[0046] This embodiment and subsequent embodiments are based on the standards for spheroidization classification in GB / T 9441-2021 (national standard for metallographic inspection of ductile iron), and the corresponding spheroidization rates also correspond to the corresponding classification standards.

[0047] Based on the performance of the one-piece bridge housing manufactured using different inoculants of Examples 1 to 10 in Example 11, the addition of cerium and zirconium has a direct impact on the performance of ductile iron castings. In particular, when cerium and zirconium are added in small amounts, they help to improve the shrinkage defects of the one-piece bridge housing castings.

[0048] The method for preparing the inoculant in Example 1 was adopted to change the addition amount of each component to prepare the inoculants of Examples 12 to 21 and Examples 22 to 31, respectively. The measured components of the inoculants prepared in each example are shown in Tables 4 and 5.

[0049] Table 4: Measured components of the inoculants of Examples 12 to 21

[0050]

[0051] Table 5: Measured composition of the inoculants of Examples 22 to 31

[0052]

[0053] Embodiment 32

[0054] Application of inoculant

[0055] The performance of using the inoculants of Examples 12 to 21 and Examples 22 to 31 on the ductile iron castings of the integrated bridge housing, the amount of the inoculant used is 0.1% of the total mass of the molten iron, and the inoculant is used as a stream inoculant.

[0056] The integrated bridge housing is the same as that in embodiment 11.

[0057] The performance parameters shown in Tables 6 and 7 were obtained by using the inoculants of Examples 12 to 21 and Examples 22 to 31 in the ductile iron castings of the integrated bridge housing.

[0058] Table 6: Performance of the inoculants of Examples 12 to 21 in ductile iron castings of integrated axle housings

[0059]

[0060] Table 7: Performance of the inoculants of Examples 22 to 31 in ductile iron castings of integrated axle housings

[0061]

[0062] Combined with the performance of the integrated bridge housing manufactured using different inoculants of Examples 12 to 21 in Example 32, in Examples 12 to 16, the zirconium content is close to 1%, and the cerium content increases from 1% to 5%, and in Examples 17 to 21, the zirconium content is close to 2%, and the cerium content increases from 1% to 5%. It can be found that after comparing Examples 17 to 21 one by one, after the zirconium content is increased from 1% to 2%, although the cerium content remains almost unchanged, the performance of graphite spheroidization and the density of the casting show an overall decline.

[0063] Combined with the performance of the one-piece bridge housing manufactured using different inoculants of Examples 22 to 31 in Example 32, in Examples 22 to 26, the cerium content is close to 1%, and the zirconium content increases from 1% to 5%, and in Examples 27 to 31, the cerium content is close to 2%, and the zirconium content increases from 1% to 5%; it can be found that in Examples 22 to 26, the performance of the ductile iron parts of Example 22 is close to that of Example 12, and as the zirconium content increases from 1% to 5%, the ductile iron parts not only show a decrease in the density of the casting, but also have a great impact on the performance of graphite spheroidization; in Examples 27 to 31, the performance of the ductile iron parts of Example 27 is close to that of Example 13, and the ductile iron parts of Example 27 are slightly better than those of Example 22 in graphite spheroidization, but as the zirconium content increases from 1% to 5%, the performance of the ductile iron parts in graphite spheroidization and the density of the casting both show an overall decline.

[0064] It can be seen that when zirconium is added in a lower amount, combined with cerium that is more than the amount of zirconium added, it is more conducive to improving the shrinkage defects of the casting of the one-piece bridge housing, and at the same time improves the performance of graphite spheroidization to a certain extent, thereby obtaining ductile iron castings with better comprehensive performance, especially when the zirconium content is close to 1% and the cerium content is between 3% and 4%.

[0065] The method for preparing the inoculant in Example 1 was adopted to change the addition amount of each component to prepare the inoculants of Examples 33 to 41 respectively. The measured components of the inoculants prepared in each example are shown in Table 8.

[0066] Table 8: Measured components of the inoculants of Examples 33 to 41

[0067]

[0068] Embodiment 42

[0069] Application of inoculant

[0070] The performance of the inoculant of Examples 33 to 41 on the ductile iron castings of the integrated bridge housing is shown in FIG. 1. The amount of the inoculant used is 0.1% of the total mass of the molten iron, and the inoculant is used as a stream inoculant.

[0071] The integrated bridge housing is the same as that in embodiment 11.

[0072] The performance parameters shown in Table 9 were obtained by using the inoculants of Examples 33 to 41 in the ductile iron castings of the integrated bridge housing.

[0073] Table 9: Performance of the inoculants of Examples 33 to 41 in ductile iron castings of an integrated axle housing

[0074]

[0075] Combined with the performance of the integrated bridge housing manufactured by using different inoculants of Examples 33 to 41 in Example 42, in Examples 33 to 41, the zirconium content is less than 1%, the cerium content is between 3% and 4%, and the zirconium content increases in Examples 38 to 41. In terms of the performance of graphite spheroidization and the density of the casting, Example 38 performs best, indicating that when the zirconium content in the inoculant is controlled to be less than 1% and the cerium content is between 3% and 4%, the performance of the ductile iron castings in graphite spheroidization and the density of the casting are significantly improved; but in Examples 33 to 37, although the ductile iron castings have good performance in graphite spheroidization, they all show micro-shrinkage, indicating that the density of the casting is not stable. Therefore, the zirconium content should be controlled above 0.7%.

[0076] Embodiment 43

[0077] Application of inoculant

[0078] Performance of the inoculant of Example 38 on the ductile iron castings of the integral axle housing.

[0079] The integrated bridge housing is the same as that in embodiment 11.

[0080] The application process of inoculant is:

[0081] 0.2~1mm particle size metallurgical grade silicon carbide, which accounts for 0.2% of the total mass of the molten iron, is used for in-launder effluent pretreatment;

[0082] Before inoculation, magnesium 15-2 spheroidizing wire was used for spheroidizing by wire feeding method. The amount of spheroidizing wire used was 1% of the total mass of molten iron. The composition of magnesium 15-2 spheroidizing wire is shown in Table 10.

[0083] The pouring instant inoculation treatment was carried out using 0.1% of the inoculant of Example 38.

[0084] Table 10: Composition of magnesium 15-2 spheroidized wire

[0085]

[0086] The role of silicon carbide is:

[0087] (1) Reduce the amount of dissolved oxygen in molten iron. After treatment, the dissolved oxygen content in molten iron can be reduced from the conventional 17.8ppm to 11.6ppm, and the roundness of graphite is improved;

[0088] (2) Reduce the supercooling of the molten iron out of the furnace to avoid the premature precipitation of graphite nodules, increase the number of eutectic clusters and graphite nodules after the molten iron is inoculated, reduce the shrinkage of the molten iron, and help obtain dense castings.

[0089] Embodiment 44

[0090] Application of inoculant

[0091] Performance of the inoculant of Example 38 on the ductile iron castings of the integral axle housing.

[0092] The integrated bridge housing is the same as that in embodiment 11.

[0093] The application process of the inoculant is:

[0094] 0.2~1mm particle size metallurgical grade silicon carbide, which accounts for 0.2% of the total mass of the molten iron, is used for in-launder effluent pretreatment;

[0095] Before inoculation, magnesium 15-2 spheroidizing wire is used for spheroidizing by wire feeding method, and the amount of spheroidizing wire used is 1% of the total mass of molten iron;

[0096] Use barium-based inoculated wire with a total mass of 0.7% of the molten iron to ensure the inoculation effect of the secondary inoculation. The main components of the barium-based inoculated wire (in mass percentage) are: Si68~75%; Ba2~4%; Al≤1.5%; Ca1~2%.

[0097] 0.1% of the inoculant of Example 38 was used for pouring instant inoculation treatment.

[0098] Embodiment 45

[0099] Application of inoculant

[0100] Performance of the inoculant of Example 38 on the ductile iron castings of the integral axle housing.

[0101] The integrated bridge housing is the same as that in embodiment 11.

[0102] The application process of inoculant is:

[0103] 0.2~1mm particle size metallurgical grade silicon carbide, which accounts for 0.2% of the total mass of the molten iron, is used for in-launder effluent pretreatment;

[0104] Before inoculation, magnesium 15-2 spheroidizing wire is used for spheroidizing by wire feeding method, and the amount of spheroidizing wire used is 1% of the total mass of molten iron;

[0105] Use barium-based inoculated wire with a total mass of 0.6% of the molten iron to ensure the inoculation effect of the secondary inoculation. The main components of the barium-based inoculated wire (in mass percentage) are: Si68~75%; Ba2~4%; Al≤1.5%; Ca1~2%.

[0106] 0.1% of the inoculant of Example 38 was used for pouring instant inoculation treatment.

[0107] Embodiment 46

[0108] Application of inoculant

[0109] Performance of the inoculant of Example 38 on the ductile iron castings of the integral axle housing.

[0110] The integrated bridge housing is the same as that in embodiment 11.

[0111] The application process of inoculant is:

[0112] 0.2~1mm particle size metallurgical grade silicon carbide, which accounts for 0.2% of the total mass of the molten iron, is used for in-launder effluent pretreatment;

[0113] Before inoculation, magnesium 15-2 spheroidizing wire is used for spheroidizing by wire feeding method, and the amount of spheroidizing wire used is 1% of the total mass of molten iron;

[0114] Use barium-based inoculated wire accounting for 0.5% of the total mass of molten iron for inoculation treatment to ensure the inoculation effect of secondary inoculation. The main components of the barium-based inoculated wire (in terms of mass percentage) are: Si68~75%; Ba2~4%; Al≤1.5%; Ca1~2%.

[0115] 0.1% of the inoculant of Example 38 was used for pouring instant inoculation treatment.

[0116] Embodiment 47

[0117] Application of inoculant

[0118] Performance of the inoculant of Example 38 on the ductile iron castings of the integral axle housing.

[0119] The integrated bridge housing is the same as that in embodiment 11.

[0120] The application process of inoculant is:

[0121] 0.2~1mm particle size metallurgical grade silicon carbide, which accounts for 0.2% of the total mass of the molten iron, is used for in-launder effluent pretreatment;

[0122] Before inoculation, magnesium 15-2 spheroidizing wire is used for spheroidizing by wire feeding method, and the amount of spheroidizing wire used is 1% of the total mass of molten iron;

[0123] Use barium-based inoculated wire with a total mass of 0.4% of the molten iron to ensure the inoculation effect of the secondary inoculation. The main components of the barium-based inoculated wire (in mass percentage) are: Si68~75%; Ba2~4%; Al≤1.5%; Ca1~2%.

[0124] 0.1% of the inoculant of Example 38 was used for pouring instant inoculation treatment.

[0125] Embodiment 48

[0126] Application of inoculant

[0127] Performance of the inoculant of Example 38 on the ductile iron castings of the integral axle housing.

[0128] The integrated bridge housing is the same as that in embodiment 11.

[0129] The application process of inoculant is:

[0130] 0.2~1mm particle size metallurgical grade silicon carbide, which accounts for 0.2% of the total mass of the molten iron, is used for in-launder effluent pretreatment;

[0131] Before inoculation, magnesium 15-2 spheroidizing wire is used for spheroidizing by wire feeding method, and the amount of spheroidizing wire used is 1% of the total mass of molten iron;

[0132] Use barium-based inoculated wire with a total mass of 0.3% of the molten iron to ensure the inoculation effect of the secondary inoculation. The main components of the barium-based inoculated wire (in mass percentage) are: Si68~75%; Ba2~4%; Al≤1.5%; Ca1~2%.

[0133] 0.1% of the inoculant of Example 38 was used for pouring instant inoculation treatment.

[0134] Embodiment 49

[0135] Application of inoculant

[0136] Performance of the inoculant of Example 38 on the ductile iron castings of the integral axle housing.

[0137] The integrated bridge housing is the same as that in embodiment 11.

[0138] The application process of inoculant is:

[0139] 0.2~1mm particle size metallurgical grade silicon carbide, which accounts for 0.2% of the total mass of the molten iron, is used for in-launder effluent pretreatment;

[0140] Before inoculation, magnesium 15-2 spheroidizing wire is used for spheroidizing by wire feeding method, and the amount of spheroidizing wire used is 1% of the total mass of molten iron;

[0141] Use barium-based inoculated wire accounting for 0.2% of the total mass of molten iron for inoculation treatment to ensure the inoculation effect of secondary inoculation. The main components of the barium-based inoculated wire (in terms of mass percentage) are: Si68~75%; Ba2~4%; Al≤1.5%; Ca1~2%.

[0142] 0.1% of the inoculant of Example 38 was used for pouring instant inoculation treatment.

[0143] Embodiment 50

[0144] Application of inoculant

[0145] Performance of the inoculant of Example 38 on the ductile iron castings of the integral axle housing.

[0146] The integrated bridge housing is the same as that in embodiment 11.

[0147] The application process of inoculant is:

[0148] 0.2~1mm particle size metallurgical grade silicon carbide, which accounts for 0.2% of the total mass of the molten iron, is used for in-launder effluent pretreatment;

[0149] Before inoculation, magnesium 15-2 spheroidizing wire is used for spheroidizing by wire feeding method, and the amount of spheroidizing wire used is 1% of the total mass of molten iron;

[0150] Use barium-based inoculated wire accounting for 0.1% of the total mass of molten iron for inoculation treatment to ensure the inoculation effect of secondary inoculation. The main components of the barium-based inoculated wire (in terms of mass percentage) are: Si68~75%; Ba2~4%; Al≤1.5%; Ca1~2%.

[0151] The pouring instant inoculation treatment was carried out using 0.1% of the inoculant of Example 38.

[0152] Table 11: Performance of the inoculants of Examples 43 to 50 in ductile iron castings of an integrated axle housing

[0153]

[0154] Combined with the performance of different application modes of the inoculant in Examples 43 to 50, spheroidizing treatment before inoculation can change the morphology of graphite precipitation from flake to spherical, thereby helping to improve the spheroidizing rate and the number of graphite nodules while ensuring the density of the casting; on the other hand, during the inoculation process, the use of silicon carbide and barium-based inoculating wires for coordinated graded inoculation can further improve the spheroidizing performance, especially the inoculation treatment with an addition amount of 0.5%, which can achieve the optimal spheroidizing effect.

[0155] In addition, the present application also provides a metallographic diagram of Example 46 and a metallographic diagram of Example 1. The metallographic diagram shows the end of the connecting plate 200 away from the shaft head 300. Figure 2 The corresponding metallographic diagram is that of the embodiment 46 application. Figure 3 The corresponding metallographic diagram is applied in Example 1.

[0156] The above embodiments are only used to illustrate the technical solutions of the present invention, but not to limit them.

Claims

1. An instantaneous inoculant containing rare earth, characterized in that: It includes silicon, aluminum, calcium, zirconium and cerium, as well as iron and inevitable impurities, of which the mass percentage of zirconium does not exceed 3% and the mass percentage of cerium is not less than 1%.

2. The rare earth-containing instantaneous inoculant according to claim 1, characterized in that: The mass percentage of zirconium does not exceed 1%.

3. The rare earth-containing instantaneous inoculant according to claim 2, characterized in that: The mass percentage of the cerium is 3-4%.

4. The rare earth-containing instantaneous inoculant according to claim 3, characterized in that: The mass percentage of zirconium is 0.7-1%.

5. Application of rare earth-containing instantaneous inoculant, characterized in that: The inoculant according to any one of claims 1 to 4 is added in an amount of 0.1% of the total mass of the molten iron for pouring instantaneous inoculation treatment.

6. The use of the rare earth-containing instantaneous inoculant according to claim 5, characterized in that: Before the pouring instantaneous inoculation treatment, the molten iron is subjected to a ladle water pretreatment and a spheroidization treatment in sequence, wherein the ladle water pretreatment uses 0.2-1 mm granular metallurgical grade silicon carbide accounting for 0.2% of the total mass of the molten iron.

7. The use of the rare earth-containing instantaneous inoculant according to claim 6, characterized in that: After spheroidization and before pouring instantaneous inoculation, a secondary inoculation treatment is carried out using a barium-based inoculation wire with a concentration of 0.1% of the total mass of the molten iron.

8. The use of the rare earth-containing instantaneous inoculant according to claim 7, characterized in that: The barium-based inoculated wire comprises, by mass percentage, 68%-75% Si, 2%-4% Ba, 1%-2% Ca and no more than 1.5% Al.

Citation Information

Patent Citations

  • Inoculant products comprising bismuth and rare earths

    CN100408710C

  • A high-efficiency inoculant for large-section ductile iron castings containing bismuth oxide

    CN116441496B

  • Formula of inoculant suitable for high-grade gray iron member and treatment method therefor

    CN109207666A

  • Inoculant for improving tensile strength of iron casting and preparation method of inoculant

    CN115505669A

  • Cast iron inoculant and method for producing cast iron inoculant

    CN118240998A