Modified biochar material as well as preparation method and application thereof

By activating straw powder, coal gangue powder and calcium-based bentonite in a mixed atmosphere of nitrogen and oxygen, and pyrolysis after esterification reaction, high porosity modified biochar material was prepared, and the existing biochar p-sulfate was solved. The problem of poor adsorption effect has achieved effective sulfate pollution removal and plant growth promotion.

CN118874407APending Publication Date: 2024-11-01ANHUI UNIVERSITY OF ARCHITECTURE

Patent Information

Application Number
CN202411006023.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-25
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

The existing biochar is not effective in adsorbing sulfate, especially the biochar prepared by a single reed straw cannot effectively improve the impact of sulfate pollution on reed growth, and calcination is performed during the preparation of composite biochar prepared from straw and coal gangue. The temperature is high and the adsorption effect does not meet expectations.

Method used

The straw powder, gangue powder and calcium-based bentonite were mixed in a mixed atmosphere of nitrogen and oxygen. The polyethylene glycol solution and OH- solution were added for esterification reaction, and then pyrolyzed in an inert gas to prepare a high porosity. and modified biochar material with good stability.

Benefits of technology

It improves the adsorption effect of biochar on sulfate, reduces the sulfate concentration in water, reduces the stress of sulfate on reeds, promotes plant growth, and effectively repairs sulfate pollution in water through the application of modified biochar materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118874407A_ABST
    Figure CN118874407A_ABST
Patent Text Reader

Abstract

The invention discloses a modified biochar material and a preparation method and application thereof, and belongs to the technical field of water pollution treatment materials.The preparation method comprises the steps that straw powder, coal gangue powder and bentonite are mixed and activated in the nitrogen and oxygen mixed atmosphere at the temperature of 80-120 DEG C, and an activated base material is obtained; adding a polyethylene glycol solution into the activated base material, uniformly mixing, adding an OH <->-containing solution, and carrying out esterification reaction at 20-40 DEG C to obtain a colloidal substance-loaded precursor; and heating the precursor loaded with the colloidal substance in inert gas to 550-600 DEG C, and carrying out pyrolysis to obtain the modified biochar material. The modified charcoal is used for repairing sulfate pollution in water, the content of sulfate in water is effectively reduced, and the problem that the concentration of sulfate in water is too high is solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of water pollution treatment materials, and in particular to a modified biochar material and a preparation method and application thereof. Background Art

[0002] Sulfate is a common anion in natural water systems. SO4 2- Increased concentrations may pose potential hazards to organisms and the ecological environment. Long-term exposure to high levels of SO4 in drinking water 2- It can cause symptoms such as diarrhea and indigestion, posing a threat to human health. In addition, high levels of SO4 2- When irrigating farmland, it will acidify the water, causing soil hardening and harming crop growth. The report shows that SO4 2- Concentration exceeds 400 mg·L -1 Far exceeds China's surface water quality standard, which is SO4 2- The limit is set at 250 mg·L -1 Therefore, an efficient and cost-effective method is required to remove SO4 from water. 2- , to mitigate potential risks to organisms and the environment.

[0003] Biochar has attracted much attention as an adsorbent due to its porous structure and cost-effectiveness. Current research on biochar focuses on the use of biochar to remove phosphorus, heavy metals and organic pollutants. Biochar usually comes from agricultural and forestry waste, such as wood, crop straw and fruit shells, as well as organic waste generated in industrial applications and urban life. Reed is a recognized aquatic ornamental herb that grows widely in wetland areas such as rivers and lakes and has ecological and economic significance. However, the growth of reed is easily affected by environmental conditions. Elevated sulfate concentrations can lead to slow growth, reduced height and yellowing of leaves, thereby reducing its value.

[0004] Effect of straw biochar on SO4 2-Solid wastes that lack sufficient adsorption capacity and contain elements such as calcium, magnesium, and iron are effective for biochar modification. These solid wastes can not only improve the stability, carbon fixation capacity, and pollutant adsorption efficiency of biochar, but also increase the nutrients and metal ions it contains, which have a certain positive effect on the adsorption effect of crops. For example, solid waste coal gangue is a metal-rich solid waste that poses a threat to land resources and environmental pollution when randomly stacked. The co-thermal dissolution of coal gangue and biomass changes the functional groups and surface charges of biochar, affecting its adsorption capacity for pollutants. The patent with publication number CN105854808A discloses a composite adsorption material based on straw and coal gangue and a preparation method thereof. Composite biochar is obtained by calcining straw and coal gangue, and the composite biochar is put into a copper sulfate solution for adsorption treatment for 15 minutes. The absorbance of the copper sulfate solution is reduced from 0.413 to 0.25. However, the composite biochar obtained by calcining straw and coal gangue has a relatively high calcination temperature during the preparation process and the adsorption effect of the composite biochar on sulfate ions needs to be further improved. To this end, the present invention provides a modified biochar material and a preparation method and application thereof. Summary of the invention

[0005] The present invention provides a modified biochar material and a preparation method and application thereof, which effectively solves the problem of biochar prepared from single reed straw on SO4 2- The adsorption capacity is effective, but it cannot effectively improve the growth environment of reed plants; although the adsorption capacity of composite biochar prepared from straw and coal gangue is improved, the calcination temperature in the preparation process is high and the composite biochar has a poor adsorption capacity for SO4 2- The technical problem that the adsorption effect still cannot achieve the expected effect is solved, and at the same time a modified biochar with good stability, high activity and high porosity is provided.

[0006] The first object of the present invention is to provide a method for preparing a modified biochar material, characterized in that it comprises the following steps:

[0007] The straw powder, coal gangue powder and calcium-based bentonite are mixed and activated in a nitrogen and oxygen mixed atmosphere at 80-120° C. to obtain an activated substrate;

[0008] Adding polyethylene glycol solution to the activated substrate, mixing well, adding OH-containing solution, and performing esterification reaction at 20-40° C. to obtain a precursor of the loaded colloidal substance;

[0009] The precursor of the loaded colloid substance is heated to 550-600° C. in an inert gas and pyrolyzed to obtain a modified biochar material.

[0010] As a preferred implementation manner, the mass ratio of the straw powder, coal gangue powder and calcium-based bentonite is 1:0.5-2.5:0.2-1.8.

[0011] As a preferred embodiment, the molecular weight of the polyethylene glycol is 300-600, and the usage ratio of the straw powder, polyethylene glycol and OH- is 1g:0.005-0.012mol:0.001-0.01mol.

[0012] As a preferred implementation, the flow rate of the mixed atmosphere is 50-100 sccm, and the content of oxygen in the mixed atmosphere is 5% to 20%.

[0013] As a preferred embodiment, the activation treatment time is 0.5 to 2 hours.

[0014] As a preferred embodiment, the esterification reaction time is 1 to 3 hours.

[0015] As a preferred embodiment, the pyrolysis time is 2 to 4 hours.

[0016] As a preferred embodiment, after pyrolysis, the primary product is obtained, which is immersed in a 1 mol / L hydrochloric acid solution for 24 hours, washed to neutrality, and dried to obtain a modified biochar material.

[0017] The second object of the present invention is to provide a modified biochar material prepared by the above preparation method.

[0018] The third object of the present invention is to provide an application of the above-mentioned modified biochar material in remediating sulfate pollution in water bodies, characterized in that the modified biochar material is added to a sulfate water body with a concentration of 0 to 1000 mg / L according to a dosage ratio of 0.5 to 5 g:500 mL of modified biochar material to water body.

[0019] Compared with the prior art, the present invention has the following beneficial effects:

[0020] The present invention provides a modified biochar material and a preparation method and application thereof. First, straw powder, coal gangue powder and bentonite are mixed, and activated in a nitrogen and oxygen mixed atmosphere at 80-120° C. to obtain an activated substrate; a polyethylene glycol solution is added to the activated substrate, mixed, and an OH-containing -The solution is subjected to an esterification reaction at 20 to 40°C to obtain a precursor of a loaded colloidal substance; the precursor of the loaded colloidal substance is heated to 550 to 600°C in an inert gas, and pyrolyzed to obtain a modified biochar material. The present invention adds bentonite to straw powder and coal gangue powder, and first activates it through a mixed atmosphere of nitrogen and oxygen to oxidize the ferrous iron in the bentonite crystals to trivalent iron, thereby increasing the proportion of the expanded layer of the bentonite. In the subsequent heating and pyrolysis process, the bentonite pyrolysis releases a large amount of water vapor, thereby generating more void structures, thereby increasing the mesoporous structure on the surface of the biochar material. In addition, polyethylene glycol and OH are added to the activated substrate. - An esterification reaction occurs to produce a composite colloidal substance, and after high-temperature pyrolysis, the composite colloidal substance is partially decomposed to produce pores, thereby further improving the pore adsorption effect of the modified biochar material.

[0021] The modified biochar prepared by the present invention was used to repair sulfate pollution in water bodies. The results showed that the modified biochar prepared by the present invention effectively reduced the sulfate content in water and solved the problem of excessive sulfate concentration in water. At the same time, the modified biochar material can reduce the stress of sulfate on reeds by reducing the activity of antioxidant enzymes and malondialdehyde content in the body and increasing the content of chlorophyll and soluble protein, thereby promoting plant growth. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 The SEM images of the modified biochar prepared in Example 1 of the present invention and the unmodified biochar of Comparative Example 1; wherein, Figure A is the unmodified biochar of Comparative Example 1, and Figure B is the modified biochar of Example 1;

[0023] Figure 2 EDS graphs of the modified biochar prepared in Example 1 of the present invention and the unmodified biochar of Comparative Example 1; wherein, Figure A is the unmodified biochar of Comparative Example 1, and Figure B is the modified biochar of Example 1;

[0024] Figure 3 FTIR graphs of the modified biochar prepared in Example 1 of the present invention and the unmodified biochar of Comparative Example 1; wherein A and C are the FTIR graphs of the modified biochar of Example 1 before and after adsorption, respectively, and B and D are the FTIR graphs of the unmodified biochar of Comparative Example 1 before and after adsorption, respectively;

[0025] Figure 4 This is a diagram showing the adsorption effect of sulfate on water bodies with different initial pH values ​​when the modified biochar prepared in Example 1 of the present invention is added;

[0026] Figure 5 This is a diagram showing the adsorption effect of sulfate by adding different amounts of modified biochar prepared in Example 1 of the present invention;

[0027] Figure 6 This is a diagram showing the adsorption effect of modified biochar prepared in Example 1 of the present invention on sulfate at different adsorption times;

[0028] Figure 7 This is a diagram showing the adsorption effect of modified biochar prepared in Example 1 of the present invention on sulfate at different sulfate concentrations;

[0029] Figure 8 The graph shows the changes in physiological indicators of reed under sulfate stress after the modified biochar prepared by Example 1 of the present invention is used; wherein, (a) is the chlorophyll content at different sulfate concentrations measured on the 60th day after the addition of the modified biochar; (b) is the SOD content at different sulfate concentrations measured on the 60th day after the addition of the modified biochar; (c) is the POT content at different sulfate concentrations measured on the 60th day after the addition of the modified biochar; (d) is the CAT content at different sulfate concentrations measured on the 60th day after the addition of the modified biochar; (e) is the MDA content at different sulfate concentrations measured on the 60th day after the addition of the modified biochar; (f) is the SP content at different sulfate concentrations measured on the 60th day after the addition of the modified biochar; Note: Different letters indicate significant differences at the p<0.05 level. DETAILED DESCRIPTION

[0030] In order to enable those skilled in the art to better understand the technical solution of the present invention and implement it, the present invention is further described below in conjunction with specific embodiments and drawings, but the embodiments are not intended to limit the present invention. The following test methods and detection methods, unless otherwise specified, are conventional methods; the reagents and raw materials, unless otherwise specified, are commercially available.

[0031] Regarding the SO4 2- The adsorption capacity is effective, but it cannot effectively improve the growth environment of reed plants; although the adsorption capacity of composite biochar prepared from straw and coal gangue is improved, the calcination temperature in the preparation process is high and the composite biochar has a poor adsorption capacity for SO4 2- The adsorption effect of the biochar still cannot achieve the expected effect. The present invention provides a modified biochar and a preparation method and application thereof. Straw powder, coal gangue powder and bentonite are mixed, and activated in a mixed atmosphere of nitrogen and oxygen at 80-120°C to obtain an activated substrate; a polyethylene glycol solution is added to the activated substrate, mixed evenly, an OH-containing solution is added, and an esterification reaction is carried out at 20-40°C to obtain a precursor of a loaded colloidal substance; the precursor of the loaded colloidal substance is heated to 550-600°C in an inert gas, and pyrolyzed to obtain a modified biochar material with good stability, high activity and high porosity.

[0032] The technical solution of the present invention is described in detail below.

[0033] The present invention first provides a method for preparing a modified biochar material, comprising the following steps:

[0034] Straw powder, coal gangue powder and calcium-based bentonite are mixed, and activated in a mixed atmosphere of nitrogen and oxygen at 80-120°C to obtain an activated substrate; bentonite is added to straw powder and coal gangue powder, and activated in a mixed atmosphere of nitrogen and oxygen for 0.5-2h to oxidize the ferrous iron in the bentonite crystals into trivalent iron, thereby increasing the proportion of the expanded layer of the bentonite. In the subsequent pyrolysis process of heating, the bentonite releases a large amount of water vapor due to pyrolysis, thereby producing more void structures, thereby increasing the mesoporous structure on the surface of the biochar material.

[0035] Add polyethylene glycol solution to the activated substrate, mix well, and add OH - The solution is subjected to esterification reaction at 20-40°C for 1-3h to obtain a precursor of the loaded colloidal substance;

[0036] The precursor of the loaded colloidal substance is heated to 550-600°C in an inert gas, pyrolyzed for 2-4 hours to obtain a primary product, which is then immersed in a 1 mol / L hydrochloric acid solution for 24 hours, washed to neutrality, and dried to obtain a modified biochar material. - An esterification reaction occurs to produce a composite colloidal substance, and after high-temperature pyrolysis, the composite colloidal substance is partially decomposed to produce holes, thereby further improving the pore adsorption effect of the modified biochar material.

[0037] In order to enrich the pore structure of the modified biochar and increase its adsorption effect on sulfate, the mass ratio of the straw powder, coal gangue powder and calcium-based bentonite is 1:0.5-2.5:0.2-1.8.

[0038] In order to further improve the pore structure of the modified biochar, the molecular weight of the polyethylene glycol is 300-600, and the usage ratio of the straw powder, polyethylene glycol and OH- is 1g:0.005-0.012mol:0.001-0.01mol.

[0039] In order to activate bentonite and increase the pore structure on the surface of biochar, the flow rate of the mixed atmosphere is 50-100 sccm, and the content of oxygen in the mixed atmosphere is 5%-20%.

[0040] The modified biochar material is applied to repair sulfate pollution in water bodies, specifically: the modified biochar material is added to a sulfate water body with a concentration of 0 to 1000 mg / L according to a dosage ratio of 0.5 to 5 g of modified biochar material to 500 mL of water.

[0041] The effects are described below through specific embodiments and comparative examples.

[0042] Example 1

[0043] A method for preparing a modified biochar material comprises the following steps:

[0044] S1, mixing straw powder, coal gangue powder and calcium-based bentonite in a mass ratio of 1:0.5:0.2, and activating the mixture in a nitrogen and oxygen mixed atmosphere at 80° C. for 0.5 h to obtain an activated substrate; the flow rate of the mixed atmosphere is 100 sccm, and the oxygen content in the mixed atmosphere is 5%;

[0045] S2, adding a polyethylene glycol solution with a molecular weight of 300 to the activated substrate according to the ratio of straw powder, polyethylene glycol and OH-1g: 0.005mol: 0.001mol, mixing, adding a polyethylene glycol solution containing OH - The solution was subjected to esterification reaction at 30°C for 2 h to obtain a precursor of the loaded colloidal substance;

[0046] S3, heating the precursor of the loaded colloidal substance to 600° C. in an inert gas, pyrolyzing for 2 h to obtain a primary product, immersing it in a 1 mol / L hydrochloric acid solution for 24 h, washing it to neutrality, and drying it to obtain a modified biochar material.

[0047] Example 2

[0048] A method for preparing a modified biochar material comprises the following steps:

[0049] S1, mixing straw powder, coal gangue powder and calcium-based bentonite in a mass ratio of 1:2.5:1.8, and activating the mixture in a nitrogen and oxygen mixed atmosphere at 120° C. for 2 h to obtain an activated substrate; the flow rate of the mixed atmosphere is 80 sccm, and the oxygen content in the mixed atmosphere is 20%;

[0050] S2, adding a polyethylene glycol solution with a molecular weight of 600 to the activated substrate according to the ratio of straw powder, polyethylene glycol and OH-1g:0.012mol:0.01mol, mixing, adding a polyethylene glycol solution containing OH - The solution was subjected to esterification reaction at 40°C for 1 h to obtain a precursor of the loaded colloidal substance;

[0051] S3, heating the precursor of the loaded colloidal substance to 550° C. in an inert gas, pyrolyzing for 3 h to obtain a primary product, immersing it in a 1 mol / L hydrochloric acid solution for 24 h, washing it to neutrality, and drying it to obtain a modified biochar material.

[0052] Example 3

[0053] A method for preparing a modified biochar material comprises the following steps:

[0054] S1, mixing straw powder, coal gangue powder and calcium-based bentonite in a mass ratio of 1:0.5:1.8, and activating the mixture in a nitrogen and oxygen mixed atmosphere at 100° C. for 1 h to obtain an activated substrate; the flow rate of the mixed atmosphere is 50 sccm, and the oxygen content in the mixed atmosphere is 10%;

[0055] S2, adding a polyethylene glycol solution with a molecular weight of 500 to the activated substrate according to the ratio of straw powder, polyethylene glycol and OH-1g: 0.012mol: 0.001mol, mixing, adding a polyethylene glycol solution containing OH - The solution was subjected to esterification reaction at 20°C for 3 h to obtain a precursor of the loaded colloidal substance;

[0056] S3, heating the precursor of the loaded colloidal substance to 580° C. in an inert gas, pyrolyzing for 4 hours to obtain a primary product, immersing it in a 1 mol / L hydrochloric acid solution for 24 hours, washing it to neutrality, and drying it to obtain a modified biochar material.

[0057] Example 4

[0058] A method for preparing a modified biochar material comprises the following steps:

[0059] S1, mixing straw powder, coal gangue powder and calcium-based bentonite in a mass ratio of 1:2.5:0.2, and activating the mixture in a nitrogen and oxygen mixed atmosphere at 90° C. for 1.5 h to obtain an activated substrate; the flow rate of the mixed atmosphere is 60 sccm, and the oxygen content in the mixed atmosphere is 15%;

[0060] S2, adding a polyethylene glycol solution with a molecular weight of 400 to the activated substrate according to the ratio of straw powder, polyethylene glycol and OH-1g: 0.005mol: 0.01mol, mixing, adding a polyethylene glycol solution containing OH - The solution was subjected to esterification reaction at 25°C for 2.5 h to obtain a precursor of the loaded colloidal substance;

[0061] S3, heating the precursor of the loaded colloidal substance to 600° C. in an inert gas, pyrolyzing for 3.5 h to obtain a primary product, immersing it in a 1 mol / L hydrochloric acid solution for 24 h, washing it to neutrality, and drying it to obtain a modified biochar material.

[0062] Example 5

[0063] A method for preparing a modified biochar material comprises the following steps:

[0064] S1, mixing straw powder, coal gangue powder and calcium bentonite in a mass ratio of 1:1:1, and activating the mixture in a nitrogen and oxygen mixed atmosphere at 110° C. for 2 h to obtain an activated substrate; the flow rate of the mixed atmosphere is 70 sccm, and the oxygen content in the mixed atmosphere is 5%;

[0065] S2, according to straw powder, polyethylene glycol and OH - 1g:0.01mol:0.005mol ratio of polyethylene glycol solution with a molecular weight of 600 was added to the activated substrate, mixed well, and OH-containing - The solution was subjected to esterification reaction at 35°C for 1.5 h to obtain a precursor of the loaded colloidal substance;

[0066] S3, heating the precursor of the loaded colloidal substance to 560° C. in an inert gas, pyrolyzing for 2.5 h to obtain a primary product, immersing it in a 1 mol / L hydrochloric acid solution for 24 h, washing it to neutrality, and drying it to obtain a modified biochar material.

[0067] Example 6

[0068] A method for preparing a modified biochar material comprises the following steps:

[0069] S1, mixing straw powder, coal gangue powder and calcium-based bentonite in a mass ratio of 1:1.5:1.5, and activating the mixture in a nitrogen and oxygen mixed atmosphere at 120° C. for 1 h to obtain an activated substrate; the flow rate of the mixed atmosphere is 90 sccm, and the oxygen content in the mixed atmosphere is 10%;

[0070] S2, according to straw powder, polyethylene glycol and OH - 1g:0.01mol:0.01mol ratio was added to the activated substrate, the polyethylene glycol solution with a molecular weight of 400 was mixed, and OH-containing - The solution was subjected to esterification reaction at 40°C for 2 h to obtain a precursor of the loaded colloidal substance;

[0071] S3, heating the precursor of the loaded colloidal substance to 550° C. in an inert gas, pyrolyzing for 4 hours to obtain a primary product, immersing it in a 1 mol / L hydrochloric acid solution for 24 hours, washing it to neutrality, and drying it to obtain a modified biochar material.

[0072] Example 7

[0073] A method for preparing a modified biochar material comprises the following steps:

[0074] S1, mixing straw powder, coal gangue powder and calcium-based bentonite in a mass ratio of 1:2:0.5, and activating the mixture in a nitrogen and oxygen mixed atmosphere at 80° C. for 0.5 h to obtain an activated substrate; the flow rate of the mixed atmosphere is 100 sccm, and the oxygen content in the mixed atmosphere is 20%;

[0075] S2, according to straw powder, polyethylene glycol and OH - 1g:0.005mol:0.008mol ratio of polyethylene glycol solution with a molecular weight of 300 was added to the activated substrate, mixed, and OH-containing - The solution was subjected to esterification reaction at 30°C for 1 h to obtain a precursor of the loaded colloidal substance;

[0076] S3, heating the precursor of the loaded colloidal substance to 600° C. in an inert gas, pyrolyzing for 3 h to obtain a primary product, immersing it in a 1 mol / L hydrochloric acid solution for 24 h, washing it to neutrality, and drying it to obtain a modified biochar material.

[0077] Example 8

[0078] A method for preparing a modified biochar material comprises the following steps:

[0079] S1, mixing straw powder, coal gangue powder and calcium-based bentonite in a mass ratio of 1:2:1, and activating the mixture in a nitrogen and oxygen mixed atmosphere at 100° C. for 1 h to obtain an activated substrate; the flow rate of the mixed atmosphere is 60 sccm, and the oxygen content in the mixed atmosphere is 15%;

[0080] S2, adding a polyethylene glycol solution with a molecular weight of 500 to the activated substrate according to the ratio of straw powder, polyethylene glycol and OH-1g:0.01mol:0.001mol, mixing, adding a polyethylene glycol solution containing OH - The solution was subjected to esterification reaction at 20°C for 3 h to obtain a precursor of the loaded colloidal substance;

[0081] S3, heating the precursor of the loaded colloidal substance to 580° C. in an inert gas, pyrolyzing for 2 h to obtain a primary product, immersing it in a 1 mol / L hydrochloric acid solution for 24 h, washing it to neutrality, and drying it to obtain a modified biochar material.

[0082] In order to further illustrate the technical effect of the present invention, the present invention is also provided with a comparative example, as follows:

[0083] Comparative Example 1

[0084] Compared with Example 1, the difference is that the straw powder is not subjected to modification treatment, but is directly pyrolyzed to obtain unmodified biochar.

[0085] A method for preparing a biochar material comprises the following steps:

[0086] The straw powder was heated to 600°C in an inert gas and pyrolyzed for 2 h to obtain a primary product, which was then immersed in a 1 mol / L hydrochloric acid solution for 24 h, washed to neutrality, and dried to obtain a biochar material, namely BC.

[0087] Characterization of the modified biochar material prepared by the present invention

[0088] 1. Morphological characterization and analysis

[0089] Since the performance of the modified biochar materials prepared in Examples 1 to 8 of the present invention are similar, Example 1 is taken as an example to illustrate the effect.

[0090] Figure 1 The SEM images of the modified biochar prepared in Example 1 of the present invention and the unmodified biochar prepared in Comparative Example 1 are shown in FIG. Figure 1 It can be seen that the unmodified biochar presents a dense structure with a smooth surface. After co-pyrolysis with coal gangue, the surface of the modified biochar is rough, forming coal gangue flocculent particles.

[0091] Figure 2 The EDS images of the modified biochar prepared in Example 1 of the present invention and the unmodified biochar of Comparative Example 1 are shown in FIG. Figure 2 It can be seen that the main components of unmodified biochar and modified biochar are C and O, respectively. After modification with coal gangue, the contents of Si and Al increased, which is the reason for the addition of coal gangue.

[0092] Figure 3 FTIR images of the modified biochar prepared in Example 1 of the present invention and the unmodified biochar of Comparative Example 1. Figure 3 It can be seen that the vibration bands of the two adsorbents are mainly concentrated at 3400 cm -1 , 1631cm -1 , 1589cm -1 , 1350cm -1 , 1087cm -1 , 762cm -1 Nearby, they are caused by -OH stretching vibration, -COOH stretching, C=C stretching, CH deformation, Si-O antisymmetric stretching and Al-O symmetric stretching. At the -OH, -COOH and C=C vibration bands, the peak intensity of the modified biochar is weakened, indicating that dehydrogenation and deoxygenation reactions occur during modification, the structural water decreases, and the pore structure increases. The increase in Si-O and Al-O intensity is due to the addition of coal gangue. From the FTIR graph after the modified biochar adsorbs sulfate, it can be seen that the intensity of C=O, C=C, Si-O and Al-O of the modified biochar decreases, indicating that they are involved in the adsorption of sulfate.

[0093] 2. Characterization of sulfate adsorption performance

[0094] Figure 4 This is a diagram showing the adsorption effect of sulfate on water bodies with different initial pH values ​​when the modified biochar prepared in Example 1 of the present invention is added.

[0095] Prepare a 500 mg / L sulfate solution, add an adsorbent so that the adsorbent content is 8 g / L, then shake at 25°C and adjust the pH to 2-12. After a period of time, take out the aqueous solution, collect the aqueous solution, measure the remaining sulfate concentration in the solution, and calculate the adsorption capacity q at a certain time. e , the specific results are as follows Figure 4 As shown in the figure, with the increase of pH, the adsorption capacity of both unmodified biochar and modified biochar showed a downward trend. When the pH increased from 2 to 12, the adsorption capacity of modified biochar for sulfate increased from 47.73 mg·g -1 Reduced to 20.14 mg g -1 The adsorption capacity of unmodified biochar for sulfate increased from 20.99 mg·g -1 Reduced to 13.17 mg g -1 , and in the pH range of 4.0-6.0, the rate of decrease is faster than in other ranges. This is because lower pH is conducive to the protonation of the adsorbent surface, so the adsorbent surface can carry more positive charges, thereby enhancing the adsorbent surface and SO4 2- The electrostatic interaction between them promotes the 2- When the pH of the solution is too high, OH- in the water will react with SO4 2- competition for active sites, resulting in a decrease in the adsorption capacity.

[0096] Figure 5 This is a diagram showing the adsorption effect of sulfate on modified biochar prepared in Example 1 of the present invention with different amounts added.

[0097] As the amount of adsorbent increased, the sulfate removal rate gradually increased from 31% at 0.05g to 79.68% at 0.5g. This is because the adsorption active sites increased with the increase in the amount of adsorbent. -1 When the dosage increases, the removal rate does not change significantly. This is because the contact specific surface area between sulfate and adsorbent is close to saturation and can no longer combine with more active sites.

[0098] Figure 6 This is a diagram showing the adsorption effect of modified biochar prepared in Example 1 of the present invention on sulfate at different adsorption times.

[0099] Prepare a 500 mg / L sulfate solution, add an adsorbent so that the adsorbent content is 8 g / L, then oscillate at 25°C. Take out the aqueous solution at regular intervals, collect the aqueous solution, measure the remaining sulfate concentration in the solution, and calculate the adsorption capacity q at a certain time. t , the specific results are as follows Figure 6 As shown in Figure 2, the process of sulfate adsorption by modified biochar can be divided into rapid adsorption, slow adsorption and adsorption equilibrium stages. After 2 h of adsorption, the adsorption capacity increased to 48.65 mg g -1 This is because there are a large number of adsorption sites on the surface of the adsorbent in the early stage, which can be quickly occupied by sulfate ions, but as time goes by, the adsorption sites are gradually saturated until an equilibrium state is reached.

[0100] Figure 7 This is a diagram showing the adsorption effect of modified biochar prepared in Example 1 of the present invention on sulfate at different sulfate concentrations.

[0101] Prepare sulfate solutions with different initial concentrations (300-800 mg / L), add adsorbent to make the adsorbent content 8 g / L, and then oscillate at 25°C. Take out the aqueous solution at regular intervals, collect the aqueous solution, measure the remaining sulfate concentration in the solution, and calculate the adsorption capacity q at a certain time. e The Langmuir model (the equation is ), Freundlich model (the equation is q e =K F ρ e n ) was used to analyze the adsorption isotherm of sulfate removal by adsorbent, where qe and qm are the equilibrium adsorption capacity and the maximum adsorption capacity, respectively, and ρ e is the adsorption equilibrium concentration, K L (L / mg) and K F (L / g) are the Langmuir and Freundlich constants related to adsorption intensity, and n is the Freundlich constant related to adsorption capacity. Figure 7 As shown in the figure: When the initial sulfate concentration is low, the adsorption capacity increases rapidly. As the initial concentration gradually increases, the adsorption capacity increases slowly and finally stabilizes. This is mainly because the adsorption sites provided by the adsorbent are fixed. When the sulfate concentration increases, more and more sulfate cannot occupy the adsorption sites, and the adsorption capacity reaches saturation. Langmuir's R 2 The Langmuir coefficient is 0.968, which is larger than Freundlich, so Langmuir can better describe the adsorption behavior of modified biochar on sulfate. This shows that the adsorption of sulfate by modified biochar is mainly monolayer uniform adsorption.

[0102] Figure 8 The figure shows the changes in physiological indicators of reed under sulfate stress after the modified biochar prepared by Example 1 of the present invention is used; wherein, (a) is the chlorophyll content at different sulfate concentrations measured on the 60th day after the addition of the modified biochar; (b) is the superoxide dismutase (SOD) content at different sulfate concentrations measured on the 60th day after the addition of the modified biochar; (c) is the peroxidase (POT) content at different sulfate concentrations measured on the 60th day after the addition of the modified biochar; (d) is the catalase (CAT) content at different sulfate concentrations measured on the 60th day after the addition of the modified biochar; (e) is the malondialdehyde (MDA) content at different sulfate concentrations measured on the 60th day after the addition of the modified biochar; (f) is the soluble protein (SP) content at different sulfate concentrations measured on the 60th day after the addition of the modified biochar; Note: Different letters indicate significant differences at the p<0.05 level.

[0103] Figure 8 Figure (a) shows the chlorophyll content under different sulfate concentrations measured on the 60th day of the experiment. As the sulfate concentration increased, the chlorophyll content decreased significantly (P < 0.05). This is because high salt stress can destroy the ultrastructure and membrane system of chloroplasts and reduce the activity of chlorophyll synthase, resulting in a significant decrease in chlorophyll content. The chlorophyll content determines the intensity of plant photosynthesis. The increase in chlorophyll content increases the utilization rate of photosynthesis and is beneficial to the growth and development of plants. This shows that the application of modified biochar has a positive effect on the growth of reeds.

[0104] Figure 8 Figure (b) shows the SOD content under different sulfate concentrations measured on the 60th day of the experiment. With the increase of sulfate concentration, the SOD activity of reeds in the blank group and modified biochar first increased and then decreased. This is because when plants are under stress, they will increase SOD activity to reduce the damage caused by stress, but when the stress reaches a certain level, the cell membrane system of the plant will form irreversible damage, resulting in a decrease in reed SOD activity. Compared with reeds without sulfate addition, the POD activity of reeds under sulfate stress was significantly increased (P < 0.05), indicating that salt stress can promote enzymatic oxidative stress response in reeds.

[0105] Figure 8 Figure (c) shows the POT content at different sulfate concentrations measured on the 60th day of the experiment. H2O2 generated by SOD is still toxic to plants, and H2O2 needs to be decomposed into H2O and O2 by POD and CAT. As the sulfate concentration increases, the POD activity in both experiments first increases and then decreases with the increase in sulfate concentration. When the sulfate concentration is 600 mg·g-1, the POD activity is the highest.

[0106] Figure 8 Figure (d) shows the CAT content under different sulfate concentrations measured on the 60th day of the experiment. When the sulfate concentration was too high or too low, the addition of modified biochar had no significant effect on CAT activity (P < 0.05).

[0107] Figure 8 Figure (e) shows the MDA content under different sulfate concentrations measured on the 60th day of the experiment. As the sulfate concentration increased, the MDA content of both the blank group and the modified biochar group increased, indicating that the higher the concentration, the greater the stress on the reed. Compared with the reed without modified biochar, the MDA content of the reed with modified biochar decreased. This shows that the addition of modified biochar can reduce the sulfate stress on plants by reducing the production of MDA.

[0108] Figure 8 Figure (f) shows the SP content at different sulfate concentrations measured on the 60th day of the experiment. As the sulfate concentration continued to increase, the SP content first increased and then decreased. Compared with the CK group without modified biochar, the SP content of the modified biochar group increased at different sulfate concentrations. The increase in SP content is beneficial to maintaining cell homeostasis and resisting the adverse effects of sulfate stress.

[0109] In summary, the modified biochar prepared by the present invention is used to repair sulfate pollution in water bodies, effectively reducing the sulfate content in water and solving the problem of excessive sulfate concentration in water. At the same time, the modified biochar material can reduce the stress of sulfate on reeds by reducing the activity of antioxidant enzymes and malondialdehyde content in the body and increasing the content of chlorophyll and soluble protein, thereby promoting plant growth.

[0110] Obviously, those skilled in the art can make various changes and modifications to the present invention without departing from the spirit and scope of the present invention. Thus, if these modifications and variations of the present invention fall within the scope of the claims of the present invention and their equivalents, the present invention is also intended to include these modifications and variations.

Claims

1. A method for preparing a modified biochar material, characterized in that: The following steps are involved: The straw powder, coal gangue powder and calcium-based bentonite are mixed and activated in a nitrogen and oxygen mixed atmosphere at 80-120° C. to obtain an activated substrate; Adding polyethylene glycol solution to the activated substrate, mixing well, adding OH-containing solution, and performing esterification reaction at 20-40° C. to obtain a precursor of the loaded colloidal substance; The precursor of the loaded colloid substance is heated to 550-600° C. in an inert gas and pyrolyzed to obtain a modified biochar material.

2. The preparation method according to claim 1, characterized in that: The mass ratio of the straw powder, coal gangue powder and calcium-based bentonite is 1:0.5-2.5:0.2-1.

8.

3. The preparation method according to claim 1, characterized in that: The molecular weight of the polyethylene glycol is 300-600, and the usage ratio of the straw powder, polyethylene glycol and OH- is 1g: 0.005-0.012mol: 0.001-0.01mol.

4. The preparation method according to claim 1, characterized in that: The flow rate of the mixed atmosphere is 50-100 sccm, and the content of oxygen in the mixed atmosphere is 5%-20%.

5. The preparation method according to claim 1, characterized in that: The activation treatment time is 0.5 to 2 hours.

6. The preparation method according to claim 1, characterized in that: The esterification reaction time is 1 to 3 hours.

7. The preparation method according to claim 1, characterized in that: The pyrolysis time is 2 to 4 hours.

8. The preparation method according to claim 1, characterized in that: After pyrolysis, the primary product was obtained, which was immersed in a 1 mol / L hydrochloric acid solution for 24 h, washed to neutrality, and dried to obtain a modified biochar material.

9. A modified biochar material prepared by the preparation method according to any one of claims 1 to 8.

10. Use of the modified biochar material according to claim 9 in remediating sulfate pollution in water bodies.

Citation Information

Patent Citations

  • Composite adsorbing material based on straw and coal gangue and preparation method thereof

    CN105854808A

  • Modified composite biochar, preparation method and applications thereof

    CN110694588A

  • Modified charcoal / attapulgite composite material as well as preparation method and application thereof

    CN114870800A

  • Agricultural biological wetting agent for culture medium as well as preparation method and application of agricultural biological wetting agent

    CN117413746A

Cited By

  • Carbon-based calcium peroxide material with oxygen slow-release function as well as preparation method and application of carbon-based calcium peroxide material

    CN120289243A