A grooved polyamide-imide nanofiber aerogel and a preparation method thereof

By using a spinning liquid containing acetone and specific organic solvents in electrospinning to form a grooved polyamide imide micro-nanofiber aerogel and performing heat crosslinking treatment, the structural stability of electrospinning materials and the structure and stability of electrospinning materials are solved. The problem of low production efficiency has achieved high performance and efficient nanofiber aerogel preparation, which is suitable for multi-field applications.

CN118854492BActive Publication Date: 2024-12-06TIANJIN POLYTECHNIC UNIV +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411339241.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-09-25
Publication Date
2024-12-06
Estimated Expiration
2044-09-25

AI Technical Summary

Technical Problem

During the preparation process, existing electrospinned nanofiber materials have problems such as poor structural stability, unpredictable and control of pore structure, high energy consumption and low production efficiency, which limits their expansion in applications in many fields.

Method used

Electrospinning is performed using a spinning liquid containing acetone and a specific organic solvent to form a grooved polyamide imide micro-nanofiber aerogel, and its mechanical properties are enhanced by heat crosslinking treatment.

Benefits of technology

It has achieved a grooved micro-nanofiber aerogel with excellent high-temperature and low-temperature thermal insulation performance, light flame retardant and excellent hydrophobic performance. It has a short process cycle, high efficiency and low cost, and is suitable for large-scale production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118854492B_ABST
    Figure CN118854492B_ABST
Patent Text Reader

Abstract

The present invention provides a grooved polyamide-imide nanofiber aerogel and a preparation method thereof. The preparation method comprises S1: dissolving polyamide-imide (PAI) and bismaleimide (BMI) in an organic solvent to obtain a spinning solution; the organic solvent comprises acetone, and at least one of N,N-dimethylformamide, dimethyl sulfoxide, and N,N-dimethylacetamide; S2: electrospinning the spinning solution to obtain the grooved polyamide-imide micro-nano fiber aerogel. The preparation method of the present invention introduces a spinning solution containing acetone and a specific organic solvent, and a grooved polyamide-imide micro-nano fiber aerogel can be obtained through an electrospinning process. The aerogel is resistant to high and low temperatures, flame-retardant and lightweight, has good thermal insulation performance, and has excellent mechanical properties, which is of great significance for expanding the application of electrospun micro-nano fibers. The preparation method has a short process production cycle, high efficiency, and low cost, and is suitable for large-scale preparation.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of nanofiber materials, and in particular to a grooved polyamide-imide micro-nano fiber aerogel and a preparation method thereof. Background Art

[0002] As a cutting-edge micro-nano fiber material, electrospun nanofibers have the advantages of diverse raw materials and scalability. However, the conventional electrospinning process often produces a film-like material with densely arranged nanofibers. This structure limits its application in more fields. In order to overcome this limitation, researchers tried to reconstruct electrospun nanofibers into porous aerogel materials in three dimensions through freeze-drying. This aerogel material has good thermal insulation properties at low temperatures and can play a heat-insulating role at high temperatures, providing application possibilities for different scenarios.

[0003] However, although this method has achieved remarkable results, there are also some problems that cannot be ignored. For example, the process causes weak interactions between discontinuous nanofibers, resulting in poor overall structural stability, which makes the material susceptible to deformation or destruction by external forces in practical applications; due to the random growth of ice crystals during the freezing process, the final pore structure is difficult to predict and control, making the material structure unstable and unpredictable, further resulting in poor mechanical properties (stretching, bending, compression) of the nanofiber aerogel; and the three-dimensional reconstruction method consumes high energy, the freeze-drying process cycle is long, and the production efficiency is low, which not only increases the production cost, but also limits the application of this process in large-scale production. Summary of the invention

[0004] In view of the deficiencies in the prior art, the present invention discloses a grooved polyamide-imide micro-nano fiber aerogel and a preparation method thereof. The preparation method is simple to operate and easy to industrialize. The grooved polyamide-imide micro-nano fiber aerogel is prepared by the method. The aerogel has excellent thermal insulation and mechanical properties.

[0005] In order to achieve the above technical objectives, on the one hand, the present invention provides a method for preparing a grooved polyamide-imide micro-nano fiber aerogel, comprising the following steps:

[0006] S1: dissolving polyamideimide (PAI) and bismaleimide (BMI) in an organic solvent to obtain a spinning solution; the organic solvent comprises acetone and at least one of N,N-dimethylformamide, dimethyl sulfoxide, and N,N-dimethylacetamide;

[0007] S2: The spinning solution is subjected to electrospinning to obtain the grooved polyamide-imide micro-nano fiber aerogel.

[0008] The above technical solution realizes the direct preparation of PAI micro-nano fiber aerogel by electrospinning; in addition, the research and development team of the present invention unexpectedly discovered based on a large number of exploratory experiments that groove-shaped micro-nano fibers can be formed by electrospinning using binary or multi-solvent spinning solutions. Based on this discovery, a spinning solution containing acetone and at least one specific organic solvent is provided in the above technical solution, so that at the beginning of electrospinning, the original jet will cause phase separation due to the rapid volatilization of acetone and form micropores on the jet surface, and the micropores will be stretched into grooves, and finally solidified after the electrospinning operation is completed to obtain groove-shaped PAI micro-nano fiber aerogels.

[0009] It is worth noting that the R&D team set the types of organic solvents contained in the spinning solution after a large number of experiments and data analysis. Among them, the specific organic solvents can optionally include at least one of N,N-dimethylformamide, dimethyl sulfoxide, and N,N-dimethylacetamide. The volatility of the acetone used is not only quite different from that of the specific organic solvents, but it can also be mixed with the specific organic solvent to ensure the solubility of PAI and BMI in the spinning solution, thereby further promoting the formation of grooves on the PAI micro-nanofibers.

[0010] In a further example of the present invention, the relative humidity field of the electrospinning operation is explored and optimized. Optionally, the ambient humidity of the electrospinning operation is 45%-90%, further optionally 75%-90%, and further optionally 90%, thereby making the prepared PAI micro-nano fibers more fluffy.

[0011] In a further example of the present invention, the amount of acetone in the spinning solution is explored and optimized. Optionally, the content of acetone in the spinning solution is less than 30wt%, and the organic solvent can completely dissolve PAI and BMI; further, 5-25wt%, and further, 10-20wt%.

[0012] In a further example of the present invention, the amount of polyamide-imide added to the spinning solution is explored and optimized. Optionally, the mass fraction of polyamide-imide in the spinning solution is 22wt%~28wt%.

[0013] In a further example of the present invention, the control submission of electrospinning is optimized. Optionally, the receiving distance of the electrospinning operation is 16-20 cm, the voltage is 9-12 kV, and the receiving roller speed is 30-60 rpm.

[0014] In a further example of the present invention, after the electrospinning is completed, the process further includes S3: subjecting the grooved polyamide-imide micro-nano fiber aerogel to a thermal crosslinking treatment, wherein the thermal crosslinking treatment is performed at a temperature of 180-220°C and the treatment time is 1-2 hours. Thus, the thermal crosslinking process is used to enhance the structural stability between the micro-nano fibers, thereby giving the grooved micro-nano fiber aerogel better mechanical properties.

[0015] On the other hand, the present invention provides a grooved polyamide-imide micro-nano fiber aerogel prepared by the above preparation method. Subsequent testing and verification found that the grooved polyamide-imide micro-nano fiber aerogel prepared by the present invention has excellent thermal insulation performance, mechanical properties, hydrophobic properties and flame retardant properties.

[0016] Compared with the prior art, the preparation method of the present invention introduces a spinning solution containing acetone and a specific organic solvent, and can obtain a grooved polyamide-imide micro-nano fiber aerogel through an electrospinning process. The aerogel is resistant to high and low temperatures, flame retardant, lightweight, has good thermal insulation performance, and has excellent mechanical properties, which is of great significance for expanding the application of electrospun micro-nano fibers. The preparation method has a short process production cycle, high efficiency, and low cost, and is suitable for large-scale preparation. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] The drawings constituting a part of the present application are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute an improper limitation of the present invention. In the drawings:

[0018] Figure 1 It is a schematic diagram of a method for preparing a grooved polyamide-imide micro-nano fiber aerogel according to the present invention;

[0019] Figure 2 The SEM comparison images of micro-nano fibers prepared by electrospinning under different humidity gradients in Example 2 are shown;

[0020] Figure 3 The comparison diagram of the fluffiness of the micro-nano fibers prepared by electrospinning under different humidity gradients in Example 2 is shown, wherein (a) the ambient humidity is 45%, (b) the ambient humidity is 60%, (c) the ambient humidity is 75%, and (d) the ambient humidity is 90%;

[0021] Figure 4 The SEM comparison diagram of PAI micro-nano-dimensional obtained by spinning solutions with different acetone contents in Example 4 is shown;

[0022] Figure 5 A comparison of the hydrophobic properties of PAI micro-nano fibers prepared from spinning solutions with different acetone contents in Example 4 is shown;

[0023] Figure 6An optical photograph of the grooved PAI micro-nanofiber aerogel obtained by heat treatment at 200° C. in Example 5 is shown;

[0024] Figure 7 A comparison diagram of the fluffiness of the grooved PAI micro-nano fiber aerogel at different thermal crosslinking temperatures in Example 5 is shown;

[0025] Figure 8 The tensile mechanical properties of the grooved PAI micro-nano fiber aerogel at different thermal crosslinking temperatures in Example 5 are shown;

[0026] Fig. 9 The thermal insulation performance diagram of the grooved PAI micro-nano fiber aerogel at room temperature at different thermal crosslinking temperatures in Example 5 is shown;

[0027] Fig.10 The flame retardant performance of the PMNFA-200°C grooved PAI micro-nanofiber aerogel in Example 5 is shown. DETAILED DESCRIPTION

[0028] In order to facilitate the understanding of the present invention, the present invention will be described more comprehensively below, and preferred embodiments of the present invention are given. However, it should be understood that these embodiments are only used for more detailed description and should not be understood as limiting the present invention in any form, i.e., not intended to limit the scope of protection of the present invention.

[0029] Unless otherwise defined, the technical terms used in the following examples have the same meanings as those generally understood by those skilled in the art to which the present invention belongs. The test reagents used in the following examples, unless otherwise specified, are all conventional biochemical reagents; the experimental methods, unless otherwise specified, are all conventional methods.

[0030] Example 1

[0031] A method for preparing a grooved polyamide-imide micro-nano fiber aerogel, such as Figure 1 As shown, the following steps are included:

[0032] S1: dissolving polyamide-imide and bismaleimide in an organic solvent to obtain a spinning solution; the organic solvent comprises acetone and at least one of N,N-dimethylformamide, dimethyl sulfoxide and N,N-dimethylacetamide;

[0033] S2: The spinning solution is electrospinned to obtain the grooved PAI micro-nano fiber aerogel.

[0034] It should be noted that in the specific process, in step S1, PAI and BMI are magnetically stirred with an organic solvent in a water bath to promote dissolution, and then allowed to stand to obtain the spinning solution. Further, the heating temperature of the water bath is 50-70°C, the magnetic stirring time is 2-4 hours, and the standing time is 6-12 hours.

[0035] It should be noted that the organic solvent may optionally include acetone, and at least one of dimethyl sulfoxide or N,N-dimethylacetamide; and may further optionally include acetone and N,N-dimethylacetamide.

[0036] It should be noted that the mass ratio of PAI to BMI in the technical solution of the present invention can be selected as (4-6):1, and can be further selected as 5:1.

[0037] Optionally, the ambient humidity of the electrospinning operation is 45%-90%, further optionally 75%-90%, and further optionally 90%.

[0038] Optionally, the content of acetone in the spinning solution may be less than 30wt%, further may be 5wt%-25wt%, further may be 10wt%-20wt%.

[0039] Optionally, the mass fraction of polyamide-imide in the spinning solution may be 22wt%-28wt%; further may be 23wt%-25wt%; further may be 25wt%.

[0040] Optionally, the receiving distance of the electrospinning operation is 16-20 cm, the voltage is 9-12 kV, and the receiving roller speed is 30-60 rpm; further optionally, the receiving distance of the electrospinning operation is 20 cm, the voltage is 11 kV, and the receiving roller speed is 30 rpm.

[0041] It should be noted that this embodiment does not limit the operating temperature of electrospinning, and electrospinning can be performed at a temperature of 25±5°C.

[0042] Optionally, after the electrospinning is completed, the process further includes S3: subjecting the grooved PAI micro-nano fiber aerogel to thermal crosslinking treatment; the temperature of the thermal crosslinking treatment may be 180-220° C., and may further be 200° C.; and the treatment time may be 1-2 hours.

[0043] Example 2

[0044] Based on the preparation method of the grooved PAI micro-nano fiber aerogel shown in Example 1, this example explores and optimizes the relative humidity field control of the electrospinning operation. It should be noted that the specific process flow shown in this example is only a preferred display and does not limit the scope of protection of the present invention.

[0045] In this embodiment, the charge jet density can be adjusted by controlling the relative humidity in the electrospinning environment, thereby directly preparing the grooved PAI micro-nano fiber aerogel. Specifically, by increasing the relative humidity of electrospinning, the solidification of the charged jet is accelerated, so that the diameter of the PAI micro-nano fiber obtained by the collecting device increases with the increase of relative humidity.

[0046] In this example, N,N-dimethylacetamide was used as solvent to prepare a spinning solution containing 25 wt% PAI and 5 wt% BMI. The PAI / BMI spinning solution was then transferred to a 10 ml syringe, the needle was assembled, and the electrospinning process parameters were adjusted. The injection speed was 2 ml·h -1 A constant DC voltage of 12 kV was applied to the metal needle and the receiving roller, the receiving distance was maintained at 18 cm, the collecting speed of the receiving roller was 50 rpm, and the relative humidity was adjusted to 45% (RH=45%), 60% (RH=60%), 75% (RH=75%), and 90% (RH=90%), and electrospun PAI micro-nanofiber materials were obtained by electrospinning process.

[0047] The SEM images and bulkiness comparison of PAI micro-nanofibers prepared by electrospinning under different humidity gradients are shown in Figure 2. Figure 2 , Figure 3 As shown. The average diameters of the PAI micro-nano fibers obtained by the collecting device were 733.45nm, 1171.39nm, 1289.97nm and 1610.30nm, respectively. The high humidity environment during electrospinning accelerated the jet solidification and promoted the transformation of the micro-nano fiber material from a 2D film to a 3D fluffy structure aerogel. Therefore, in the technical solution of the present invention, the ambient humidity of the electrospinning operation is 45%-90%, further optionally 75%-90%, and further optionally 90%.

[0048] Example 3

[0049] Based on the preparation method of the grooved PAI micro-nano fiber aerogel described in Example 1, this example explores and optimizes the PAI content in the prepared spinning solution and the electrospinning process. It should be noted that the specific process flow shown in this example is only a better demonstration and does not limit the scope of protection of the present invention.

[0050] Specifically, this embodiment sets N, N-dimethylacetamide spinning solutions with PAI concentrations of 23wt%, 25wt% and 28wt%, respectively, and the mass ratio of PAI to BMI in the spinning solution is 5:1, and the spinning solution is stirred in a water bath at 50-70°C for 2-6h to obtain. Subsequently, this embodiment performs electrospinning at an ambient humidity of 90%, and the control conditions of the electrospinning process are: the receiving distance is 16-20cm, the voltage is 9-12kV, and the receiving roller speed is 30-60rpm, and electrospinning is performed.

[0051] Through exploration, this embodiment found that if the PAI concentration is too high, the needle may be clogged during electrospinning, which is not conducive to the smooth progress of spinning. Combined with the discovery in Example 2 that the larger the diameter of the PAI micro-nano fibers obtained by electrospinning, the fluffier the macroscopic structure of the aerogel, the mass fraction of polyamide-imide in the spinning solution in the technical scheme of the present invention can be selected as 22wt%-28wt%, further selected as 23wt%-25wt%, and further selected as 25wt%.

[0052] In addition, this embodiment has been explored and found that when the electrospinning process is a receiving distance of 20 cm, a voltage of 11 kV, and a receiving roller speed of 30 rpm, the jet is relatively stable and the micro-nano fiber deposition and stacking are good and fast. Therefore, the electrospinning process parameters are further selected as a receiving distance of 20 cm, a voltage of 11 kV, and a receiving roller speed of 30 rpm.

[0053] Example 4

[0054] Based on the preparation method of the grooved PAI micro-nano fiber aerogel shown in Example 1, this example explores and optimizes the amount of acetone added to the spinning solution. It should be noted that the specific process flow shown in this example is only a preferred display and does not limit the scope of protection of the present invention.

[0055] In this embodiment, a PAI / BMI spinning solution with a PAI concentration of 25 wt % is prepared, wherein the mass ratio of PAI to BMI is 5:1, and the organic solvent used is N,N-dimethylacetamide, or a binary organic solvent in which acetone is used to replace part of the N,N-dimethylacetamide.

[0056] Specifically, in this embodiment, the acetone addition amount is 0wt% (AC-0), 10wt% (AC-10), and 20wt% (AC-20) of the spinning solution, and the PAI spinning solution is further transferred to a 10ml syringe. The electrospinning process is used for spinning in an environment with a relative humidity of 90%, and the injection speed is 2ml·h -1A constant DC voltage of 12 kV was applied between the metal needle and the receiving roller, the receiving distance was kept at 18 cm, and the collecting speed of the receiving roller was 50 rpm. PAI micro-nano fiber aerogel was prepared by electrospinning. Comparison of SEM images of micro-nano fibers prepared by different spinning solutions Figure 4 , hydrophobic properties comparison Figure 5 .

[0057] like Figure 4 As shown, when the acetone mass fraction is 0wt%, the surface of the PAI micro-nano fiber is smooth and no groove structure is formed; when the acetone mass fraction is 10wt%, a shallow groove structure is formed on the surface of the micro-nano fiber. When the acetone mass fraction is further increased to 20wt%, the grooves on the surface of the micro-nano fiber deepen, forming obvious groove-shaped PAI micro-nano fibers. The exploratory experiment of this embodiment found that when the acetone mass fraction is increased to 30wt%, the spinning solution is prone to form solid agglomerates, which is not conducive to the electrospinning operation. Figure 5 It can be confirmed that the hydrophobicity of the grooved PAI micro-nano fiber aerogel is improved with the addition of acetone. When the amount of acetone added reaches 10wt%, the hydrophobicity improvement trend is more gentle. Therefore, the content of acetone in the spinning solution in the technical solution of the present invention can be selected to be less than 30wt%, further selected to be 5wt%-25wt%, further selected to be 10wt%-20wt%, and further selected to be 20%.

[0058] This example further tests the performance parameters of the prepared grooved PAI micro-nano fiber aerogel. When the amount of acetone added to the spinning solution is 10-20%, the diameter of the prepared grooved PAI micro-nano fiber is 2.8-3.2 μm, and the density of the grooved micro-nano fiber aerogel is 5.72-4.4 mg / cm 3 The contact angle of the grooved micro-nano fiber aerogel is 133.1~137.4°, and the thermal conductivity of the grooved micro-nano fiber aerogel material is 0.02718~0.02586W·m -1 K -1 ”.

[0059] Among them, the method for measuring the diameter of micro-nano fibers is as follows: import the SEM image of the sample into the image software, measure the diameters of 100 fibers, calculate their diameter distribution and then take the average value; density measurement method: weigh the mass of the measured sample and calculate its volume, and calculate it through the formula (density = mass m / volume V); contact angle test: use a contact angle meter to measure the contact angle; thermal conductivity measurement: the test results are analyzed by a thermal conductivity meter (hot disk), and the test standards used are: ISO22007-2.2; GBT32064-2015.

[0060] Example 5

[0061] Based on the preparation method of the grooved PAI micro-nano fiber aerogel shown in Example 1, this embodiment also includes thermal crosslinking treatment of the grooved PAI micro-nano fiber aerogel after the electrospinning is completed. In this embodiment, the problem of thermal crosslinking treatment is explored and optimized. It should be noted that the specific process flow shown in this embodiment is only a better display and does not limit the scope of protection of the present invention.

[0062] Specifically, in this embodiment, a spinning solution containing 25wt% PAI, 5wt% BMI, and 20%wt% acetone is used. Under 90% humidity conditions, the conditions for controlling the electrostatic method are a receiving distance of 20cm, a voltage of 11kV, and a receiving roller speed of 30rpm to obtain a grooved PAI micro-nano fiber aerogel PMNFA; then, thermal cross-linking is performed under different temperature conditions to form a cross-linked structure between the grooved PAI nanofibers, giving the aerogel structure stability.

[0063] In this embodiment, three thermal cross-linking temperature gradients are set, namely, 180°C (PMNFA-180°C), 200°C (PMNFA-200°C), and 220°C (PMNFA-220°C), and the treatment time is 1 hour. Figure 6 The optical photograph of the grooved PAI micro-nanofiber aerogel prepared under heat treatment conditions at 200°C is shown.

[0064] This example further tests the performance parameters of the grooved PAI micro-nano fiber aerogel after heat treatment. The density of the grooved PAI micro-nano fiber aerogel obtained after heat treatment at 180℃-220℃ for 1h is 7.02~20.55mg / cm 3 The tensile strength is 77.3~181.4kPa, the shrinkage is 13.5%~55.7%, and the thermal conductivity of the grooved PAI micro-nanofiber aerogel is 0.02586~0.03838W·m -1 K -1 .

[0065] Figure 7 The results show the bulkiness comparison between PMNFA aerogel without thermal crosslinking and aerogel thermally crosslinked at different temperature gradients, which verifies that the thermal crosslinking temperature of the present invention can be selected as 180-220°C; by comparison, it is found that the bulkiness of PMNFA-180°C and PMNFA-200°C aerogels is better than that of PMNFA-220°C.

[0066] Figure 8The tensile mechanical properties of PMNFA aerogel without thermal crosslinking and aerogel with different temperature gradient thermal crosslinking are shown in the figure. It can be confirmed that when the thermal crosslinking temperature is 180℃, the tensile strength is not significantly improved, when the thermal crosslinking temperature is 200℃, the tensile strength is significantly improved, and when the thermal crosslinking temperature is 220℃, the strain decreases sharply, and at Figure 7 It can be clearly observed that the grooved PAI micro-nanofiber aerogel shrinks significantly.

[0067] Fig. 9 The thermal insulation performance of PMNFA without thermal crosslinking and thermal crosslinking aerogels with different temperature gradients is compared. Figure 7-Figure 9 It can be confirmed that the temperature of thermal crosslinking in the technical solution of the invention can be selected as 180~220°C, and further selected as 200°C; the processing time can be selected as 1~2h.

[0068] Furthermore, in this example, the flame retardancy of PMNFA-200°C grooved PAI micro-nano fiber aerogel was tested. Fig.10 As shown in the figure, the specific operation process is: use tweezers to take a sample with an AC content of 20% and contact it with the flame of an alcohol lamp, and then leave the flame. During the observation process, it can be seen that there is no droplet phenomenon in the combustion process of the grooved PAI micro-nano fiber aerogel, and it extinguishes itself when leaving the fire, indicating that it can effectively prevent the spread of open flames, confirming that the grooved PAI micro-nano fiber aerogel of the present invention has excellent flame retardant properties.

[0069] It should be noted that the above contents are further detailed descriptions of the present invention in combination with specific implementation methods, and it cannot be determined that the specific implementation of the present invention is limited to these descriptions; the dimensional data of this embodiment does not necessarily limit the technical solution, but only shows one of the specific working conditions. For ordinary technicians in the technical field to which the present invention belongs, several simple improvements and modifications can be made without departing from the concept of the present invention, which should be regarded as falling within the scope of protection of the present invention.

Claims

1. A method for preparing grooved polyamide-imide micro-nano fiber aerogel, characterized in that: The following steps are involved: S1: dissolving polyamide-imide and bismaleimide in an organic solvent to obtain a spinning solution; the organic solvent comprises acetone and at least one selected from N,N-dimethylformamide, dimethyl sulfoxide, and N,N-dimethylacetamide; S2: The spinning solution is subjected to electrospinning to obtain the grooved polyamide-imide micro-nano fiber aerogel; The ambient humidity of the electrospinning operation is 45%-90%; the content of acetone in the spinning solution is less than 30wt%.

2. The method for preparing the grooved polyamide-imide micro-nano fiber aerogel according to claim 1, characterized in that: The ambient humidity of the electrospinning operation is 75%-90%.

3. The method for preparing the grooved polyamide-imide micro-nano fiber aerogel according to claim 1, characterized in that: The content of acetone in the spinning solution is 5wt%-25wt%.

4. The method for preparing the grooved polyamide-imide micro-nano fiber aerogel according to claim 3, characterized in that: The content of acetone in the spinning solution is 10wt%-20wt%.

5. The method for preparing the grooved polyamide-imide micro-nano fiber aerogel according to claim 1, characterized in that: The mass fraction of polyamide-imide in the spinning solution is 22wt%-28wt%.

6. The method for preparing the grooved polyamide-imide micro-nano fiber aerogel according to claim 1, characterized in that: The receiving distance of the electrospinning operation is 16-20 cm, the voltage is 9-12 kV, and the receiving roller speed is 30-60 rpm.

7. The method for preparing the grooved polyamide-imide micro-nano fiber aerogel according to claim 1, characterized in that: After the electrospinning is completed, the method further includes S3: performing a thermal cross-linking treatment on the grooved polyamide-imide micro-nano fiber aerogel; The temperature of the thermal crosslinking treatment is 180-220° C., and the treatment time is 1-2 hours.

8. A grooved polyamide-imide micro-nano fiber aerogel prepared by the preparation method according to any one of claims 1 to 7.