PETG (polyethylene terephthalate glycol) consumable for 3D (three-dimensional) printing and processing method of PETG consumable

By adding diethylene glycol and polybutylene terephthalate to PETG filaments and adopting a specific polymerization and granulation process, the problem of deformation and warping of PETG filaments in 3D printing is solved, and the printing speed and quality are improved. , achieving a more efficient 3D printing process.

CN118772597AInactive Publication Date: 2024-10-15SENBO (YANCHENG) 3D TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411005982.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-25
Publication Date
2024-10-15
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing PETG filaments are easily deformed during 3D printing, causing the bottom layer of the printed object to deform or warp, affecting the printing quality, and the printing speed is slow, resulting in low 3D printing efficiency.

Method used

By adding diethylene glycol and polybutylene terephthalate, combined with a specific polymerization reaction and granulation process, the fluidity and thermal stability of the consumables are improved, ensuring that the material maintains stable performance at high temperatures and avoids deformation and warping. Improve printing speed and quality.

Benefits of technology

It improves the fluidity and thermal stability of consumables, ensures stable material supply during the printing process, avoids deformation and warping, increases printing speed and efficiency, and maintains the shape stability of printed parts.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118772597A_ABST
    Figure CN118772597A_ABST
Patent Text Reader

Abstract

The invention discloses a PETG consumable for 3D printing and a processing method thereof, and relates to the technical field of 3D printing consumables, the PETG consumable comprises the following raw materials by weight: 20-30 parts of terephthalic acid, 10-12 parts of ethylene glycol, 10-15 parts of 1, 3-propylene glycol, 10-15 parts of 1, 3-propylene glycol, 10-15 parts of 1, 3-propylene glycol, 10-15 parts of 1, 3-propylene glycol, 10-15 parts of The composite material is prepared from the following components in parts by weight: 20-30 parts of polybutylene terephthalate, 6-9 parts of 1, 4-cyclohexanedimethanol, 6-9 parts of diethylene glycol, 12-18 parts of ethylene glycol antimony, 15-28 parts of sodium acetate, 25-40 parts of polybutylene terephthalate, 8-14 parts of a lubricant and 10-16 parts of an antioxidant. The 3D printer is not prone to blockage or extrusion in 3D printing, stable material supply in the printing process is guaranteed, pause or distortion in the printing process is avoided, the printing quality is guaranteed while the printing speed is increased, a PETG printed piece is not prone to buckling deformation after being cooled, and the 3D printer is suitable for 3D printing. And good shape stability can be kept at a high printing speed.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of 3D printing consumables, and in particular to a PETG consumable for 3D printing and a processing method thereof. Background Art

[0002] 3D printing technology is a technology that uses 3D printing equipment to add materials layer by layer to manufacture three-dimensional products based on the designed 3D model. It is an emerging technology that is rapidly developing in the manufacturing industry. 3D printing technology has been widely used in aerospace, medical, education, construction and other fields. PETG is a copolyester with very low crystallinity or even no crystallinity at all. It has excellent optical properties and good processability. In addition, it has excellent properties such as non-toxicity and environmental protection. Using PETG material for 3D printing can not only overcome the problem of insufficient toughness of polylactic acid printing consumables, but also overcome the problems of easy shrinkage of ABS printing consumables during the printing process and poor dimensional stability of printed products.

[0003] However, the existing PETG consumables have a low thermal deformation temperature and are prone to deformation during 3D printing. If the hot bed temperature is not high enough or the printing environment temperature is unstable, the printed object will be deformed or warped at the bottom layer, affecting the printing quality. In addition, the printing speed is slow, resulting in low 3D printing efficiency. Summary of the invention

[0004] The object of the present invention is to provide a PETG consumable for 3D printing and a processing method thereof, so as to solve the problem that the existing PETG consumable proposed in the above background technology is easy to deform in 3D printing, resulting in deformation or warping of the printed object at the bottom layer, affecting the printing quality, and the printing speed is slow during the printing process, resulting in low 3D printing efficiency.

[0005] To achieve the above-mentioned purpose, the present invention provides the following technical scheme: a PETG consumable for 3D printing, comprising the following raw materials in parts by weight: 20-30 parts by weight of terephthalic acid, 10-12 parts by weight of ethylene glycol, 10-15 parts by weight of 1,4-cyclohexanedimethanol, 6-9 parts by weight of diethylene glycol, 12-18 parts by weight of ethylene glycol antimony, 15-28 parts by weight of sodium acetate, 25-40 parts by weight of polybutylene terephthalate, 8-14 parts by weight of a lubricant and 10-16 parts by weight of an antioxidant.

[0006] Preferably, the lubricant is any one of polytetrafluoroethylene and silicone oil.

[0007] Preferably, the antioxidant is any one of butyl hydroxyphenol, butyl hydroxybenzoate and sodium sulfide.

[0008] A method for processing PETG consumables for 3D printing, comprising the following steps:

[0009] S1. Accurately weigh terephthalic acid, ethylene glycol, 1,4-cyclohexanedimethanol, diethylene glycol, antimony glycol and sodium acetate, and then put them into a polymerization reactor respectively;

[0010] S2, nitrogen is introduced into the polymerization reactor, and the air in the reactor is replaced with nitrogen three times, and the pressure in the reactor is maintained at 0.22-0.25 MPa to carry out esterification reaction;

[0011] S3, control the outlet valve opening to control the outlet rate. When the outlet water volume is greater than 90% of the theoretical outlet water volume, the esterification pressure decreases, the esterification liquid temperature increases, and the esterification ends.

[0012] S4, slowly reducing the pressure to enter a low vacuum for pre-polycondensation. After the pre-polycondensation is completed, the liquid temperature in the kettle is raised to 275-283°C for final polycondensation reaction. The vacuum degree in the kettle is lower than 70Pa;

[0013] S5, after the polycondensation is completed, the material is discharged through water-cooling and then pelletized to obtain PETG particles;

[0014] S6, PETG particles, polybutylene terephthalate, lubricant and antioxidant are mixed and granulated, and then dried and extruded to obtain PETG consumables.

[0015] Preferably, in step S2, the replacing with nitrogen three times comprises the following steps:

[0016] S21, passing nitrogen into the polymerization reactor for 5-10 minutes to allow the nitrogen to fully replace the air in the reactor;

[0017] S22, exhaust the gas in the reactor through the exhaust valve at the bottom, and continue to introduce nitrogen to ensure that the air in the reactor is removed as much as possible;

[0018] S23, repeat the above steps, and perform nitrogen replacement three times continuously to ensure that the air in the kettle is basically eliminated;

[0019] S24. When all replacements are completed, turn off the nitrogen gas source and confirm that the kettle has been replaced with pure nitrogen.

[0020] Preferably, in step S2, the liquid temperature in the polymerization reactor during the esterification reaction is maintained at 220-240°C.

[0021] Preferably, in step S4, the pre-polycondensation time is 40-45 minutes.

[0022] Preferably, in step S6, the mixed granulation is dried and then extruded to obtain the PETG consumables, comprising the following steps:

[0023] S61, adding PETG particles and polybutylene terephthalate into a high-speed mixer, adding a lubricant and an antioxidant into the mixer, and starting the high-speed mixer for mixing;

[0024] S62, the mixed particles are extruded and granulated at 215-260° C. by a twin-screw extruder at a speed of 160 r / min;

[0025] S63, repeating twice to obtain uniformly mixed particles and drying the particles;

[0026] S64. The dried particles are extruded through a single screw extruder to obtain PETG filaments.

[0027] Preferably, in step S6, the diameter of the PETG consumable is 1.75±0.5 mm.

[0028] Compared with the prior art, the present invention has the following beneficial effects:

[0029] 1. In the present invention, the addition of diethylene glycol improves the fluidity of the consumables, so that the PETG consumables can flow out of the nozzle evenly during 3D printing, and are not prone to clogging or extrusion problems, thereby ensuring a stable material supply during the printing process, avoiding pauses or distortions during the printing process, and improving the printing speed while ensuring the printing quality. The PETG prints are less likely to warp and deform after cooling, and can maintain good shape stability at a faster printing speed, thereby improving printing efficiency.

[0030] 2. In the present invention, by blending and adding polybutylene terephthalate, the PETG consumables have better thermal stability, can maintain stable performance at high temperatures, and are not prone to deterioration or thermal deformation, which helps to maintain stable printing quality at a higher printing speed. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Figure 1 A flowchart of a PETG consumable for 3D printing and a processing method thereof of the present invention;

[0032] Figure 2 It is a thermal decomposition temperature statistical diagram of the present invention. DETAILED DESCRIPTION

[0033] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the implementation regulations described are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0034] The present invention will be further described below in conjunction with the embodiments.

[0035] Example 1

[0036] like Figure 1 As shown, this embodiment provides a PETG consumable for 3D printing, comprising the following raw materials in parts by weight: 20 parts by weight of terephthalic acid, 10 parts by weight of ethylene glycol, 10 parts by weight of 1,4-cyclohexanedimethanol, 6 parts by weight of diethylene glycol, 12 parts by weight of ethylene glycol antimony, 15 parts by weight of sodium acetate, 25 parts by weight of polybutylene terephthalate, 8 parts by weight of lubricant and 10 parts by weight of antioxidant;

[0037] Among them, the lubricant is polytetrafluoroethylene and the antioxidant is sodium sulfide.

[0038] A method for processing PETG consumables for 3D printing, comprising the following steps:

[0039] Step 1, accurately weighing terephthalic acid, ethylene glycol, 1,4-cyclohexanedimethanol, diethylene glycol, ethylene glycol antimony and sodium acetate, and then respectively putting them into a polymerization reactor;

[0040] Step 2, nitrogen is introduced into the polymerization reactor, and the air in the reactor is replaced with nitrogen three times, and the air in the reactor is discharged, and the pressure in the reactor is maintained at 0.22-0.25 MPa to carry out esterification reaction;

[0041] Wherein, the liquid temperature in the polymerization reactor during the esterification reaction is maintained at 220-240°C;

[0042] Wherein, replacing with nitrogen three times comprises the following steps:

[0043] 21) Pass nitrogen into the polymerization reactor for 5-10 minutes to allow the nitrogen to fully replace the air in the reactor;

[0044] 22) Exhaust the gas in the reactor through the exhaust valve at the bottom, and continue to introduce nitrogen to ensure that the air in the reactor is removed as much as possible;

[0045] 23) Repeat the above steps and perform nitrogen replacement three times in succession to ensure that the air in the kettle is basically eliminated;

[0046] 24) When all replacements are completed, turn off the nitrogen source and confirm that the kettle has been replaced with pure nitrogen;

[0047] Step 3: Control the outlet valve opening to control the outlet rate. When the outlet water volume is greater than 90% of the theoretical outlet water volume, the esterification pressure is reduced, the esterification liquid temperature is increased, and the esterification is completed.

[0048] Step 4: Slowly reduce the pressure to enter a low vacuum for pre-condensation. After the pre-condensation is completed, the liquid temperature in the kettle is raised to 275-283°C for final polycondensation. The vacuum degree in the kettle is lower than 70Pa; wherein the pre-condensation time is 45min;

[0049] Step 5: After the polycondensation is completed, the PETG particles are obtained by water-cooling the strips and then pelletizing them.

[0050] Step 6: PETG particles, polybutylene terephthalate, lubricant and antioxidant are mixed and granulated, and then dried and extruded to obtain PETG consumables;

[0051] The process of mixing and granulating, drying and then extruding to obtain PETG consumables comprises the following steps:

[0052] 61) adding PETG particles and polybutylene terephthalate into a high-speed mixer, adding a lubricant and an antioxidant into the mixer, and starting the high-speed mixer to mix;

[0053] 62) the mixed particles are extruded and granulated by a twin-screw extruder at a speed of 160 r / min at 215-260° C.;

[0054] 63) Repeat the process twice to obtain uniformly mixed particles and dry the particles;

[0055] 64) The dried particles are extruded through a single screw extruder to obtain PETG filaments;

[0056] Among them, the diameter of PETG consumables is 1.75±0.5mm.

[0057] Example 2

[0058] like Figure 1 As shown, this embodiment provides a PETG consumable for 3D printing, comprising the following raw materials in parts by weight: 25 parts by weight of terephthalic acid, 11 parts by weight of ethylene glycol, 13 parts by weight of 1,4-cyclohexanedimethanol, 7 parts by weight of diethylene glycol, 15 parts by weight of ethylene glycol antimony, 19 parts by weight of sodium acetate, 32 parts by weight of polybutylene terephthalate, 10 parts by weight of lubricant and 13 parts by weight of antioxidant;

[0059] Wherein, polytetrafluoroethylene is selected as lubricant and butyl hydroxyphenol is selected as antioxidant.

[0060] A method for processing PETG consumables for 3D printing, comprising the following steps:

[0061] Step 1, accurately weighing terephthalic acid, ethylene glycol, 1,4-cyclohexanedimethanol, diethylene glycol, ethylene glycol antimony and sodium acetate, and then respectively putting them into a polymerization reactor;

[0062] Step 2, nitrogen is introduced into the polymerization reactor, and the air in the reactor is replaced with nitrogen three times, and the air in the reactor is discharged, and the pressure in the reactor is maintained at 0.22-0.25 MPa to carry out esterification reaction;

[0063] Wherein, the liquid temperature in the polymerization reactor during the esterification reaction is maintained at 220-240°C;

[0064] Wherein, replacing with nitrogen three times comprises the following steps:

[0065] 21) Pass nitrogen into the polymerization reactor for 5-10 minutes to allow the nitrogen to fully replace the air in the reactor;

[0066] 22) Exhaust the gas in the reactor through the exhaust valve at the bottom, and continue to introduce nitrogen to ensure that the air in the reactor is removed as much as possible;

[0067] 23) Repeat the above steps and perform nitrogen replacement three times in succession to ensure that the air in the kettle is basically eliminated;

[0068] 24) When all replacements are completed, turn off the nitrogen source and confirm that the kettle has been replaced with pure nitrogen;

[0069] Step 3: Control the outlet valve opening to control the outlet rate. When the outlet water volume is greater than 90% of the theoretical outlet water volume, the esterification pressure is reduced, the esterification liquid temperature is increased, and the esterification is completed.

[0070] Step 4: Slowly reduce the pressure to enter a low vacuum for pre-condensation. After the pre-condensation is completed, the liquid temperature in the kettle is raised to 275-283°C for final polycondensation. The vacuum degree in the kettle is lower than 70Pa; wherein the pre-condensation time is 45min;

[0071] Step 5: After the polycondensation is completed, the PETG particles are obtained by water-cooling the strips and then pelletizing them.

[0072] Step 6: PETG particles, polybutylene terephthalate, lubricant and antioxidant are mixed and granulated, and then dried and extruded to obtain PETG consumables;

[0073] The process of mixing and granulating, drying and then extruding to obtain PETG consumables comprises the following steps:

[0074] 61) adding PETG particles and polybutylene terephthalate into a high-speed mixer, adding a lubricant and an antioxidant into the mixer, and starting the high-speed mixer to mix;

[0075] 62) the mixed particles are extruded and granulated by a twin-screw extruder at a speed of 160 r / min at 215-260° C.;

[0076] 63) Repeat the process twice to obtain uniformly mixed particles and dry the particles;

[0077] 64) The dried particles are extruded through a single screw extruder to obtain PETG filaments;

[0078] Among them, the diameter of PETG consumables is 1.75±0.5mm.

[0079] Example 3

[0080] like Figure 1 As shown, this embodiment provides a PETG consumable for 3D printing, comprising the following raw materials in parts by weight: 30 parts by weight of terephthalic acid, 12 parts by weight of ethylene glycol, 15 parts by weight of 1,4-cyclohexanedimethanol, 9 parts by weight of diethylene glycol, 18 parts by weight of ethylene glycol antimony, 28 parts by weight of sodium acetate, 40 parts by weight of polybutylene terephthalate, 14 parts by weight of lubricant and 16 parts by weight of antioxidant;

[0081] Among them, silicone oil is selected as the lubricant and sodium sulfide is selected as the antioxidant.

[0082] A method for processing PETG consumables for 3D printing, comprising the following steps:

[0083] Step 1, accurately weighing terephthalic acid, ethylene glycol, 1,4-cyclohexanedimethanol, diethylene glycol, ethylene glycol antimony and sodium acetate, and then respectively putting them into a polymerization reactor;

[0084] Step 2, nitrogen is introduced into the polymerization reactor, and the air in the reactor is replaced with nitrogen three times, and the air in the reactor is discharged, and the pressure in the reactor is maintained at 0.22-0.25 MPa to carry out esterification reaction;

[0085] Wherein, the liquid temperature in the polymerization reactor during the esterification reaction is maintained at 220-240°C;

[0086] Wherein, replacing with nitrogen three times comprises the following steps:

[0087] 21) Pass nitrogen into the polymerization reactor for 5-10 minutes to allow the nitrogen to fully replace the air in the reactor;

[0088] 22) Exhaust the gas in the reactor through the exhaust valve at the bottom, and continue to introduce nitrogen to ensure that the air in the reactor is removed as much as possible;

[0089] 23) Repeat the above steps and perform nitrogen replacement three times in succession to ensure that the air in the kettle is basically eliminated;

[0090] 24) When all replacements are completed, turn off the nitrogen source and confirm that the kettle has been replaced with pure nitrogen;

[0091] Step 3: Control the outlet valve opening to control the outlet rate. When the outlet water volume is greater than 90% of the theoretical outlet water volume, the esterification pressure is reduced, the esterification liquid temperature is increased, and the esterification is completed.

[0092] Step 4: Slowly reduce the pressure to enter a low vacuum for pre-condensation. After the pre-condensation is completed, the liquid temperature in the kettle is raised to 275-283°C for final polycondensation. The vacuum degree in the kettle is lower than 70Pa; wherein the pre-condensation time is 40min;

[0093] Step 5: After the polycondensation is completed, the PETG particles are obtained by water-cooling the strips and then pelletizing them.

[0094] Step 6: PETG particles, polybutylene terephthalate, lubricant and antioxidant are mixed and granulated, and then dried and extruded to obtain PETG consumables;

[0095] The process of mixing and granulating, drying and then extruding to obtain PETG consumables comprises the following steps:

[0096] 61) adding PETG particles and polybutylene terephthalate into a high-speed mixer, adding a lubricant and an antioxidant into the mixer, and starting the high-speed mixer to mix;

[0097] 62) the mixed particles are extruded and granulated by a twin-screw extruder at a speed of 160 r / min at 215-260° C.;

[0098] 63) Repeat the process twice to obtain uniformly mixed particles and dry the particles;

[0099] 64) The dried particles are extruded through a single screw extruder to obtain PETG filaments;

[0100] Among them, the diameter of PETG consumables is 1.75±0.5mm.

[0101] Comparative Example 1

[0102] The PETG consumables for 3D printing and the processing method thereof provided in this embodiment are substantially the same as those in Embodiment 1, the main difference being that diethylene glycol is not added to the raw materials.

[0103] Comparative Example 2

[0104] The PETG consumable material for 3D printing and the processing method thereof provided in this embodiment are substantially the same as those in Embodiment 1, the main difference being that polybutylene terephthalate is not added to the raw material.

[0105] Comparative Example 3

[0106] The PETG consumables for 3D printing and the processing method thereof provided in this embodiment are substantially the same as those in Embodiment 1, the main difference being that sodium acetate is not added to the raw materials.

[0107] Performance testing and result analysis

[0108] The PETG consumables prepared in Examples 1-3 and Comparative Examples 1-3 were subjected to performance tests, including DSC test, TG test, printing hot bed temperature test and printing speed test, and the relevant data were recorded in Table 1;

[0109] Table 1: Test data record table

[0110]

[0111] It can be seen from Table 1 that, compared with Comparative Examples 1-3, the PETG consumables prepared in Examples 1-3 have excellent thermal decomposition temperature and good thermal stability. In the 3D printing process, the filaments of the consumables are smooth without faults, the warping height of the 3D printed products is small, and an excellent printing speed can be maintained during the printing process.

[0112] The present invention improves the fluidity of the consumables by adding diethylene glycol, so that the PETG consumables can flow out of the nozzle evenly during 3D printing, and are not prone to clogging or extrusion problems, thereby ensuring stable material supply during the printing process, avoiding suspension or distortion during the printing process, and ensuring printing quality while improving the printing speed. The PETG consumables have good thermal stability and can maintain stable performance at high temperatures, and are not prone to deterioration or thermal deformation, which helps to maintain stable printing quality at a higher printing speed. The smaller warping height during printing of the present invention indicates that the PETG printed part is less prone to warping and deformation after cooling, and can maintain good shape stability at a faster printing speed, thereby improving printing efficiency.

[0113] Although the present invention has been described in detail with reference to the aforementioned embodiments, it is still possible for those skilled in the art to modify the technical solutions described in the aforementioned embodiments, or to make equivalent substitutions for some of the technical features therein. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A PETG consumable for 3D printing, characterized in that: The invention comprises the following raw materials in parts by weight: 20-30 parts by weight of terephthalic acid, 10-12 parts by weight of ethylene glycol, 10-15 parts by weight of 1,4-cyclohexanedimethanol, 6-9 parts by weight of diethylene glycol, 12-18 parts by weight of ethylene glycol antimony, 15-28 parts by weight of sodium acetate, 25-40 parts by weight of polybutylene terephthalate, 8-14 parts by weight of a lubricant and 10-16 parts by weight of an antioxidant.

2. A PETG consumable for 3D printing according to claim 1, characterized in that: The lubricant is selected from any one of polytetrafluoroethylene and silicone oil.

3. The PETG consumable for 3D printing according to claim 1, characterized in that: The antioxidant is selected from any one of butyl hydroxyphenol, butyl hydroxybenzoate and sodium sulfide.

4. A method for processing PETG consumables for 3D printing, characterized in that: Using a PETG consumable for 3D printing as described in any one of claims 1 to 3, comprising the following steps: S1. Accurately weigh terephthalic acid, ethylene glycol, 1,4-cyclohexanedimethanol, diethylene glycol, antimony glycol and sodium acetate, and then put them into a polymerization reactor respectively; S2, nitrogen is introduced into the polymerization reactor, and the air in the reactor is replaced with nitrogen three times, and the pressure in the reactor is maintained at 0.22-0.25 MPa to carry out esterification reaction; S3, control the outlet valve opening to control the outlet rate. When the outlet water volume is greater than 90% of the theoretical outlet water volume, the esterification pressure decreases, the esterification liquid temperature increases, and the esterification ends. S4, slowly reducing the pressure to enter a low vacuum for pre-polycondensation. After the pre-polycondensation is completed, the liquid temperature in the kettle is raised to 275-283°C for final polycondensation reaction. The vacuum degree in the kettle is lower than 70Pa; S5, after the polycondensation is completed, the material is discharged through water-cooled strands and then pelletized to obtain PETG particles; S6, PETG particles, polybutylene terephthalate, lubricant and antioxidant are mixed and granulated, and then dried and extruded to obtain PETG consumables.

5. A method for processing PETG consumables for 3D printing according to claim 4, characterized in that: In step S2, the three times of replacement with nitrogen includes the following steps: S21, passing nitrogen into the polymerization reactor for 5-10 minutes to allow the nitrogen to fully replace the air in the reactor; S22, exhaust the gas in the reactor through the exhaust valve at the bottom, and continue to introduce nitrogen to ensure that the air in the reactor is removed as much as possible; S23, repeat the above steps, and perform nitrogen replacement three times continuously to ensure that the air in the kettle is basically eliminated; S24. When all replacements are completed, turn off the nitrogen gas source and confirm that the kettle has been replaced with pure nitrogen.

6. A method for processing PETG consumables for 3D printing according to claim 4, characterized in that: In step S2, the liquid temperature in the polymerization reactor during the esterification reaction is maintained at 220-240°C.

7. A method for processing PETG consumables for 3D printing according to claim 4, characterized in that: In step S4, the pre-polycondensation time is 40-45 minutes.

8. A method for processing PETG consumables for 3D printing according to claim 4, characterized in that: In step S6, the mixed granulation is dried and then extruded to obtain PETG consumables, which includes the following steps: S61, adding PETG particles and polybutylene terephthalate into a high-speed mixer, adding a lubricant and an antioxidant into the mixer, and starting the high-speed mixer for mixing; S62, the mixed particles are extruded and granulated at 215-260° C. by a twin-screw extruder at a speed of 160 r / min; S63, repeating twice to obtain uniformly mixed particles and drying the particles; S64. The dried particles are extruded through a single screw extruder to obtain PETG filaments.

9. A method for processing PETG consumables for 3D printing according to claim 4, characterized in that: In step S6, the diameter of the PETG consumable is 1.75±0.5 mm.