Welded member having excellent fatigue characteristics in welded portion
By controlling the Si, Mn and Cr content of the welding part and the shape of the weld bead, the welding process is optimized, the fatigue characteristics and corrosion problems of the welded parts are solved, and excellent durability and economical welding technology of high-strength steel are achieved.
Patent Information
- Application Number
- CN202380024552.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2023-02-21
- Filing Date
- 2023-03-27
- Publication Date
- 2024-10-15
AI Technical Summary
Existing welding technology has problems with fatigue properties and corrosion in high-strength steel automotive chassis components, especially weld metal defects and poor painting caused by gas shielded arc welding, which increases production costs and corrosion risks.
By controlling the Si, Mn and Cr content of the welding part and optimizing the weld bead shape, we ensure that the fatigue life of the welding part reaches more than 245,000 cycles, while reducing the fatigue damage sensitivity of the welding part, using constant voltage controlled gas shielded arc welding technology. , utilizing the current flow between the front end of the welding wire and the molten metal to enhance the welding process.
It effectively improves the low-cycle/high-cycle fatigue life of the welded part, reduces the fatigue damage sensitivity of the welded part, enhances the corrosion resistance and durability of the welded part, and ensures the excellent fatigue characteristics and economy of the welded parts.
Smart Images

Figure CN118786002A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a welded component having excellent fatigue properties at a welded portion. More specifically, the present invention relates to a gas shielded arc welded portion that can ensure excellent durability and economy required for manufacturing parts. Background Art
[0002] In the automotive industry, due to fuel efficiency regulations for environmental protection such as global warming, the research on technologies to reduce the weight of vehicle bodies and parts is becoming a major issue. Chassis parts, which are crucial to the driving performance of automobiles, also need to follow this trend and use high-strength steel to reduce weight.
[0003] In order to achieve such lightweight components, the strength of the material must be improved, and ensuring the durability of components made of high-strength steel under repeated fatigue loads is an important factor.
[0004] However, when assembling automobile chassis parts, arc welding is mainly used to ensure strength, and arc welding is achieved by melting the welding wire to achieve lap welding between parts, so it is inevitable that the connection part has a geometric shape. Such a connection part becomes a repeated fatigue stress concentration part (notch effect) and becomes the starting point of fracture, which eventually leads to a decrease in the durability of the parts, so there is a limitation that the advantage of using high-strength steel is lost.
[0005] Therefore, in order to improve the fatigue characteristics of the weld, it is most important to reduce the angle (toe angle) of the end of the weld bead where the main stress is concentrated, and controlling the material and stress of the weld toe is an important factor. In addition, as mentioned above, due to the trend of high strength and lightweight of parts, the material is thinner, and the demand for rust resistance to prevent penetration corrosion has also increased. As a result, the use of coated steel tends to increase, but the weld metal of arc welding does not have a coating, so there is a limitation that the corrosion resistance after painting is poor compared with the base material. Therefore, there is a problem that the weld of the chassis parts made of coated steel plates will corrode early in the harsh corrosive environment when the vehicle is running and the fatigue characteristics will decrease. On the other hand, when gas shielded arc welding is performed on coated steel, due to the generation of zinc and other vapors, a large number of pits and pore-like pore defects will appear in the weld, and there is a concern that the strength of the weld will decrease, so the reduction in welding productivity has become a problem. In addition, for general uncoated steel, the slag generated in the weld during gas shielded arc welding can also cause poor painting, which becomes a factor in reducing corrosion resistance after painting. Therefore, when manufacturing parts, there is a problem of increased costs due to post-processing processes such as pickling or brushing to remove the slag after welding.
[0006] Recently, the development of lightweight chassis parts for next-generation environmentally friendly vehicles has been actively carried out, and in particular, the development of welding technology that can improve the characteristics of welded parts while ensuring economic efficiency has become an important issue. Summary of the invention
[0007] 1. Technical issues to be resolved
[0008] The present invention aims to provide a gas shielded arc welded component capable of ensuring excellent fatigue properties in the field of the automotive industry.
[0009] The problems of the present invention are not limited to the above-mentioned contents. Additional problems of the present invention are described throughout the specification, and it is not difficult for a person skilled in the art to understand the additional problems of the present invention from the contents described in the specification of the present invention.
[0010] (II) Technical solution
[0011] One aspect of the present invention relates to a welded component having excellent fatigue properties at a welded portion, wherein:
[0012] The welding component comprises a base material; and a welding portion,
[0013] The weld portion contains, in weight %, C: 0.001 to 0.30%, Si: 1.00% or less and excluding 0%, Mn: 0.50 to 3.00%, P: 0.030% or less and excluding 0%, S: 0.030% or less and excluding 0%, Cr: 1.50% or less and excluding 0%, Mo: 0.60% or less and excluding 0%, Al: less than 0.10% and excluding 0%, Ni: 0.40% or less and excluding 0%, Ti: less than 0.10% and excluding 0%, Fe and other inevitable impurities in the balance, and satisfies the following relationship 1, and
[0014] The weld bead shape of the weld portion satisfies the following Relationship 2.
[0015] [Equation 1]
[0016] 0.30≤[Si]+0.25×([Mn]+[Cr])≤0.66
[0017] In the above relational expression 1, [Si], [Mn], and [Cr] represent the contents (weight %) of the respective elements in parentheses with respect to the weld portion.
[0018] [Equation 2]
[0019] e1 / b2≤0.35
[0020] In the relation 2, Figure 1As described above, e1 represents the distance from the point where a line connected from the weld root of the lap weld along a direction perpendicular to the lower plate intersects with a line connected from the weld toe of the lower plate to the weld toe of the upper plate, and b2 represents the distance from the weld toe of the lower plate to the weld root.
[0021] The weld bead shape of the weld portion may further satisfy the following relational expression 3.
[0022] [Equation 3]
[0023] θ2-θ1≥34°
[0024] In the relation 3, Figure 2 As shown, θ1 represents the internal angle formed by a line parallel to the reference plane on the lower plate and a line connecting the weld toe of the lower plate to the weld toe of the upper plate, and θ2 represents the internal angle formed by a line parallel to the lower reference plane of the upper plate of the lap weld and a line connecting the weld root to the weld toe of the upper plate.
[0025] The weld may further include, in weight %, one or more of Nb: 0.10% or less, V: 0.10% or less, Zr: 0.10% or less, and B: 0.01% or less.
[0026] The weld may further include Cu: 0.50% or less in terms of weight %.
[0027] The welded portion can meet a fatigue life of more than 245,000 cycles under a maximum load of 10.1 kN (a ratio of the minimum load to the maximum load of 0.1 and a repetitive load frequency of 15 Hz).
[0028] In terms of weight%, the base material may include C: 0.04-0.18%, Si: 2.0% or less and including 0%, Mn: 0.5-3.0%, Cr: 2.0% or less and including 0%, Mo: 2.0% or less and including 0%, Al: 0.01-0.10%, P: 0.05% or less and excluding 0%, S: 0.05% or less and excluding 0%, and the balance Fe and other inevitable impurities.
[0029] The base material may further contain, in weight %, one or more of Ti: 0.20% or less, Nb: 0.10% or less, and Cu: 0.10% or less.
[0030] The base material may have a thickness of 0.8 to 4.0 mm.
[0031] Furthermore, another aspect of the present invention relates to an automobile component including the welding member.
[0032] (III) Beneficial effects
[0033] According to the present invention described above, as a next-generation welding technology that ensures performance and cost competitiveness in sync with the era of widespread electric vehicles, a gas shielded arc weld having excellent weld fatigue characteristics can be effectively provided.
[0034] Various beneficial advantages and effects of the present invention are not limited to the above contents and can be more easily understood in the process of describing the specific embodiments of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] Figure 1 1 is a diagram showing factors for determining the shape of a weld bead of an overlap weld portion obtained by overlap welding of steel plates in one embodiment of the present invention.
[0036] Figure 2 1 is another view showing factors for determining the weld bead shape of the lap weld portion obtained by lap welding of steel plates in one embodiment of the present invention. DETAILED DESCRIPTION
[0037] The present invention is described below.
[0038] The present invention is characterized in that the Si, Mn and Cr contents of the weld are controlled in order to ensure the excellent fatigue properties of the weld. As a result of the control of the contents of these component elements, in the gas shielded arc welding which is usually controlled by constant voltage, the current flows through the arc column between the front end of the welding wire and the molten metal, that is, the arc force is strengthened, so that the position with the maximum penetration depth can be moved from the outer side of the lower plate of the lap weld connection (toe direction) to the weld root side where the upper plate and the lower plate meet the weld metal, thereby achieving the effect of improving the low-cycle fatigue life under the application of relatively high fatigue load. Here, the low-cycle fatigue life is defined as less than 245,000 cycles, and the high-cycle fatigue life is defined as more than 245,000 cycles.
[0039] In addition, the present invention controls the weld bead of the weld to a predetermined shape by controlling the Si, Mn and Cr contents of the weld as described above, thereby reducing the fatigue damage sensitivity at the weld root and weld toe of the lap weld, thereby improving the low-cycle / high-cycle fatigue life of the weld, and at the same time further reducing the fatigue damage sensitivity at the weld toe, thereby obtaining a high-cycle fatigue life that can further improve relatively low fatigue loads.
[0040] First, a welded component according to one aspect of the present invention is described. The welded component of the present invention comprises a base material and a weld. At this time, the alloy composition of the weld is first described. The content of the alloy composition described below is weight %.
[0041] C:0.001~0.30%
[0042] The C is a main element, which can reduce the starting temperature of the acicular ferrite, bainite and martensite phase transformation based on non-diffusion phase transformation according to the continuous cooling in the high-temperature austenite phase during the solidification process of the weld metal. If the C content is less than 0.001%, the hardening performance is reduced, not only it is difficult to ensure the sufficient strength of the weld metal, but also due to the above-mentioned principle, the starting temperature of the low-temperature phase transformation will not be sufficiently reduced, so the tensile residual stress offset effect of the weld based on the low-temperature phase transformation expansion effect during the cooling process will be significantly reduced, and there may be a disadvantage of not being able to form a large-angle grain boundary structure with a large orientation angle difference between grains. On the other hand, if the C content is greater than 0.30%, the viscosity of the molten metal is reduced, not only the weld shape becomes poor, but also it will cause the weld metal to be over-hardened, and there may be a disadvantage of reduced toughness.
[0043] Si: 1.00% or less and excluding 0%
[0044] The Si is an element that promotes deoxidation of the molten metal during arc welding (deoxidizing element), which is beneficial to suppress the generation of pores and increase the starting temperature of low-temperature phase transformation. On the other hand, if the Si content is greater than 1.00%, a lot of non-conductive slag is generated, resulting in poor painting of the weld, and due to excessive deoxidation, the surface activation of the weld is insufficient, which may result in a disadvantage of reduced penetration of the molten metal. Therefore, in the present invention, it is preferred to control the Si content to 1.00% or less. The Si content is further preferably 0.75% or less, more preferably 0.50% or less, and most preferably 0.25% or less.
[0045] Mn: 0.50~3.00%
[0046] Mn is a deoxidizing element, which promotes the deoxidation of the molten metal during arc welding, helps to suppress the generation of pores, and reduces the low-temperature phase transformation start temperature like C. If the content of Mn is less than 0.5%, the deoxidation effect is insufficient, and there may be a disadvantage that pores are easily generated. On the other hand, if the content of Mn is more than 3.0%, the viscosity of the molten metal becomes too high, and when the welding speed is fast, the molten metal cannot flow into the welding part properly, and there may be a disadvantage that the weld bead shape is easily poor due to the formation of a humping weld. More preferably, the Mn content is limited to 2.50% or less.
[0047] Cr: 1.50% or less and 0% or less
[0048] The Cr is a ferrite stabilizing element, which lowers the low temperature transformation start temperature and is useful for improving the strength by ensuring the hardenability of the weld metal. If the Cr content is greater than 1.50%, the brittleness of the weld metal may increase unnecessarily in some cases, and there may be a disadvantage that it is difficult to ensure sufficient toughness. The Cr content is more preferably 1.40% or less, further preferably 1.30% or less, and most preferably 1.20% or less.
[0049] Mo: 0.60% or less and excluding 0%
[0050] Mo is a ferrite stabilizing element and is useful for ensuring hardening properties that improve the strength of the weld metal. If the content of Mo is greater than 0.60%, there may be a disadvantage that the toughness of the weld metal decreases in some cases.
[0051] P: 0.030% or less and excluding 0%
[0052] P is an element that is usually mixed as an inevitable impurity in steel and is also an element that is generally contained as an impurity in solid wire for arc welding. If the content of P is greater than 0.030%, there may be a disadvantage that high temperature cracking of the weld metal becomes apparent.
[0053] S: 0.030% or less and excluding 0%
[0054] The S is an element that is usually mixed as an inevitable impurity in steel, and is also an element contained as a regular impurity in solid wire for arc welding. If the S content is more than 0.030%, the toughness of the weld metal deteriorates in some cases, the surface tension of the molten metal is insufficient during welding, and the molten part flows out excessively due to gravity during rapid vertical welding (welding from top to bottom in vertical welding), which may cause the weld bead shape to become poor.
[0055] Al: less than 0.10% and excluding 0%
[0056] The Al is a deoxidizing element, and even in a trace amount, it can promote the deoxidation of the molten metal during arc welding, thereby improving the strength of the weld metal. In order to ensure the above-mentioned effect, the lower limit of the Al content is 0%. If the Al content is 0.10% or more, the generation of Al-based oxides increases, and in some cases the strength and toughness of the weld metal decrease, and there may be a disadvantage that the weld part becomes sensitive to poor electroplating caused by non-conductive oxides. More preferably, the Al content is limited to less than 0.07%.
[0057] Ti: less than 0.10% and excluding 0%
[0058] The Ti is a deoxidizing element, and even in a trace amount, it can promote the deoxidation of the molten metal during arc welding, thereby improving the strength of the weld metal. In addition, it can promote the development of acicular ferrite that can improve the toughness of the weld. In order to ensure the above-mentioned effects, the lower limit of the Ti content is 0%. If the Ti content is 0.10% or more, the generation of Ti-based oxides increases, and there may be a disadvantage that the strength and toughness of the weld metal decrease in some cases. More preferably, the Ti content is limited to less than 0.07%.
[0059] Ni: 0.40% or less and excluding 0%
[0060] The Ni is an element that can improve the strength and toughness of the weld metal. In order to ensure the above-mentioned effects, the lower limit of the Ni content is 0%. However, if the Ni content is greater than 0.40%, there may be a disadvantage of being sensitive to cracking, so the Ni content is set to 0.40% or less. The Ni content is more preferably 0.30% or less, further preferably 0.20% or less, and most preferably 0.10% or less.
[0061] Although not particularly limited, according to one embodiment of the present invention, optionally, the welding component may further include one or more of Nb: 0.10% or less, V: 0.10% or less, Zr: 0.10% or less, and B: 0.01% or less.
[0062] Nb: 0.10% or less
[0063] Nb is an element that can improve the strength and toughness of weld metal by improving hardenability and making the microstructure dense. In addition, it has the effect of improving the flow of molten metal and stabilizing the arc during arc welding. However, if the content of Nb is greater than 0.10%, low melting point compounds are formed at the grain boundaries, which may easily cause high temperature cracking.
[0064] V: 0.10% or less
[0065] The V is an element that can improve the strength and toughness of the weld metal by improving the hardenability and making the microstructure dense. In addition, the V is a precipitation strengthening element that can improve the strength of the weld metal by generating carbonitrides. However, if the V content is greater than 0.10%, there may be a disadvantage that the toughness of the weld metal decreases in some cases due to excessive strength caused by excessive precipitates. Therefore, the V content is set to 0.10% or less.
[0066] Zr: 0.10% or less
[0067] The Zr is an element that promotes deoxidation of molten metal during arc welding (deoxidizing element), and is helpful in suppressing the generation of pores. However, if the content of the Zr is greater than 0.10%, there may be a disadvantage that the electroplating property of the welded part is reduced. Therefore, the Zr content is set to 0.10% or less.
[0068] B: 0.01% or less
[0069] B is an element that improves the strength of the weld metal by improving the hardenability. However, if the content of B is greater than 0.01%, the toughness of the weld metal may decrease in some cases due to excessive hardenability. Therefore, the B content is set to 0.01% or less.
[0070] In addition, although not particularly limited, according to one embodiment of the present invention, optionally, the welding part may further include Cu: 0.50% or less in terms of weight %.
[0071] Cu: 0.50% or less
[0072] The Cu is an element that effectively improves the strength of the weld metal. However, if the Cu content is greater than 0.50%, there may be a disadvantage that the crack sensitivity of the weld metal becomes high. The Cu content is more preferably 0.45% or less, further preferably 0.40% or less, and most preferably 0.30% or less. On the other hand, in order to fully obtain the effect of improving the strength, the weld metal may contain 0.01% or more of the Cu.
[0073] In addition, the remaining component of the present invention is iron (Fe). However, unexpected impurities are inevitably mixed into the raw materials or the surrounding environment during the conventional manufacturing process, so the mixing of impurities is not excluded. The impurities are impurities known to any ordinary technician, so all relevant contents are not specifically mentioned in the present invention.
[0074] Relation 1
[0075] The present invention also controls the contents of Si, Mn and Cr to satisfy the following relational expression 1. As a result of the control of the contents of these component elements, in the gas shielded arc welding which is usually controlled by constant voltage, the position with the maximum penetration depth is moved from the outer side (toe direction) of the lower plate of the lap weld connection to the weld root side where the upper plate and the lower plate meet the weld metal by the current flow through the arc column between the front end of the welding wire, that is, the arc force is strengthened, so that the effect of improving the low-cycle fatigue life to which a relatively high fatigue load is applied can be obtained. Here, the low-cycle fatigue life is defined as less than 245,000 cycles, and the high-cycle fatigue life is defined as more than 245,000 cycles. If the value defined by the following relational expression 1 is less than 0.30, despite the above-mentioned effect, the generation of pore defects in the weld becomes sensitive due to insufficient deoxidation of the weld, and the problem of reduced fatigue strength of the weld may occur instead, and if the value defined by the following relational expression 1 is greater than 0.66, the problem of difficulty in controlling the position with the maximum penetration depth in the above-mentioned lap weld to move to the weld root side may occur. More preferably, the contents of Si, Mn and Cr are controlled so that the values defined by the following relational expression 1 satisfy 0.35 to 0.60.
[0076] [Equation 1]
[0077] 0.30≤[Si]+0.25×([Mn]+[Cr])≤0.66
[0078] In the above relational expression 1, [Si], [Mn], and [Cr] represent the contents (weight %) of the respective elements in parentheses with respect to the weld portion.
[0079] On the other hand, the weld bead constituting the welded part of the present invention preferably has a predetermined shape. Specifically, the welding ratio of the welded part is preferably controlled to a value defined by the following relational expression 2 to be 0.35 or less.
[0080] [Equation 2]
[0081] e1 / b2≤0.35
[0082] In the relation 2, Figure 1 As described above, e1 represents the distance from the point where a line connected from the weld root of the lap weld along a direction perpendicular to the lower plate intersects with a line connected from the weld toe of the lower plate to the weld toe of the upper plate, and b2 represents the distance from the weld toe of the lower plate to the weld root.
[0083] The reason why the weld bead shape of the overlapped weld obtained by welding is limited to the one shown in the above-mentioned relational expression 2 is that, according to the principle of the above-mentioned relational expression 1, the position with the maximum penetration depth of the overlapped weld is appropriately moved from the outer side of the lower plate (toe direction) to the root side, thereby reducing the fatigue damage sensitivity at the root. At the same time, when the value of e1 in relational expression 2 is lower than the value of b2 by an appropriate proportion, fatigue damage can be prevented at the toe, and the high-cycle fatigue life under relatively low fatigue load can be effectively improved. If the value defined by relational expression 2 is greater than 0.35, the fatigue damage of the toe becomes sensitive under relatively low fatigue load, and the problem of shortening the high-cycle fatigue life may occur. More preferably, the value defined by relational expression 2 is controlled to be less than 0.30.
[0084] Furthermore, in the present invention, the weld bead shape of the weld portion is more preferably formed to satisfy the following Relational Expression 3.
[0085] [Equation 3]
[0086] θ2-θ1≥34°
[0087] In the relation 3, Figure 2 As shown, θ1 represents the internal angle formed by a line parallel to the reference plane on the lower plate and a line connecting the weld toe of the lower plate to the weld toe of the upper plate, and θ2 represents the internal angle formed by a line parallel to the lower reference plane of the upper plate of the lap weld and a line connecting the weld root to the weld toe of the upper plate.
[0088] The reason for controlling the weld bead shape as shown in the relational expression 3 is that, according to the principles of the above-mentioned relational expressions 1 and 2, the fatigue damage sensitivity is reduced at the weld root and weld toe of the overlap weld, thereby improving the low-cycle / high-cycle fatigue life of the weld, and at the same time, the fatigue damage sensitivity is further reduced at the weld toe to further improve the high-cycle fatigue life of relatively low fatigue loads. If the value of θ2 decreases, the fatigue stress concentration at the weld root decreases, but the fatigue stress concentration at the weld toe increases, and if the value of θ1 decreases, the fatigue stress concentration at the weld toe decreases, but the fatigue stress concentration at the weld root increases. Therefore, through the research of the present invention, it is found that according to the above-mentioned principle, when the values defined by the relational expressions 1 and 2 are controlled to appropriate values, and the value defined by the relational expression 3 is controlled to be above 34°, the low-cycle / high-cycle fatigue life of the overlap weld can be effectively improved at the same time. If the value defined by the relational expression 3 is less than 34°, even if the low-cycle fatigue life of the weld increases, the problem of shortening the high-cycle fatigue life may occur.
[0089] On the other hand, in the present invention, there is no particular limitation on the alloy composition of the parent material. However, as an example, in terms of weight %, the parent material may include C: 0.04-0.18%, Si: 2.0% or less and including 0%, Mn: 0.5-3.0%, Cr: 2.0% or less and including 0%, Mo: 2.0% or less and including 0%, Al: 0.01-0.10%, P: 0.05% or less and 0% excluding, S: 0.05% or less and 0% excluding, Fe and other inevitable impurities in the balance. In addition, optionally, the parent material may also include one or more of Ti: 0.20% or less and including 0%, Nb: 0.10% or less and including 0% and Cu: 0.10% or less and including 0%. In addition, the parent material may have a thickness of 0.8-4.0 mm.
[0090] In addition, in the present invention, the specific composition of the welding wire used to form the welded portion is not limited. As an example, the following solid welding wire can be used: in terms of weight %, the solid welding wire contains C: 0.001-0.30%, Si: 0.25% or less and excluding 0%, Mn: 0.50-3.00%, P: 0.030% or less and excluding 0%, S: 0.030% or less and excluding 0%, Cr: 1.50% or less and excluding 0%, Mo: 0.60% or less and excluding 0%, Al: less than 0.10% and excluding 0%, Ni: 0.40% or less and excluding 0%, Cu: 0.50% or less and excluding 0%, Ti: less than 0.10% and excluding 0%, and the balance is Fe and other inevitable impurities. In addition, optionally, the welding wire composition may further include one or more of Nb: 0.10% or less, V: 0.10% or less, and Zr: 0.10% or less, or may further include B: 0.01% or less.
[0091] On the other hand, in the present invention, the type of shielding gas used in the welding of the base material is not particularly limited. As the shielding gas, 100% CO2 gas, Ar+20CO2 gas, Ar+10%CO2 gas, Ar+5%CO2 gas, Ar+2%O2 gas, etc. can be used. However, when Ar+5-20%CO2 is used as the shielding gas, the significant effect of the present invention can be exerted. That is, in the present invention, in order to ensure the tensile strength of the welded part without the occurrence of weld metal or fuse rupture, it is preferred that 5-20% CO2 is mixed in Ar as the shielding gas during the welding.
[0092] Modes for Carrying Out the Invention
[0093] Hereinafter, the present invention is further described in detail by examples. However, it should be noted that the following examples are only used to illustrate the present invention and are not intended to limit the scope of the present invention. Because the scope of the present invention depends on the contents recorded in the claims and the contents reasonably derived therefrom.
[0094] (Example)
[0095]
Table 1
[0096]
[0097]
Table 2
[0098]
[0099] * The balance in Table 2 above is Fe and unavoidable impurities.
[0100] Two pieces (a pair of 135 mm and 110 mm in length) of four hot-rolled pickled steel plate base materials having alloy compositions as shown in Table 1 above were prepared respectively, with a thickness of 2.0 mm, a width of 150 mm, a length of 135 mm and 110 mm, and a tensile strength of 380 MPa (steel material 1), 540 MPa (steel material 2), 670 MPa (steel material 3), and 780 MPa (steel material 4). In addition, solid wires for gas shielded arc welding having alloy compositions as shown in Table 2 above were prepared.
[0101] Next, the hot-dip galvanized steel sheets were overlapped using the solid welding wires. At this time, pulse current (Pulse DC) (shielding gas: Ar+20% CO2) was used as the welding method, and the shielding gas flow rate was 20 l / min. The angle of the welding torch was 45° relative to the vertical direction of the base material, the protruding length of the welding wire was 15 mm, and the welding current / voltage / speed conditions were 200A-20V-80cm / min. In addition, the overlap gap (Gap) was 0 mm and the overlap length was 25 mm.
[0102] On the other hand, welding was started at a position 10 mm from the starting point in the width direction of the welding base material, the welding length was 130 mm, and then welding was ended at a position 10 mm from the end point on the opposite side of the welding starting position.
[0103] For each weld formed by the welding, the microstructure of the cross section perpendicular to the longitudinal direction at the center of the weld in the longitudinal direction was observed with an optical microscope to confirm the area of the weld metal in advance, and the area was cut into a fine chip shape. Next, for each chip sample, the chemical composition of the weld metal was measured by an emission spectrometry method based on high-frequency inductively coupled plasma (ICP), and the results are shown in Table 3 below.
[0104] Furthermore, factors for determining the bead shape of the weld portion formed by the welding were determined, and the values of each factor according to these factors are shown in Table 4 below, and the values of Relational Expressions 2 and 3 were calculated and recorded.
[0105] In the following Table 4, the units of a, b1, b2, e1, e2 are mm, and the units of θ1, θ2 are °, which are respectively defined as follows.
[0106] First, if Figure 1 As mentioned above, a represents the length of a line connected perpendicularly to the weld root from the point where a line connecting the boundary point (weld root) where the upper plate and the lower plate of the self-lap weld meet the weld metal in a direction perpendicular to the lower plate intersects with a line connected from the end (weld toe) of the weld metal of the lower plate. Relative to the thickness of the base material (mm), this length can be more than 77%.
[0107] b1 represents the length from the point where a line connected from the weld root in a direction perpendicular to the lower plate intersects with a line connected from the weld toe to the weld root, and this length can be more than 99% relative to the base material thickness (mm).
[0108] b2 represents the length from the weld toe to the weld root of the lower plate, which can be more than 99% of the base material thickness (mm).
[0109] e1 represents the length from the point where a line connected from the weld root in a direction perpendicular to the lower plate intersects with a line connected from the weld toe of the lower plate to the end (weld toe) of the weld metal of the upper plate. This length can be more than 11% relative to the thickness of the base material (mm).
[0110] e2 represents the maximum penetration depth of the weld metal in the vertical direction from the line parallel to the reference surface on the lower plate. Relative to the thickness of the parent material (mm), this length can be more than 11%.
[0111] In addition, as attached Figure 2 As shown, θ1 represents the internal angle formed by a line parallel to the reference surface on the lower plate and a line connecting the weld toe of the lower plate to the weld toe of the upper plate.
[0112] like Figure 2 As shown, θ2 represents the internal angle formed by a line parallel to the lower reference surface of the upper plate and a line connecting the weld root to the weld toe of the upper plate.
[0113] In addition, fatigue properties were measured for the welded portion formed by welding as described above, and the results are shown in Table 5 below. At this time, the specific fatigue property measurement method is as follows: First, a rectangular sample with a width of 50 mm and a length of 220 mm was collected from the center of each welding sample, and then a rectangular sample with a width of 50 mm and a length of 40 mm was placed at both ends in the length direction of the fatigue sample as a spacer (Spacer), and welded by two-point resistance spot welding. This is to ensure that the sample remains uniaxial during the tensile fatigue test. Next, a tensile-tensile fatigue test was performed under three load conditions with maximum load values of 10.1 kN, 9.1 kN and 8.1 kN to determine the fatigue life (number of cycles), at which the ratio of the minimum load to the maximum load (minimum load / maximum load) was 0.1, and the repetitive load frequency was 15 Hz. In addition, the minimum load refers to the minimum value of the repetitive load with the above-mentioned constant load application frequency, and the maximum load refers to the maximum value of the repetitive load.
[0114]
Table 3
[0115]
[0116] * The balance in Table 3 above is Fe and unavoidable impurities.
[0117]
Table 4
[0118]
[0119]
[0120]
Table 5
[0121]
[0122] As shown in Tables 1-5 above, for Inventive Examples 1-4, in which the alloy composition of the weld is optimally controlled to satisfy Relationship 1 and the weld bead shape is optimally controlled, that is, in which Relationships 2-3 are satisfied, it can be confirmed that a welded component having relatively excellent fatigue properties can be obtained. In contrast, for Comparative Examples 1-4, since Relationship 1 of the alloy composition of the weld is not satisfied and Relationships 2-3 of the weld bead shape are not satisfied, the results show that the low-cycle / high-cycle fatigue life under all fatigue test load conditions evaluated is worse than that of Inventive Examples 1-4.
Claims
1. A welded component having excellent fatigue properties at a welded portion, in, The welding component comprises a base material; and a welding portion, The weld portion contains, in weight %, C: 0.001 to 0.30%, Si: 1.00% or less and excluding 0%, Mn: 0.50 to 3.00%, P: 0.030% or less and excluding 0%, S: 0.030% or less and excluding 0%, Cr: 1.50% or less and excluding 0%, Mo: 0.60% or less and excluding 0%, Al: less than 0.10% and excluding 0%, Ni: 0.40% or less and excluding 0%, Ti: less than 0.10% and excluding 0%, Fe and other inevitable impurities in the balance, and satisfies the following relationship 1, and The weld bead shape of the welded portion satisfies the following relational expression 2: [Equation 1] 0.30≤[Si]+0.25×([Mn]+[Cr])≤0.66 In the above relational formula 1, [Si], [Mn], and [Cr] represent the contents (weight %) of the respective elements in parentheses with respect to the weld portion. [Equation 2] e1 / b2≤0.35 In the relational expression 2, as shown in FIG. 1 , e1 represents the distance from the point where a line connected from the weld root of the lap weld in a direction perpendicular to the lower plate intersects with a line connected from the weld toe of the lower plate to the weld toe of the upper plate, and b2 represents the distance from the weld toe of the lower plate to the weld root.
2. The welded component having excellent weld fatigue properties according to claim 1, in, The weld bead shape of the welded portion further satisfies the following relational expression 3, [Equation 3] θ2-θ1≥34° In the relationship 3, as shown in Figure 2, θ1 represents the internal angle formed by a line parallel to the reference plane on the lower plate and a line connected from the weld toe of the lower plate to the weld toe of the upper plate, and θ2 represents the internal angle formed by a line parallel to the lower reference plane of the upper plate of the lap weld and a line connected from the weld root to the weld toe of the upper plate.
3. The welded component having excellent weld fatigue properties according to claim 1, in, The weld portion further includes, in weight %, one or more of Nb: 0.10% or less, V: 0.10% or less, Zr: 0.10% or less, and B: 0.01% or less.
4. The welded component having excellent weld fatigue properties according to claim 1, in, The welded portion further includes, in weight %, Cu: 0.50% or less.
5. The welded component having excellent weld fatigue properties according to claim 1, in, The welded portion meets a fatigue life of more than 245,000 cycles under a maximum load of 10.1 kN (a ratio of a minimum load to a maximum load of 0.1 and a repetitive load frequency of 15 Hz).
6. The welded component having excellent weld fatigue properties according to claim 1, in, In terms of weight %, the base material includes C: 0.04-0.18%, Si: 2.0% or less and including 0%, Mn: 0.5-3.0%, Cr: 2.0% or less and including 0%, Mo: 2.0% or less and including 0%, Al: 0.01-0.10%, P: 0.05% or less and excluding 0%, S: 0.05% or less and excluding 0%, and the balance is Fe and other inevitable impurities.
7. The welded component having excellent weld fatigue properties according to claim 6, in, The base material further contains, in weight %, at least one of Ti: 0.20% or less, Nb: 0.10% or less, and Cu: 0.10% or less.
8. The welded component having excellent weld fatigue properties according to claim 1, in, The base material has a thickness of 0.8 to 4.0 mm.
9. An automobile component comprising the welded part according to claim 1.