Preparation method of flower-shaped spherical silver powder

By combining the liquid phase chemical reduction method with the use of polysodium disulfide dipropane sulfonate and ascorbic acid, combined with the dropwise addition of dispersants and self-assembly methods, the problems of complex processes and unstable structures in the existing technology are solved, and a fabric suitable for photovoltaics is prepared. The highly stable flower-shaped spherical silver powder of the battery's low-temperature silver paste improves conductivity and lifespan.

CN118808668AActive Publication Date: 2024-10-22XIAMEN UNIV

Patent Information

Application Number
CN202410911546.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-09
Publication Date
2024-10-22
Estimated Expiration
2044-07-09

AI Technical Summary

Technical Problem

The process for preparing micro-nano-scale flower-like silver powder in the existing technology is complex, environmentally unfriendly, high energy consumption, poor repeatability, many impurities, and the structure of the silver powder is unstable, resulting in poor conductivity and short life of photovoltaic silver paste.

Method used

A liquid-phase chemical reduction method is used, adding sodium polydisulfide propane sulfonate (SPS) as the precursor, ascorbic acid as the reducing agent, and using dispersants such as xanthan gum, polyvinylpyrrolidone (PVP) and sodium carboxymethylcellulose. (CMC-Na), etc., prepared flower-shaped spherical silver powder through dropping and self-assembly methods, avoiding the introduction of seed crystals and additional adjustment of reaction conditions.

Benefits of technology

The prepared flower-shaped spherical silver powder has high stability, uniform conductive network, is suitable for low-temperature sintering, reduces preparation costs and process complexity, and is suitable for low-temperature silver paste applications in photovoltaic cells.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118808668A_ABST
    Figure CN118808668A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of flower-shaped spherical silver powder, which comprises the following steps: (1) firstly preparing a silver nitrate solution, then adding sodium 3, 3 '-dithiodipropane sulfonate into the silver nitrate solution, and stirring until the sodium 3, 3'-dithiodipropane sulfonate is fully dissolved to obtain a precursor solution; (2) firstly preparing a reducing agent solution, then adding a dispersing agent, and stirring until the materials are uniformly mixed to obtain a reducing agent-dispersing agent mixed solution; (3) in a dark environment, dropwise adding the precursor solution and the reducing agent-dispersing agent mixed solution into deionized water which is being stirred, and curing after dropwise adding to obtain a silver colloid solution; and (4) sequentially centrifuging, washing and drying the silver colloid solution to obtain the flower-shaped spherical silver powder. The method has the advantages of being simple, efficient, low in cost, large in process window and the like, and subsequent commercialized mass production is facilitated.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of conductive material preparation, and particularly relates to a method for preparing flower-shaped spherical silver powder. Background Art

[0002] Silver has unique antibacterial, conductive, and catalytic properties, so it is widely used in microelectronics, catalysts, biomedicine, conductive pastes, and other fields. At present, researchers at home and abroad have studied and prepared silver particles with various special morphologies, including but not limited to spheres, flakes, dendrites, cubes, flowers, lines, triangles, etc. Among them, flower-shaped silver powder has attracted widespread attention from researchers due to its special physical and chemical properties.

[0003] In recent years, the photovoltaic industry has developed rapidly, and conductive silver paste is a key material for photovoltaic cells. As the conductive phase of conductive silver paste, the importance of silver powder is self-evident. Today, photovoltaic technology is moving towards the third generation of technological change, among which HJT technology is widely favored by companies in the photovoltaic industry. HJT batteries need to use low-temperature silver paste, and low-temperature silver paste requires that the silver powder used has good low-temperature sintering properties and volume resistivity. Silver nanowires are not considered due to their high preparation cost. The orientation of micro-nano flaky silver powder during printing will lead to uneven conductivity. Flower-shaped silver powder has many contact points and good low-temperature sintering activity, which is more suitable as the conductive phase of low-temperature silver paste.

[0004] At present, the liquid phase chemical reduction method is often used to prepare flower-shaped silver powder of micro-nano scale in the prior art, but most reaction systems have problems such as complicated process flow, environmental unfriendliness, high energy consumption, poor repeatability, many impurities, and unstable flower-shaped structure of silver powder. The technical solutions disclosed in CN 103273082 A and CN 103551589 A introduce iron elements in the preparation process, which is difficult to clean. The residual iron elements will cause the poor conductivity of photovoltaic silver paste and short life. In addition, the flower-shaped structure of the prepared silver powder is not obvious and the morphology is unstable. The flower-shaped silver powder prepared in the technical solution disclosed in CN 114192769 A has obvious structural characteristics, but the preparation process is too cumbersome, with many error sources, and the sphericity of the flower-shaped silver powder prepared is not high, and breakpoints are prone to occur in the subsequent printing process, resulting in reduced conductivity of the silver paste. 。 Summary of the invention

[0005] The present invention aims to overcome the defects of the prior art and provide a method for preparing flower-shaped spherical silver powder.

[0006] The technical solution of the present invention is as follows:

[0007] A method for preparing flower-shaped spherical silver powder comprises the following steps:

[0008] (1) first preparing a silver nitrate solution, then adding sodium poly(disulfide bis(propane sulfonate)) (SPS) to the silver nitrate solution, and stirring until fully dissolved to obtain a precursor solution;

[0009] (2) first preparing a reducing agent solution, then adding a dispersant, and stirring until the mixture is uniformly mixed to obtain a reducing agent-dispersant mixed solution;

[0010] (3) In a light-proof environment at 28-32° C., equal volumes of the precursor solution and the reducing agent-dispersant mixed solution are symmetrically added dropwise into the stirring deionized water at a rate of 1-2 mL / s, and after the addition is completed, the reaction is kept warm for 4-6 minutes, and then aged at room temperature to obtain a silver colloid solution;

[0011] (4) The silver colloid solution is centrifuged, washed and dried in sequence to obtain flower-shaped spherical silver powder.

[0012] In a preferred embodiment of the present invention, the molar ratio of the poly (sodium disulfide bispropane sulfonate) (SPS) to silver nitrate is 0.001-0.005:1, and the concentration of the silver nitrate solution is 0.2-0.3 mol / L.

[0013] In a preferred embodiment of the present invention, the reducing agent is ascorbic acid, and the concentration of the reducing agent solution is 0.1-0.2 mol / L.

[0014] In a preferred embodiment of the present invention, the dispersant is at least one of xanthan gum, polyvinyl pyrrolidone (PVP), sodium carboxymethyl cellulose (CMC-Na) and alkyl polyglycoside (APG).

[0015] Further preferably, the dispersant consists of polyvinyl pyrrolidone and alkyl glycoside.

[0016] More preferably, the dispersant is an alkyl glycoside.

[0017] Further preferably, the dispersant consists of sodium carboxymethyl cellulose and alkyl glycoside.

[0018] In a preferred embodiment of the present invention, the reducing agent is ascorbic acid; the dispersant consists of polyvinyl pyrrolidone and alkyl glycoside, or is alkyl glycoside, or consists of sodium carboxymethyl cellulose and alkyl glycoside.

[0019] A flower-shaped spherical silver powder is prepared by the above preparation method.

[0020] The beneficial effects of the present invention are:

[0021] 1. The flower-shaped spherical silver powder prepared by the present invention is formed by self-assembly of nano-thin silver sheets with a thickness of about 40nm, and the particle size ranges from 1 to 3μm. The surface-level nanostructure of the flower-shaped spherical silver powder can greatly increase the contact area between the silver powders and form a uniform conductive network.

[0022] 2. The present invention belongs to the liquid phase chemical reduction method. SPS is added to the precursor solution to control the system to form a continuous and stable sheet structure. The addition of a dispersant to the reducing agent solution can promote the self-assembly of nano-thin silver sheets into flower-like spherical silver powders, effectively preventing the agglomeration of the formed silver powders.

[0023] 3. The present invention does not introduce seed crystals, and self-assembles in one step. In addition, there is no need to adjust the pH and temperature of the reaction system during the reaction. It has the advantages of simplicity, high efficiency, low cost, and a large process window, which is conducive to subsequent commercial mass production. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 This is a 5000x SEM image of the flower-shaped spherical silver powder prepared in Example 1 of the present invention (the scale bar in the figure represents 1 μm).

[0025] Figure 2 This is a 10,000-fold SEM image of the flower-shaped spherical silver powder prepared in Example 1 of the present invention (the scale bar 1 in the figure represents 100 nm).

[0026] Figure 3 This is a 10,000-fold SEM image of the flower-shaped spherical silver powder prepared in Example 2 of the present invention (the scale bar 1 in the figure represents 100 nm).

[0027] Figure 4 This is a 5000x SEM image of the comparative silver powder prepared in Comparative Example 1 of the present invention (the scale 1 small grid in the figure is 1 μm).

[0028] Figure 5 This is a 5000x SEM image of the comparative silver powder prepared in Comparative Example 2 of the present invention (the scale 1 small grid in the image represents 1 μm). DETAILED DESCRIPTION

[0029] The technical solution of the present invention is further illustrated and described below through specific implementation modes in combination with the accompanying drawings.

[0030] Example 1

[0031] (1) Preparation of precursor solution: First prepare 25 mL of 0.25 mol / L silver nitrate solution, then add 0.006 g of SPS to the silver nitrate solution and stir magnetically for 5 to 8 min until fully dissolved to obtain a precursor solution.

[0032] (2) Preparation of reducing agent-dispersant mixed solution: First prepare 25 mL of 0.15 mol / L ascorbic acid solution, then weigh 0.003 g PVP and 0.005 g APG and add them to the ascorbic acid solution, and stir magnetically for 2 min to obtain a reducing agent-dispersant mixed solution.

[0033] (3) In a light-proof environment at 30° C., the precursor solution and the reducing agent-dispersant mixed solution are symmetrically added dropwise into the stirring deionized water (the deionized water is heated in a water bath at 30° C.) at a rate of 2 mL / s. After the addition is completed, the reaction is kept warm for 5 minutes, and then aged at room temperature for 10 minutes to obtain a silver colloid solution;

[0034] (4) The silver colloid solution is centrifuged, washed and dried in sequence to obtain flower-shaped spherical silver powder. The centrifugal parameters are 10000r / min for 3min; the washing method is 3 times of deionized water washing and 2 times of anhydrous ethanol washing; the drying condition is drying in a forced air drying oven at 60°C for 8h.

[0035] Example 2

[0036] (1) Preparation of precursor solution: First prepare 25 mL of 0.25 mol / L silver nitrate solution, then add 0.006 g SPS and 0.003 g PVP to the silver nitrate solution, and stir magnetically for 5 to 8 min until fully dissolved to obtain a precursor solution.

[0037] (2) Preparation of reducing agent-dispersant mixed solution: 25 mL of 0.15 mol / L ascorbic acid solution was prepared, and then 0.005 g of APG was weighed and added to the ascorbic acid solution. The mixture was stirred magnetically for 2 min to obtain a reducing agent-dispersant mixed solution.

[0038] (3) In a light-proof environment at 30° C., the precursor solution and the reducing agent-dispersant mixed solution are symmetrically added dropwise into the stirring deionized water (the deionized water is heated in a water bath at 30° C.) at a rate of 2 mL / s. After the addition is completed, the reaction is kept warm for 5 minutes, and then aged at room temperature for 10 minutes to obtain a silver colloid solution;

[0039] (4) The silver colloid solution is centrifuged, washed and dried in sequence to obtain flower-shaped spherical silver powder. The centrifugal parameters are 10000r / min for 3min; the washing method is 3 times of deionized water washing and 2 times of anhydrous ethanol washing; the drying condition is drying in a forced air drying oven at 60°C for 8h.

[0040] Example 3

[0041] (1) Preparation of precursor solution: First prepare 25 mL of 0.25 mol / L silver nitrate solution, then add 0.006 g of SPS to the silver nitrate solution and stir magnetically for 5 to 8 min until fully dissolved to obtain a precursor solution.

[0042] (2) Preparation of reducing agent-dispersant mixed solution: First prepare 25 mL of 0.15 mol / L ascorbic acid solution, then weigh 0.003 g CMC-Na and 0.005 g APG and add them to the ascorbic acid solution, and stir magnetically for 2 min to obtain a reducing agent-dispersant mixed solution.

[0043] (3) In a light-proof environment at 30° C., the precursor solution and the reducing agent-dispersant mixed solution are symmetrically added dropwise into the stirring deionized water (the deionized water is heated in a water bath at 30° C.) at a rate of 2 mL / s. After the addition is completed, the reaction is kept warm for 5 minutes, and then aged at room temperature for 10 minutes to obtain a silver colloid solution;

[0044] (4) The silver colloid solution is centrifuged, washed and dried in sequence to obtain flower-shaped spherical silver powder. The centrifugal parameters are 10000r / min for 3min; the washing method is 3 times of deionized water washing and 2 times of anhydrous ethanol washing; the drying condition is drying in a forced air drying oven at 60°C for 8h.

[0045] Comparative Example 1

[0046] (1) Preparation of precursor solution: Weigh silver nitrate and add deionized water to prepare 25 mL of 0.25 mol / L silver nitrate solution.

[0047] (2) Preparation of reducing agent-dispersant mixed solution: First prepare 25 mL of 0.15 mol / L ascorbic acid solution, then weigh 0.003 g PVP and 0.005 g APG and add them to the ascorbic acid solution, and stir magnetically for 2 min to obtain a reducing agent-dispersant mixed solution.

[0048] (3) In a light-proof environment at 30° C., the precursor solution and the reducing agent-dispersant mixed solution are symmetrically added dropwise into the stirring deionized water (the deionized water is heated in a water bath at 30° C.) at a rate of 2 mL / s. After the addition is completed, the reaction is kept warm for 5 minutes, and then aged at room temperature for 10 minutes to obtain a silver colloid solution;

[0049] (4) The silver colloid solution is centrifuged, washed and dried in sequence to obtain comparative silver powder. The centrifugal parameters are 10000r / min for 3min, the washing method is 3 times of deionized water washing and 2 times of anhydrous ethanol washing, and the drying condition is drying in a forced air drying oven at 60°C for 8h.

[0050] The difference between Comparative Example 1 and Example 1 is that SPS is not added to the precursor solution.

[0051] Comparative Example 2

[0052] (1) Preparation of precursor solution: First prepare 25 mL of 0.25 mol / L silver nitrate solution, then add 0.006 g of SPS to the silver nitrate solution and stir magnetically for 5 to 8 min until fully dissolved to obtain a precursor solution.

[0053] (2) Preparation of reducing agent solution: Weigh ascorbic acid and add deionized water to prepare 25 mL of 0.15 mol / L ascorbic acid solution.

[0054] (3) In a light-proof environment at 30° C., the precursor solution and the reducing agent solution are symmetrically added dropwise at a rate of 2 mL / s into the stirring deionized water (the deionized water is heated in a water bath at 30° C.), and after the addition is completed, the reaction is kept warm for 5 minutes, and then aged at room temperature for 10 minutes to obtain a silver colloid solution;

[0055] (4) The silver colloid solution is centrifuged, washed and dried in sequence to obtain comparative silver powder. The centrifugal parameters are 10000r / min for 3min, the washing method is 3 times of deionized water washing and 2 times of anhydrous ethanol washing, and the drying condition is drying in a forced air drying oven at 60°C for 8h.

[0056] The difference between Comparative Example 2 and Example 1 is that no dispersant is added to the reducing agent solution.

[0057] Depend on Figure 1 and Figure 2 It can be seen that the flower-shaped spherical silver powder prepared in Example 1 of the present invention is formed by self-assembly of nano-thin sheets of silver with a thickness of 40 nm, and the flower as a whole is spherical in shape, and its surface contact sites are more than those of a smooth sphere.

[0058] Depend on Figure 3 It can be seen that the flower-shaped spherical silver powder prepared in Example 2 of the present invention has a more obvious flower-shaped structure, but its sphericity is not as good as that of the silver powder prepared in Example 1.

[0059] Depend on Figure 4 and Figure 5 It can be seen that in Comparative Example 1, no SPS was added, and the comparative silver powder obtained was spherical as a whole, but there was almost no flower-like structure, and the silver powder particles were uneven in size; in Comparative Example 2, no dispersant was added, and the comparative silver powder obtained was shaped like a flat boat as a whole. The flat boat was still composed of thin silver flakes, but it failed to self-assemble into flower-shaped spherical silver powder and had poor dispersibility.

[0060] The above description is only a preferred embodiment of the present invention, and therefore cannot be used to limit the scope of the present invention. That is, equivalent changes and modifications made according to the patent scope of the present invention and the contents of the specification should still fall within the scope of the present invention.

Claims

1. A method for preparing flower-shaped spherical silver powder, characterized in that: The steps include: (1) first preparing a silver nitrate solution, then adding sodium polydisulfide propane sulfonate to the silver nitrate solution, and stirring until fully dissolved to obtain a precursor solution; (2) first preparing a reducing agent solution, then adding a dispersant, and stirring until the mixture is uniformly mixed to obtain a reducing agent-dispersant mixed solution; (3) In a light-proof environment at 28-32° C., equal volumes of the precursor solution and the reducing agent-dispersant mixed solution are symmetrically added dropwise into the stirring deionized water at a rate of 1-2 mL / s, and after the addition is completed, the reaction is kept warm for 4-6 minutes, and then aged at room temperature to obtain a silver colloid solution; (4) The silver colloid solution is centrifuged, washed and dried in sequence to obtain flower-shaped spherical silver powder.

2. The preparation method according to claim 1, characterized in that: The molar ratio of the sodium polydisulfide dipropane sulfonate to silver nitrate is 0.001-0.005:1, and the concentration of the silver nitrate solution is 0.2-0.3 mol / L.

3. The preparation method according to claim 1 or 2, characterized in that: The reducing agent is ascorbic acid, and the concentration of the reducing agent solution is 0.1-0.2 mol / L.

4. The preparation method according to claim 1 or 2, characterized in that: The dispersant is at least one of xanthan gum, polyvinyl pyrrolidone, sodium carboxymethyl cellulose and alkyl glycoside.

5. The preparation method according to claim 4, characterized in that: The dispersant consists of polyvinyl pyrrolidone and alkyl glycoside.

6. The preparation method according to claim 4, characterized in that: The dispersant is an alkyl glycoside.

7. The preparation method according to claim 4, characterized in that: The dispersant consists of sodium carboxymethyl cellulose and alkyl glycoside.

8. The preparation method according to claim 1 or 2, characterized in that: The reducing agent is ascorbic acid; the dispersant consists of polyvinyl pyrrolidone and alkyl glycoside, or is alkyl glycoside, or consists of sodium carboxymethyl cellulose and alkyl glycoside.

9. A flower-shaped spherical silver powder, characterized in that: Prepared by the preparation method described in any one of claims 1 to 8.

Citation Information

Patent Citations

  • Flower-like spherical silver powder preparing method

    CN103273082A

  • Method for synthesizing flower-shaped silver micro-particles

    CN103551589A

  • Hollow-structure cauliflower-like metal silver powder and preparation method

    CN116833418A

  • Silver powder and method for producing same

    WO2013133103A1

Cited By

  • Flower-shaped silver powder and preparation method and application thereof

    CN122077012A