Phosphorus-nitrogen synergistic structure type flame-retardant PET (polyethylene terephthalate) and preparation method thereof
By synthesizing melamine diphenyl phosphite and terephthalate covalently during PET polycondensation, a phosphorus-nitrogen synergistic flame-retardant PET structure was prepared, solving the problems of PET flammability and dripping, and improving the flame retardant effect and mechanical properties.
Patent Information
- Application Number
- CN202411107948.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-13
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2044-08-13
AI Technical Summary
The flammability of PET and the severe flame dripping phenomenon during combustion limit its application in medical, aerospace, and home applications. Existing flame retardants are prone to migration and instability in PET, leading to secondary fires and burns.
Melamine diphenyl phosphite was synthesized using the Atherton-Todd reaction and used as a phosphorus-nitrogen flame retardant chain extender. It then formed covalent bonds with terephthalic acid and ethylene glycol during the PET polycondensation process to prepare a phosphorus-nitrogen synergistic flame retardant PET.
It achieves highly efficient flame retardancy of PET, forming a uniform charcoal foam layer that provides heat insulation, oxygen isolation, and smoke suppression, thereby improving the thermal stability and mechanical properties of PET and preventing dripping.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of polyester material preparation, and specifically relates to a phosphorus-nitrogen synergistic structural flame-retardant PET and a preparation method thereof. Background Art
[0002] Semi-crystalline thermoplastic polymer polyethylene terephthalate (PET) has been widely used in beverage bottles, fibers, films, transportation and other fields due to its good mechanical properties, fatigue resistance, chemical resistance, spinnability and low cost to meet the diverse needs of daily life. However, when considering fire safety requirements, PET's flammability and the serious flame droplets accompanying the combustion process make it prone to fire and secondary injuries. This seriously limits the application of PET in medical, aviation, home and other materials.
[0003] At present, the main means to improve the flame retardant effect of PET is to add flame retardants to the formula. Flame retardants are mainly divided into two categories: additive flame retardants and structural flame retardants. Compared with additive flame retardants, structural flame retardants mainly participate in the reaction during the polymerization or polycondensation process and are combined with the main chain or side chain of the polymer to play a flame retardant role. Since this type of flame retardant partially participates in the reaction and is combined with the polymer chain structure, it has good stability and is not easy to migrate. Among them, phosphorus-containing flame retardants are highly valued for their high flame retardant efficiency, good thermal stability, low toxicity and environmental friendliness. Unfortunately, when most phosphorus-containing flame retardants are flame-retardant for PET, they will also cause serious melting droplets of PET when exposed to fire, resulting in secondary fires and direct burns. The other type of nitrogen-based flame retardants mainly release non-combustible gases during the decomposition process, reduce the concentration of combustible gases, and play a flame retardant role. Therefore, there is a certain synergistic and synergistic effect between the phosphorus and nitrogen flame retardant elements. The emerging phosphorus and nitrogen synergistic flame retardant is a type of environmentally friendly flame retardant. When its products are burning, a uniform carbon foam layer is formed on the surface of the product. The foam layer has the functions of heat insulation, oxygen isolation, smoke suppression and dripping prevention. It is in line with the current trend of low-toxicity and low-smoke flame retardants. It is considered to be one of the future development directions of flame retardants and has become a hot spot in the flame retardant field in recent years. Summary of the invention
[0004] The purpose of the present invention is to provide a phosphorus-nitrogen synergistic structural flame-retardant PET and a preparation method thereof. Melamine is combined with diphenyl phosphite through an Atherton-Todd reaction to prepare a phosphorus-nitrogen-containing flame-retardant chain extender (melamine diphenyl phosphite), and melamine diphenyl phosphite is further polymerized with terephthalic acid, dimethyl terephthalate, and ethylene glycol prepolymer to prepare a structural flame-retardant PET.
[0005] In order to achieve the above object, the technical solution adopted by the present invention is as follows:
[0006] The present invention first provides a phosphorus-nitrogen-containing flame retardant chain extender, namely melamine diphenyl phosphite, and the preparation method thereof is as follows:
[0007] (1) dissolving melamine and diphenyl phosphite in a molar ratio of 1:4 to 8 in a CCl4 solvent to obtain a melamine CCl4 solution and a diphenyl phosphite CCl4 solution, respectively;
[0008] (2) placing the melamine CCl4 solution in an ice bath, adding 20% of the total mass of the solution NaOH solution and 1% of the total mass of the solution benzyltriethylammonium chloride, and mixing well;
[0009] (3) slowly adding diphenyl phosphite CCl4 solution to the solution obtained in step (2) with continuous stirring for 1 hour;
[0010] (4) heating to 15-30°C for 4 hours, washing with water, standing for stratification, removing the water layer, distilling under reduced pressure, recovering the CCl4 solvent, and obtaining melamine diphenyl phosphite, the structural formula of which is as follows:
[0011]
[0012] With the triazine ring of melamine as the center, three amine groups are respectively connected to a diphenyl phosphite group to form melamine diphenyl phosphite containing multiple nitrogen and phosphorus elements.
[0013] The reaction equation of the preparation process of melamine diphenyl phosphite is:
[0014]
[0015] The reaction is achieved by the Atherton-Todd method. First, the phosphorus-hydrogen bond of the phosphite diester is broken under alkaline conditions, and the formed phosphite diester anion attacks carbon tetrachloride to obtain a chlorine atom to form an acyl chloride phosphite diester intermediate, converting the PH bond into a P-Cl bond. Since the acyl chloride phosphite diester is too active, it will then react with alcohols or amines to synthesize phosphates or phosphoramides.
[0016]
[0017]
[0018] Since the triazine ring of melamine has three amine groups with high reaction activity, they can be combined with diphenyl phosphite respectively by controlling the ratio of reactants and reaction conditions to obtain the above-mentioned melamine diphenyl phosphite.
[0019] The present invention also provides a method for preparing phosphorus-nitrogen synergistic structural flame-retardant PET, wherein the raw material ratio is as follows by weight:
[0020] Terephthalic acid (or dimethyl terephthalate, or a mixture of the two in any proportion) 100 parts
[0021] Ethylene glycol 50-500 parts
[0022] 2-5 parts of melamine diphenyl phosphite
[0023] Catalyst 0.2~0.5 parts
[0024] (a) stirring and dissolving melamine diphenyl phosphite and ethylene glycol accounting for 5 to 20 wt % of the total amount of ethylene glycol at a temperature of 60 to 100° C., and then dispersing by ultrasonic vibration to prepare a melamine diphenyl phosphite-ethylene glycol solution;
[0025] (b) mixing terephthalic acid, the remaining ethylene glycol and the catalyst for esterification reaction at a temperature of 235 to 250° C., a pressure of 0.25 to 0.3 MPa and a time of 2 to 4 hours;
[0026] (c) heating the product obtained in step (b) to 250-280° C. and reducing the pressure to 6000-10000 Pa to perform a pre-polycondensation reaction for 45-60 min;
[0027] (d) adding the melamine phenyl phosphite-ethylene glycol solution of step (a) to the product obtained in step (c), adjusting the vacuum degree to ≤70 Pa, and continuing the reaction for 1 to 4 hours to obtain phosphorus-nitrogen synergistic structural flame-retardant PET.
[0028] Wherein, terephthalic acid can also be replaced by dimethyl terephthalate, or the two can be mixed in any proportion; the catalyst is antimony oxide or ethylene glycol antimony.
[0029]
[0030] The mechanism of melamine diphenyl phosphite participating in the PET polycondensation reaction is shown in the above formula. The present invention first uses the Atherton-Todd reaction to open the phosphorus-hydrogen bond in diphenyl phosphite, so that it reacts with the primary amine group of melamine to synthesize melamine diphenyl phosphite; and then further adds melamine diphenyl phosphite to the PET polycondensation reaction, wherein the phosphite group undergoes an ester exchange reaction with the terminal hydroxyl group of the PET prepolymer, and is connected to the PET molecular chain, playing the role of a phosphorus-nitrogen synergistic structural flame retardant. At the same time, because it has multiple phosphite groups, it can play the role of a chain extender during PET polycondensation, thereby improving the molecular weight and crystallization performance of PET.
[0031] In summary, the present invention has the following beneficial effects:
[0032] 1. The present invention synthesizes a novel nitrogen-phosphorus synergistic structural flame retardant from melamine and diphenyl phosphite, grafts melamine and diphenyl phosphite onto the molecular chain of PET, connects them with covalent bonds, and realizes nitrogen-phosphorus synergistic flame retardancy at the molecular level, and will not cause the flame retardancy of the product to decrease over time.
[0033] 2. The phosphorus-nitrogen synergistic structural flame-retardant PET prepared by the present invention introduces phosphorus-nitrogen flame-retardant elements into the PET molecular chain through chemical bonds, and has good thermal stability and processing performance. In addition, phenyl phosphite also has good antioxidant and chain-extending effects on PET. As an esterification promoter, it makes the PET molecular chain grow and produces a cross-linked structure, thereby improving its mechanical properties such as tensile strength and impact strength. DETAILED DESCRIPTION
[0034] The following embodiments may enable those skilled in the art to better understand the present invention, but are not intended to limit the present invention in any form.
[0035] Example 1
[0036] Preparation of melamine diphenyl phosphite
[0037] (1) dissolving melamine and diphenyl phosphite in a CCl4 solvent in a molar ratio of 1:6, respectively, to obtain a melamine CCl4 solution and a diphenyl phosphite CCl4 solution, respectively;
[0038] (2) placing the melamine CCl4 solution in an ice bath, adding 20% of the total mass of the solution NaOH solution and 1% of the total mass of the solution benzyltriethylammonium chloride, and mixing well;
[0039] (3) slowly adding diphenyl phosphite CCl4 solution to the solution obtained in step (2) with continuous stirring for 1 hour;
[0040] (4) heating to 20° C. to react for 4 h, washing with water, allowing to stand for stratification, removing the water layer, and performing vacuum distillation to recover the CCl4 solvent to obtain melamine diphenyl phosphite.
[0041] Example 2
[0042] Preparation of phosphorus-nitrogen synergistic structural flame-retardant PET
[0043] The raw material ratio is as follows:
[0044]
[0045]
[0046] (a) at a temperature of 85° C., stirring and dissolving melamine diphenyl phosphite and ethylene glycol accounting for 10 wt % of the total amount of ethylene glycol, and then dispersing by ultrasonic oscillation to prepare a melamine diphenyl phosphite-ethylene glycol solution;
[0047] (b) mixing the remaining ethylene glycol of terephthalic acid with the catalyst for esterification reaction at a temperature of 240° C., a pressure of 0.3 MPa, and a time of 3 h;
[0048] (c) heating the product obtained in step (b) to 280° C. and reducing the pressure to 10000 Pa to perform a pre-polycondensation reaction for 60 min;
[0049] (d) adding the melamine diphenyl phosphite-ethylene glycol solution obtained in step (a) to the product obtained in step (c), adjusting the vacuum degree to ≤70 Pa, and continuing the reaction for 2 hours to obtain phosphorus-nitrogen synergistic structural flame-retardant PET.
[0050] Example 3
[0051] Preparation of phosphorus-nitrogen synergistic structural flame-retardant PET
[0052] The raw material ratio is as follows:
[0053]
[0054] (a) at a temperature of 80° C., melamine diphenyl phosphite and ethylene glycol accounting for 15 wt % of the total amount of ethylene glycol are stirred and dissolved, and then ultrasonically dispersed to prepare a melamine diphenyl phosphite-ethylene glycol solution;
[0055] (b) mixing the remaining ethylene glycol of terephthalic acid with the catalyst for esterification reaction at a temperature of 245° C., a pressure of 0.28 MPa, and a time of 2.5 h;
[0056] (c) heating the product obtained in step (b) to 260° C. and reducing the pressure to 8000 Pa to perform a pre-polycondensation reaction for 50 min;
[0057] (d) adding the melamine diphenyl phosphite-ethylene glycol solution obtained in step (a) to the product obtained in step (c), adjusting the vacuum degree to ≤70 Pa, and continuing the reaction for 3 hours to obtain phosphorus-nitrogen synergistic structural flame-retardant PET.
[0058] Example 4
[0059] Preparation of phosphorus-nitrogen synergistic structural flame-retardant PET
[0060] The raw material ratio is as follows:
[0061]
[0062] (a) at a temperature of 85° C., stirring and dissolving melamine diphenyl phosphite and ethylene glycol accounting for 12 wt % of the total amount of ethylene glycol, and then dispersing by ultrasonic oscillation to prepare a melamine diphenyl phosphite-ethylene glycol solution;
[0063] (b) mixing the remaining ethylene glycol of terephthalic acid with the catalyst for esterification reaction at a temperature of 235° C., a pressure of 0.25 MPa, and a time of 3.5 h;
[0064] (c) heating the product obtained in step (b) to 280° C. and reducing the pressure to 6000 Pa to carry out a pre-polycondensation reaction for 45 min;
[0065] (d) adding the melamine diphenyl phosphite-ethylene glycol solution obtained in step (a) to the product obtained in step (c), adjusting the vacuum degree to ≤70 Pa, and continuing the reaction for 3.5 hours to obtain phosphorus-nitrogen synergistic structural flame-retardant PET.
[0066] Comparative Example 1
[0067] The raw material ratio is as follows:
[0068] 100 parts of terephthalic acid
[0069] 100 parts of ethylene glycol
[0070] Catalyst (Sb2O3) 0.5 parts
[0071] Terephthalic acid, ethylene glycol and a catalyst were mixed and esterified at 250°C and 0.3 MPa for 3 hours; a pre-polycondensation reaction was carried out at 260°C and 10000 Pa for 1 hour; the condensation reaction was continued for 3 hours while maintaining 260°C and vacuuming until the pressure was less than 70 Pa to complete the polycondensation reaction and obtain PET material.
[0072] Table 1 Mechanical properties and flame retardant properties of PET materials
[0073]
[0074] It can be seen from Table 1 that compared with Comparative Example 1, the limiting oxygen index and anti-combustion performance of PET prepared by adding melamine phenyl phosphite flame retardant in Examples 2-4 are significantly improved, reaching the UL-94 test V0 level, indicating that the phosphorus-nitrogen synergistic structural flame retardant can effectively improve the flame retardant effect of PET materials. At the same time, the PET material compounded with melamine diphenyl phosphite has a significant improvement in tensile strength and impact strength. This is because the polyphosphate group in the structure of the structural flame retardant plays a role in chain extension and cross-linking of the PET molecular chain segments, the molecular crystallinity is improved, and the mechanical strength is enhanced.
[0075] The above embodiments of the present invention are merely examples for clearly illustrating the present invention, and are not intended to limit the embodiments of the present invention. Those skilled in the art should understand that the above specific descriptions are illustrative rather than restrictive, and should not be used to limit the scope of protection of the present invention.
Claims
1. A phosphorus-nitrogen synergistic structural flame-retardant PET, It is characterized in that It is prepared from the following raw materials by weight Terephthalic acid, dimethyl terephthalate 100 parts Ethylene glycol 50~500 parts 2-5 parts of melamine diphenyl phosphite Catalyst 0.2~0.5 parts The preparation method of described melamine diphenyl phosphite is as follows: (1) Dissolve melamine and diphenyl phosphite in CCl 4 Solvent, respectively, to obtain melamine CCl 4 Solution and diphenyl phosphite CCl 4 Solution; (2) Melamine CCl 4 The solution was placed in an ice bath, and NaOH solution and benzyltriethylammonium chloride were added and mixed well; (3) Slowly add diphenyl phosphite CCl to the solution obtained in step (2) under stirring. 4 Solution; (4) Heat to 15-30℃ and react for 4h, wash with water, let stand to separate layers, remove the water layer, and perform vacuum distillation to recover CCl 4 Solvent to obtain melamine diphenyl phosphite.
2. The phosphorus-nitrogen synergistic structural flame-retardant PET according to claim 1, It is characterized in that In step (1), the molar ratio of melamine to diphenyl phosphite is 1:4-8.
3. The phosphorus-nitrogen synergistic structural flame-retardant PET according to claim 1, It is characterized in that In step (2), the amount of NaOH solution added is melamine CCl 4 20% of the total mass of the solution, the amount of benzyltriethylammonium chloride added is melamine CCl 4 1% of the total mass of the solution.
4. The phosphorus-nitrogen synergistic structural flame-retardant PET according to claim 1, It is characterized in that The catalyst is antimony oxide or antimony glycol.
5. The phosphorus-nitrogen synergistic structural flame-retardant PET according to claim 1, It is characterized in that The terephthalic acid and dimethyl terephthalate are mixed in any proportion.
6. A method for preparing the phosphorus-nitrogen synergistic structural flame-retardant PET according to any one of claims 1 to 5, It is characterized in that The following steps are involved: (a) stirring and dissolving melamine diphenyl phosphite and part of ethylene glycol at a temperature of 60-100° C., and then dispersing them by ultrasonic vibration to prepare a melamine diphenyl phosphite-ethylene glycol solution; (b) mixing terephthalic acid, the remaining ethylene glycol and the catalyst for esterification reaction at a temperature of 235-250°C, a pressure of 0.25-0.3 MPa and a time of 2-4 hours; (c) heating the product obtained in step (b) to 250-280° C. and reducing the pressure to 6000-10000 Pa to perform a pre-polycondensation reaction for 45-60 min; (d) adding the melamine phenyl phosphite-ethylene glycol solution described in step (a) to the product obtained in step (c), and continuing the reaction for 1 to 4 hours to obtain phosphorus-nitrogen synergistic structural flame-retardant PET.
7. The method for preparing the phosphorus-nitrogen synergistic structural flame-retardant PET according to claim 6, It is characterized in that In step (b), the amount of ethylene glycol added is 5-20wt% of the total amount of ethylene glycol.
8. The method for preparing the phosphorus-nitrogen synergistic structural flame-retardant PET according to claim 6, It is characterized in that In step (d), the reaction vacuum is adjusted to ≤70Pa.
Citation Information
Patent Citations
Hexaphenyl phosphate ester melamine salt fire retardant and method for preparing same
CN102190814A
Compound flame-retardant polyethylene glycol terephthalate system and preparation method thereof
CN105924911A
Phosphorus-nitrogen-containing flame-retardant polyester and preparation method thereof
CN111533894A
Flame retardant poly(trimethylene terephthalate) composition
US20110172329A1
Cited By
Cable filling flame-retardant composite fiber paper rope
CN120636934A
A type of cable filled with flame-retardant composite fiber paper rope
CN120636934B