Ti35 / austenitic stainless steel heterogeneous connecting piece for nuclear spent fuel aftertreatment equipment and preparation method of Ti35 / austenitic stainless steel heterogeneous connecting piece
Through the explosive composite welding technology of Ti35 titanium alloy and austenitic stainless steel heterogeneous connectors, combining the advantages of both, the problems of low interface bonding strength and high cost are solved, high strength and corrosion resistance are achieved, and production costs are reduced. .
Patent Information
- Application Number
- CN202411296353.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-18
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2044-09-18
AI Technical Summary
When the existing explosive composite welding technology is used to prepare titanium-stainless steel composite pipes, the interface bonding strength is low, the cost is high, and brittle phases or holes are easily introduced, making it difficult to meet the high strength and corrosion resistance requirements of spent nuclear fuel reprocessing equipment.
The heterogeneous connectors of Ti35 titanium alloy and austenitic stainless steel are used, which are machined after explosive composite welding. It combines the high strength of Ti35 titanium alloy and the corrosion resistance of austenitic stainless steel to reduce costs and improve the interface bonding strength, avoiding intermediate The use of layer metal.
It achieves more than 99% of the bonding area and a shear strength of more than 240MPa. It has the corrosion resistance and welding performance of high-concentration boiling nitric acid, reduces production costs, and avoids self-corrosion of interface metal and increased material costs.
Smart Images

Figure CN118809102A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of heterogeneous metal composite preparation of nuclear spent fuel reprocessing equipment component connection structures, and specifically relates to a Ti35 / austenitic stainless steel heterogeneous connector for nuclear spent fuel reprocessing equipment and a preparation method thereof. Background Art
[0002] Explosive welding is a new metal welding process and technology that uses explosives as energy, which is a combination of pressure welding, fusion welding and diffusion welding. During the explosion, the chemical energy of the explosive is mostly converted into the kinetic energy of the composite material through multiple and multiple energy transfers, absorption, conversion and distribution (very short, measured in microseconds), causing it to collide with the substrate at high speed, achieving metallurgical bonding between the substrate and the composite material, and the composite interface is in a corrugated shape. This technology can make full use of the various excellent properties of the substrate and the composite material, such as corrosion resistance, acid and alkali resistance, high and low temperature resistance, etc., and quickly achieve strong metallurgical bonding of any metal, especially dissimilar metal materials. It has been widely used in chemical industry, petroleum, shipbuilding, military, nuclear industry, aerospace and other fields.
[0003] As a new type of alternative energy, nuclear energy is increasingly widely used, and the research and development of post-nuclear fuel treatment equipment has received more and more attention. As component dissolvers, highly radioactive waste acid evaporators and nitric acid recoverers that have been in high-concentration nitric acid equipment for a long time, the service environment is particularly harsh, which has become a difficult point in research in recent years. The earliest used high-purity austenitic stainless steel is prone to intergranular passivation and intergranular corrosion in boiling nitric acid, which is far from meeting the technical requirements of the equipment. Therefore, the development of alternative new materials has become a major trend. Titanium-stainless steel composite material is a layered metal composite material with pure titanium or titanium alloy and stainless steel parts as base and composite materials respectively. This type of material combines the advantages of titanium and titanium alloys with stainless steel while overcoming the shortcomings of single material functions. In particular, it has excellent corrosion resistance and becomes the best substitute. It is currently widely used in petroleum, chemical, medical, light industry, environmental protection, aerospace and other fields. It is an indispensable structural material in modern chemical industry and pressure vessels.
[0004] However, the current process parameters for preparing titanium-stainless steel composite pipes using explosive welding technology mostly refer to the welding process of titanium-steel explosive composite plates. In order to avoid the formation of composite interfaces that lead to low interface bonding strength of TiC, FeTi, Fe 2 The addition of an intermediate layer of metal (such as niobium, molybdenum, nickel, silver, copper, vanadium, etc.) is generally used to prevent the atomic diffusion between titanium and steel. The intermediate layer of metal must not only be able to effectively isolate the diffusion of Ti, Fe and C atoms, but also cannot react with titanium and steel to form intermetallic compounds, or the generated intermetallic compounds have little damage to the interface. Although the addition of the intermediate layer of metal can avoid TiC, FeTi or Fe 2The generation of Ti will also introduce new problems, not only increasing the cost of raw materials and production, but also causing the titanium and steel interfaces to slide relative to each other, which is not conducive to shape control. In addition, the addition of the intermediate layer of metal will also introduce new brittle phases or holes at the interface, making the interface situation more complicated.
[0005] Therefore, there is an urgent need to develop or improve the existing explosive composite welding technology to produce titanium-stainless steel composite pipes with high strength and corrosion resistance to solve or alleviate the above problems. Summary of the invention
[0006] The technical problem to be solved by the present invention is to provide a Ti35 / austenitic stainless steel heterogeneous connector for nuclear spent fuel reprocessing equipment in view of the deficiencies of the above-mentioned prior art. The Ti35 / austenitic stainless steel heterogeneous connector has a bonding area of more than 99% and a minimum shear strength of not less than 240 MPa. It combines the high strength of Ti35 titanium alloy, corrosion resistance to high-concentration boiling nitric acid, and intergranular corrosion resistance, plasticity and welding performance of austenitic stainless steel, solving the problems of low shear strength of a single stainless steel pipe and self-corrosion caused by direct contact with corrosive media.
[0007] In order to solve the above technical problems, the technical solution adopted by the present invention is: a Ti35 / austenitic stainless steel heterogeneous connector for nuclear spent fuel reprocessing equipment, characterized in that the heterogeneous connector is obtained by explosive composite welding after an austenitic stainless steel bar is inserted into a Ti35 tube or a Ti35 bar is inserted into an austenitic stainless steel tube, and then machining.
[0008] The present invention provides a Ti35 / austenitic stainless steel heterogeneous connector, wherein the Ti35 titanium alloy is an α-type corrosion-resistant titanium alloy, which can work for a long time in a high-concentration oxidizing acid solution (containing cations) environment in a boiling state, but its cost is relatively high. Austenitic stainless steel is widely used in the nuclear power industry as an important structural material, which can work in a high-concentration acid solution, but it is not resistant to cationic corrosion, and its cost is lower than that of Ti35 titanium alloy. A joint pipe composited with the two materials has the different material characteristics of the base and the composite material, meets the process requirements of the process equipment system, and reduces the cost of the system. It can be used to manufacture the connection structure of equipment components such as petrochemical and nuclear chemical pressure vessels, towers, kettles, tanks, troughs, transition joints, etc. Under the premise of no special requirements, a structure with austenitic stainless steel on the outside and Ti35 titanium alloy on the inside is selected as much as possible, because the pipe diameter is larger outside, and stainless steel is cheaper, thereby reducing the cost.
[0009] The above-mentioned Ti35 / austenitic stainless steel heterogeneous connector for nuclear spent fuel reprocessing equipment is characterized in that the composition of the Ti35 tube and Ti35 bar in terms of mass percentage all satisfies: Ta 5.5%~6.5%, Fe≤0.15%, C≤0.08%, N≤0.03%, H≤0.01%, O≤0.15%, and the balance is titanium and unavoidable impurity elements; the grade of the austenitic stainless steel bar or austenitic stainless steel tube is S30403 or S32168. Compared with traditional pure titanium materials, the present invention further reduces the corrosion resistance cost by adding 5.5%~6.5% of metal tantalum Ta by mass percentage. Ta can form an infinite solid solution with Ti, greatly enhancing the corrosion resistance of titanium alloy in reducing and oxidizing media while improving the strength of titanium alloy. By adopting S30403 or S32168 austenitic stainless steel, it has the advantages of low carbon content, acid corrosion resistance, and intergranular corrosion resistance.
[0010] The above-mentioned Ti35 / austenitic stainless steel heterogeneous connector for nuclear spent fuel reprocessing equipment is characterized in that the wall thickness of the Ti35 tube and the austenitic stainless steel tube is greater than 2 mm, and the diameter of the Ti35 rod and the austenitic stainless steel rod is greater than 6 mm. The present invention ensures the effect of explosive composite welding by controlling the wall thickness of the Ti35 tube and the austenitic stainless steel tube, and prevents the defects such as cracking in the explosive composite welding due to too small wall thickness, and ensures the effect of explosive composite welding by controlling the diameter of the Ti35 rod and the austenitic stainless steel rod, and prevents the defects that the diameter is too small and the explosion shock wave is not easy to make them combine together, and the smaller the rod diameter, the more explosives are needed, and the higher the risk factor.
[0011] In addition, the present invention also provides a method for preparing a Ti35 / austenitic stainless steel heterogeneous connector for nuclear spent fuel reprocessing equipment, characterized in that the method comprises the following steps: Step 1, weighing titanium sponge, tantalum powder and titanium powder, and mixing them to obtain raw materials; Step 2: Smelting the raw materials obtained in step 1 in a vacuum consumable arc melting furnace to obtain a Ti35 ingot, and then performing rough forging, fine forging, extrusion and rolling on the Ti35 ingot in sequence to obtain a Ti35 tube or a Ti35 bar; Step 3: Select austenitic stainless steel bars or austenitic stainless steel pipes; Step 4: polishing the surface of the Ti35 tube obtained in step 2 and the austenitic stainless steel bar selected in step 3 or the Ti35 bar obtained in step 2 and the austenitic stainless steel tube selected in step 3; Step 5. Assemble the polished Ti35 tube and austenitic stainless steel bar or the polished austenitic stainless steel tube and Ti35 bar in step 4, and then put them into an explosion-proof container. Then, evenly apply butter on the outer surface of the Ti35 tube or the austenitic stainless steel tube. Then, arrange explosives in the gap between the Ti35 tube or the austenitic stainless steel tube and the explosion-proof container, perform explosive composite welding, and finally perform machining to obtain a Ti35 / austenitic stainless steel heterogeneous connector.
[0012] In the present invention, Ti35 tubes or Ti35 rods are first prepared, and austenitic stainless steel rods or austenitic stainless steel tubes are selected. Then, the Ti35 tubes and austenitic stainless steel rods are assembled, explosive composite welding is performed, and finally machining is performed to obtain a Ti35 tube / austenitic stainless steel rod heterogeneous connector with Ti35 outside and austenitic stainless steel inside, or the Ti35 rod and austenitic stainless steel tube are assembled, explosive composite welding is performed, and finally machining is performed to obtain an austenitic stainless steel tube / Ti35 rod heterogeneous connector with austenitic stainless steel outside and Ti35 inside.
[0013] The machining process in the present invention is to open a hole in the center of the product obtained after explosive composite welding, so that the Ti35 / austenitic stainless steel heterogeneous connector is formed by Ti35 pipe wrapping austenitic stainless steel pipe or austenitic stainless steel pipe wrapping Ti35 pipe, and the upper part of the outer layer material is eliminated, and the inner layer material in the relative direction is eliminated to obtain the Ti35 / austenitic stainless steel heterogeneous connector in the form of a pipe joint.
[0014] The above method is characterized in that the grade of the titanium sponge in step 1 is grade 0, the grade is MHT-100, and the specification is 0.83mm~12.7mm; the tantalum powder is FTa-01 metallurgical grade, and the specification is not greater than -325 mesh; the grade of the titanium powder is TP200-1, the specification is not greater than -200 mesh, and the Mg mass content is not greater than 0.1%. The present invention ensures the quality of the Ti35 / austenitic stainless steel heterogeneous connector by controlling the grade and specification of the raw materials.
[0015] The above method is characterized in that the smelting in step 2 is repeated for more than 3 times. The present invention ensures the uniformity of Ti35 ingots through multiple smelting.
[0016] The above method is characterized in that the polishing in step 4 is polishing to a surface roughness of not more than Ra1.6μm. The present invention controls the surface roughness so that the Ti35 tube and austenitic stainless steel bar or the Ti35 bar and austenitic stainless steel tube have good surface roughness, have a higher area bonding law, and improve the product qualification rate.
[0017] The above method is characterized in that there is a gap of 2mm to 6mm between the assembled Ti35 pipe and austenitic stainless steel bar or between the austenitic stainless steel pipe and the Ti35 bar in step 5, and a steel cover is installed on the top of the assembled Ti35 pipe and austenitic stainless steel bar or between the austenitic stainless steel pipe and the Ti35 bar. The present invention limits the gap between the pipe and the bar, so that the pipe and the bar are tightly matched, effectively avoiding deformation after explosive composite, and completely covers the Ti35 pipe or the austenitic stainless steel pipe by adding a steel cover to prevent explosives from entering the joint surface between the two, thereby ensuring the effect of explosive composite welding.
[0018] The above method is characterized in that a pad is provided at the bottom of the explosion-proof container in step 5. The pad is provided to play an isolation role, making it easy to take out the prepared Ti35 / austenitic stainless steel heterogeneous connector.
[0019] The above method is characterized in that, in the explosive composite welding described in step 5, the detonator is placed on the top of the explosion-resistant container, the explosive is TNT explosive, and the detonation velocity is 2300m / s~2500m / s. The present invention selects TNT explosive to replace the rock emulsion explosive commonly used in titanium-steel composite plates. TNT explosive has high detonation velocity and high energy, and can complete the strong metallurgical bonding of the base and composite materials in a very short time or almost instantaneously, thereby ensuring the quality of the Ti35 / austenitic stainless steel heterogeneous connector.
[0020] Compared with the prior art, the present invention has the following advantages: 1. The bonding area of the Ti35 / austenitic stainless steel heterogeneous connector of the present invention reaches more than 99%, and the minimum shear strength is not less than 240MPa. It has the high strength of Ti35 titanium alloy, the corrosion resistance to high-concentration boiling nitric acid, and the intergranular corrosion resistance, plasticity and welding performance of austenitic stainless steel, and solves the problems of low shear strength of a single stainless steel pipe and self-corrosion caused by direct contact with corrosive media. It greatly reduces the cost of using titanium alone to prepare pressure vessel connection structural parts in nuclear spent fuel reprocessing. With the continuous advancement of my country's equipment manufacturing technology, the application field of Ti35 / austenitic stainless steel composite materials will continue to expand, making the actual application of engineering develop towards economic development.
[0021] 2. Compared with traditional pure titanium materials, the present invention adds 5.5% to 6.5% by mass of tantalum Ta to further reduce the cost of corrosion resistance. Ta can form an infinite solid solution with Ti, greatly enhancing the corrosion resistance of titanium alloy in reducing and oxidizing media while improving the strength of titanium alloy. By using S30403 or S32168 austenitic stainless steel, it has the advantages of low carbon content, acid corrosion resistance, and intergranular corrosion resistance, and has high strength, corrosion resistance and good thermal stability.
[0022] 3. Compared with the conventional explosive composite welding method of adding an intermediate metal layer, the present invention prepares Ti35 / austenitic stainless steel heterogeneous connectors without adding any intermediate layer metal, which can effectively reduce the input of materials and costs, reduce the generation of unnecessary intermetallic compounds, ensure the strength of the composite interface, and avoid the occurrence of metal self-corrosion on the bonding surface. Compared with titanium alloy / stainless steel composite pipe joints prepared by traditional rolling and friction welding methods, the composite pipe prepared by the explosive composite welding method has the advantages of large bonding area, high bonding strength and high production efficiency.
[0023] 4. The present invention limits the gap between the assembled Ti35 tube and the austenitic stainless steel bar or the austenitic stainless steel tube and the Ti35 bar, so that the bar and the tube are tightly matched, effectively avoiding deformation after explosive compounding.
[0024] 5. The present invention uses TNT explosives in explosive composite welding to replace the rock emulsion explosives commonly used in titanium-steel composite plates. TNT explosives have high detonation velocity and high energy, and can complete the strong metallurgical bonding of the base and composite materials in a very short time or almost instantaneously. In addition, no intermediate phase or intermetallic compound is basically produced at the interface between the base and the composite materials, which not only avoids the increase of materials and costs, but also the obtained material has high interface bonding strength and excellent corrosion resistance in extreme corrosive environments, avoiding the occurrence of metal internal corrosion, and has excellent comprehensive performance.
[0025] 6. The present invention prevents the surface from being overburned by applying butter, thereby improving the surface performance of the Ti35 / austenitic stainless steel heterogeneous connector.
[0026] The technical solution of the present invention is further described in detail below through the accompanying drawings and embodiments. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 It is a schematic diagram of the structure after the austenitic stainless steel pipe and Ti35 rod are assembled in Example 1 of the present invention.
[0028] Figure 2 Schematic diagram of the structure of the Ti35 / austenitic stainless steel heterogeneous connector prepared in Example 1 of the present invention.
[0029] Figure 3 This is a SEM image of the connection between the Ti35 / austenitic stainless steel heterogeneous connector Ti35 and the austenitic stainless steel prepared in Example 1 of the present invention.
[0030] Figure 4 It is a schematic diagram of the structure after the Ti35 tube and the austenitic stainless steel bar are assembled in Example 2 of the present invention.
[0031] Figure 5Schematic diagram of the structure of the Ti35 / austenitic stainless steel heterogeneous connector prepared in Example 2 of the present invention. DETAILED DESCRIPTION
[0032] Example 1 This embodiment includes the following steps: Step 1, weighing titanium sponge, tantalum powder and titanium powder, and mixing them to obtain raw materials; the grade of the titanium sponge is grade 0, the brand is MHT-100, and the specification is 0.83mm~12.7mm; the tantalum powder is FTa-01 metallurgical grade, and the specification is not greater than -325 mesh; the brand of the titanium powder is TP200-1, the specification is not greater than -200 mesh, and the Mg mass content is not greater than 0.1%; Step 2: Use a vacuum consumable arc melting furnace to melt the raw materials obtained in step 1 three times to obtain a Ti35 ingot, and then perform rough forging, fine forging and rolling on the Ti35 ingot in sequence to obtain a Ti35 rod with a diameter of 30 mm; the composition of the Ti35 rod satisfies the following by mass percentage: Ta 5.5%, Fe 0.15%, C 0.08%, N 0.03%, H 0.01%, O 0.12%, and the balance is titanium and unavoidable impurity elements; Step 3: Select austenitic stainless steel pipe with a wall thickness of 6 mm and a grade of S30403 (022Cr19Ni10); Step 4: polish the surface of the Ti35 rod obtained in step 2 and the austenitic stainless steel pipe selected in step 3 until the surface roughness is not greater than Ra1.6μm; Step 5. Assemble the polished austenitic stainless steel pipe and Ti35 rod in step 4, with a gap of 6 mm between the assembled austenitic stainless steel pipe and Ti35 rod, and then put them into an explosion-proof container with a pad at the bottom, and then evenly spread butter on the outer surface of the austenitic stainless steel pipe, and then arrange TNT explosives in the gap between the austenitic stainless steel pipe and the explosion-proof container, and add a steel cover on the top, and then perform explosive composite welding at a detonation speed of 2300m / s, and finally perform leveling, trimming and machining to obtain a Ti35 / austenitic stainless steel heterogeneous connector with austenitic stainless steel wrapped with Ti35.
[0033] Figure 1 is a schematic diagram of the structure of the austenitic stainless steel pipe and Ti35 rod assembled in this embodiment. Figure 1 It can be seen that the Ti35 rod is inserted into the austenitic stainless steel pipe with a gap between the two.
[0034] Figure 2 is a schematic diagram of the structure of the Ti35 / austenitic stainless steel heterogeneous connector prepared in this embodiment. Figure 2It can be seen that in the Ti35 / austenitic stainless steel heterogeneous connector prepared in this embodiment, the specifications of the Ti35 titanium alloy tube are 26.7 mm×2.87 mm (diameter×height), the dimensions of the austenitic stainless steel tube are 32.5 mm×2.87 mm (diameter×height), and the Ti35 titanium alloy protrudes out of the austenitic stainless steel.
[0035] Figure 3 is a SEM image of the connection between the Ti35 / austenitic stainless steel heterogeneous connector Ti35 and the austenitic stainless steel prepared in this embodiment. Figure 3 It can be seen that there are usually periodic ripples on the bonding surface after explosive recombination. The wavy bonding ensures the bonding strength of the interface. There are also vortices in the wavy bonding. During the explosive recombination process, the material in the vortex is in a molten state, and an intermediate compound formed by Fe and Ti elements is formed here.
[0036] Example 2 This embodiment includes the following steps: Step 1, weighing titanium sponge, tantalum powder and titanium powder, and mixing them to obtain raw materials; the grade of the titanium sponge is grade 0, the brand is MHT-100, and the specification is 0.83mm~12.7mm; the tantalum powder is FTa-01 metallurgical grade, and the specification is not greater than -325 mesh; the brand of the titanium powder is TP200-1, the specification is not greater than -200 mesh, and the Mg mass content is not greater than 0.1%; Step 2: Use a vacuum consumable arc melting furnace to melt the raw materials obtained in step 1 three times to obtain a Ti35 ingot, and then perform rough forging, fine forging, extrusion and rolling on the Ti35 ingot in sequence to obtain a Ti35 tube with a wall thickness of 8 mm; the composition of the Ti35 tube meets the following mass percentages: Ta 6%, Fe 0.09%, C 0.05%, N 0.03%, H0.005%, O 0.10%, and the balance is titanium and unavoidable impurity elements; Step 3: Select austenitic stainless steel bars with a diameter of 76 mm and a grade of S32168 (06Cr18Ni11Ti); Step 4: polish the Ti35 tube obtained in step 2 and the austenitic stainless steel bar selected in step 3 until the surface roughness is not greater than Ra1.6 μm; Step 5. Assemble the polished Ti35 pipe and austenitic stainless steel bar in step 4, with a gap of 3 mm between the assembled Ti35 pipe and austenitic stainless steel bar. Then put them into an explosion-proof container with a pad at the bottom, and then evenly spread butter on the outer surface of the Ti35 pipe. Then, arrange TNT explosives in the gap between the Ti35 pipe and the explosion-proof container, add a steel cover on the top, and then perform explosive composite welding at a detonation speed of 2400m / s. Finally, perform leveling, trimming and machining to obtain a Ti35 / austenitic stainless steel heterogeneous connector with Ti35 wrapped with austenitic stainless steel.
[0037] Figure 4 is a schematic diagram of the structure of the Ti35 tube and the austenitic stainless steel bar after assembly in this embodiment. Figure 4 As can be seen in the figure, the austenitic stainless steel bar is inserted into the Ti35 tube.
[0038] Figure 5 is a schematic diagram of the structure of the Ti35 / austenitic stainless steel heterogeneous connector prepared in this embodiment. Figure 5 It can be seen that in the Ti35 / austenitic stainless steel heterogeneous connector prepared in this embodiment, the specifications of the Ti35 titanium alloy tube are 73mm×5.16mm (diameter×height), the dimensions of the austenitic stainless steel tube are 83.4mm×5.16mm (diameter×height), and the austenitic stainless steel protrudes out of the Ti35 titanium alloy.
[0039] Example 3 This embodiment includes the following steps: Step 1, weighing titanium sponge, tantalum powder and titanium powder, and mixing them to obtain raw materials; the grade of the titanium sponge is grade 0, the brand is MHT-100, and the specification is 0.83mm~12.7mm; the tantalum powder is FTa-01 metallurgical grade, and the specification is not greater than -325 mesh; the brand of the titanium powder is TP200-1, the specification is not greater than -200 mesh, and the Mg mass content is not greater than 0.1%; Step 2: Use a vacuum consumable arc melting furnace to melt the raw materials obtained in step 1 three times to obtain a Ti35 ingot, and then perform rough forging, fine forging and rolling on the Ti35 ingot in sequence to obtain a Ti35 rod with a diameter of 170 mm; the composition of the Ti35 rod satisfies the following by mass percentage: Ta 6.5%, Fe 0.15%, C 0.08%, N 0.03%, H 0.004%, O0.08%, and the balance is titanium and unavoidable impurity elements; Step 3: Select austenitic stainless steel pipe with a wall thickness of 10 mm and a grade of S30403 (022Cr19Ni10); Step 4: polish the surface of the Ti35 rod obtained in step 2 and the austenitic stainless steel pipe selected in step 3 until the surface roughness is not greater than Ra1.6μm; Step 5. Assemble the polished austenitic stainless steel pipe and Ti35 rod in step 4, with a gap of 2 mm between the assembled austenitic stainless steel pipe and Ti35 rod, and then put them into an explosion-proof container with a pad at the bottom, and then evenly spread butter on the outer surface of the austenitic stainless steel pipe, and then arrange TNT explosives in the gap between the austenitic stainless steel pipe and the explosion-proof container, and add a steel cover on the top, and then perform explosive composite welding at a detonation speed of 2500m / s, and finally perform leveling, trimming and machining to obtain a Ti35 / austenitic stainless steel heterogeneous connector with austenitic stainless steel wrapped with Ti35.
[0040] After testing, the specifications of the Ti35 titanium alloy tube in the Ti35 / austenitic stainless steel heterogeneous connector prepared in this embodiment are 168.3 mm×7.11 (diameter×height), the size of the austenitic stainless steel tube is 182.5 mm×7.11 (diameter×height), and the Ti35 titanium alloy protrudes out of the austenitic stainless steel.
[0041] The Ti35 / austenitic stainless steel heterogeneous connectors prepared in Examples 1 to 3 were tested for hardness using a HVS-50 Vickers hardness tester with a load of 1 kg. The average value was taken after hitting 5 points. The test results are shown in Table 1.
[0042] The Ti35 / austenitic stainless steel heterogeneous connectors prepared in Examples 1 to 3 were subjected to a tensile test using an electronic universal testing machine. The sample nominal section size was a rectangular specimen of 1 to 2×5×30 mm. The average values of the tensile strength, yield strength and elongation of three identically treated samples were taken. The test results are shown in Table 1.
[0043] The Ti35 / austenitic stainless steel heterogeneous connectors prepared in Examples 1 to 3 were subjected to corrosion current measurement using a P4000 electrochemical workstation. The test conditions were: 2 The Ti35 / austenitic stainless steel heterojunction prepared in Examples 1 to 3 was used as the working electrode, the saturated calomel electrode was used as the reference electrode, and the platinum sheet was used as the auxiliary electrode; the nitric acid electrolyte containing 0.8 mol / L was heated to boiling in a water bath, and hydrogen was introduced into the electrolyte at a flow rate of 20 mL / min; the sample was subjected to a linear potential scan at a scan rate of 2 mV / s. The average value was taken after measuring 3 samples, and the test results are shown in Table 1.
[0044] The interfacial shear strength of the Ti35 / austenitic stainless steel heterogeneous connectors prepared in Examples 1 to 3 was tested, and the average value was taken after measuring 3 samples. The test results are shown in Table 1.
[0045] Table 1
[0046] As shown in Table 1, the Ti35 / austenitic stainless steel heterogeneous connector prepared by the present invention has high hardness and strength and excellent corrosion resistance. The hardness reaches 301HV, the tensile strength reaches 417MPa, the yield strength reaches 310MPa, the elongation reaches 41%, and the corrosion current reaches 0.69μA / cm 2 , the maximum shear strength is 412.8MPa.
[0047] The Ti35 / austenitic stainless steel heterogeneous connectors prepared in Examples 1 to 3 were subjected to ultrasonic flaw detection. The flaw detection results showed that the bonding rates of the Ti35 / austenitic stainless steel heterogeneous connectors prepared in Examples 1 to 3 were all greater than 99.8%. According to GJB3797-2015, the tensile shear strength of the interface was tested, and the tensile shear strength of the interface was greater than 350.0 MPa.
[0048] The above is only a preferred embodiment of the present invention and does not limit the present invention in any way. Any simple modification, change and equivalent change made to the above embodiment according to the technical essence of the present invention still falls within the protection scope of the technical solution of the present invention.
Claims
1. A Ti35 / austenitic stainless steel heterogeneous connector for nuclear spent fuel reprocessing equipment, characterized in that: The heterogeneous connector is obtained by inserting an austenitic stainless steel bar into a Ti35 tube or inserting a Ti35 bar into an austenitic stainless steel tube, performing explosive composite welding, and then machining.
2. The Ti35 / austenitic stainless steel heterogeneous connector for nuclear spent fuel reprocessing equipment according to claim 1, characterized in that: The compositions of the Ti35 tube and the Ti35 rod meet the following requirements in percentage by mass: Ta 5.5% to 6.5%, Fe≤0.15%, C≤0.08%, N≤0.03%, H≤0.01%, O≤0.15%, and the remainder is titanium and unavoidable impurity elements; the grade of the austenitic stainless steel rod or the austenitic stainless steel tube is S30403 or S32168.
3. The Ti35 / austenitic stainless steel heterogeneous connector for nuclear spent fuel reprocessing equipment according to claim 1, characterized in that: The wall thickness of the Ti35 tube and the austenitic stainless steel tube is greater than 2 mm, and the diameter of the Ti35 rod and the austenitic stainless steel rod is greater than 6 mm.
4. A method for preparing a Ti35 / austenitic stainless steel heterogeneous connector for nuclear spent fuel reprocessing equipment as claimed in any one of claims 1 to 3, characterized in that: The method comprises the following steps: Step 1, weighing titanium sponge, tantalum powder and titanium powder, and mixing them to obtain raw materials; Step 2: Smelting the raw materials obtained in step 1 in a vacuum consumable arc melting furnace to obtain a Ti35 ingot, and then performing rough forging, fine forging, extrusion and rolling on the Ti35 ingot in sequence to obtain a Ti35 tube or a Ti35 bar; Step 3: Select austenitic stainless steel bars or austenitic stainless steel pipes; Step 4: polishing the surface of the Ti35 tube obtained in step 2 and the austenitic stainless steel bar selected in step 3 or the Ti35 bar obtained in step 2 and the austenitic stainless steel tube selected in step 3; Step 5. Assemble the polished Ti35 tube and austenitic stainless steel bar or the polished austenitic stainless steel tube and Ti35 bar in step 4, and then put them into an explosion-proof container. Then, evenly apply butter on the outer surface of the Ti35 tube or the austenitic stainless steel tube. Then, arrange explosives in the gap between the Ti35 tube or the austenitic stainless steel tube and the explosion-proof container, perform explosive composite welding, and finally perform machining to obtain a Ti35 / austenitic stainless steel heterogeneous connector.
5. The method according to claim 4, characterized in that The grade of the titanium sponge described in step 1 is grade 0, the brand is MHT-100, and the specification is 0.83mm~12.7mm; the tantalum powder is FTa-01 metallurgical grade, and the specification is not greater than -325 mesh; the brand of the titanium powder is TP200-1, the specification is not greater than -200 mesh, and the Mg mass content is not greater than 0.1%.
6. The method according to claim 4, characterized in that The smelting in step 2 is repeated more than 3 times.
7. The method according to claim 4, characterized in that The polishing in step 4 is polishing until the surface roughness is not greater than Ra1.6μm.
8. The method according to claim 4, characterized in that In step 5, there is a gap of 2 mm to 6 mm between the assembled Ti35 tube and austenitic stainless steel bar or the austenitic stainless steel tube and Ti35 bar, and a steel cover is installed on the top of the assembled Ti35 tube and austenitic stainless steel bar or the austenitic stainless steel tube and Ti35 bar.
9. The method according to claim 4, characterized in that In step 5, a pad is provided at the bottom of the explosion-proof container.
10. The method according to claim 4, characterized in that In the explosive composite welding described in step 5, the detonator is placed on the top of the explosion-resistant container, the explosive is TNT explosive, and the detonation speed is 2300m / s~2500m / s.
Citation Information
Patent Citations
Titanium and titanium alloy / steel composite board and method of manufacturing the same
CN101402268A
Production method for ultralong thin titanium / steel compound plate
CN102441769A
Zirconium / steel composite board preparation method
CN104741880A
Rolling method for explosive cladding titanium-steel-titanium double-faced composite board
CN105057353A
Copper-tantalum corrosion-resistant reinforced austenitic stainless steel and preparation method thereof