Resveratrol-loaded microsphere mixed biological material as well as preparation method and application thereof

By using composite microsphere biomaterials loaded with resveratrol and mixing mesoporous silica with biphasic calcium phosphate, the degradation rate of the scaffold and osteoinduction effect were regulated, thus solving the problem of insufficient drug release of resveratrol in the treatment of periodontitis and achieving a long-term therapeutic effect for periodontitis.

CN118892557APending Publication Date: 2024-11-05KUNMING HOSPITAL OF TRADITIONAL CHINESE MEDICINE +1
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410927517.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-11
Publication Date
2024-11-05

AI Technical Summary

Technical Problem

In the existing technology, resveratrol has poor drug release kinetics in the treatment of periodontitis, resulting in low effective utilization rate. In addition, the mesoporous silica loading capacity is limited, which cannot effectively repair alveolar bone and affect the treatment effect.

Method used

By using resveratrol-loaded composite microsphere biomaterials, and mixing mesoporous silica with biphasic calcium phosphate, the degradation rate and osteoinduction effect of the scaffold are regulated, and a scaffold is prepared to improve the therapeutic effect.

Benefits of technology

With a limited number of implantable scaffolds, the scaffolds possess a moderate degradation rate and the ability to promote bone tissue growth, achieving the goal of long-term treatment of periodontitis and improving treatment outcomes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118892557A_ABST
    Figure CN118892557A_ABST
Patent Text Reader

Abstract

The invention relates to a resveratrol-loaded microsphere mixed biological material as well as a preparation method and application thereof, and belongs to the field of medical biological materials. The preparation method comprises the following steps: (1) preparing polystyrene microspheres; (2) preparation of mesoporous silica microspheres with cavity structures; (3) loading resveratrol on the mesoporous silica microspheres with the cavity structures; and (4) preparation of a microsphere mixed biological material: preparing a biological material formed by mixing the resveratrol-loaded cavity structure silicon dioxide microspheres and biphase calcium phosphate, and preparing the mixed biological material into a stent to be applied to periodontitis treatment, so that the treatment effect of the stent on periodontitis is improved under the condition that the number of implanted stents is limited.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of medical biomaterials, and relates to a microsphere mixed biomaterial loaded with resveratrol, and a preparation method and application thereof. Background Art

[0002] Periodontitis is the sixth most common health problem in the world, affecting 11% of the world's population. Its main manifestations are gingival inflammation, periodontal pocket formation, alveolar bone resorption, loose and displaced teeth, and it is the main cause of tooth loss in adults. At the same time, alveolar bone resorption can lead to alveolar bone defects. Due to insufficient bone mass, teeth can easily become loose and fall off, which will not only cause facial deformities in patients, but also affect the body's chewing, breathing, language and other functions, and will have adverse effects on patients both physiologically and psychologically. Most of the commonly used periodontitis treatments in clinical practice are currently designed to eliminate periodontal microorganisms, such as periodontal drug therapy, basic periodontal treatment and periodontal surgical treatment. However, due to the abuse and resistance of antibiotics, few surgical indications and long treatment cycles, patients are unable to persist in maintenance, resulting in unsatisfactory treatment effects for periodontitis.

[0003] In order to avoid adverse reactions caused by systemic medication, the treatment of periodontitis focuses on removing local irritants by implanting stents in the affected area, promoting the repair and regeneration of bone tissue on the basis of eliminating inflammation. Since only a single stent is usually implanted in the affected area for periodontitis treatment, the therapeutic effect of the stent material directly determines its therapeutic effect on periodontitis. Therefore, when the stent has anti-inflammatory and bone repair effects, its therapeutic effect on periodontitis will be significantly improved. Resveratrol has anti-inflammatory and bone-promoting effects, but its drug release kinetics are poor, it is difficult to dissolve in water, and its metabolic performance is poor, resulting in a low effective utilization rate of resveratrol in the treatment of periodontitis, limited therapeutic effect, and inability to maintain long-term stable therapeutic effects, which limits its promotion and application in the treatment of periodontitis. By utilizing the drug-loading properties of mesoporous silica, resveratrol can be loaded onto mesoporous silica to alleviate the problem of resveratrol burst release. However, the osteogenic effect of resveratrol is relatively weak, and the resveratrol loading capacity of mesoporous silica is relatively limited. As a result, when it is made into a scaffold and the number of implanted scaffolds is limited, it cannot effectively repair the alveolar bone, affecting its therapeutic effect on periodontitis.

[0004] Therefore, it is necessary to provide a composite microsphere biomaterial loaded with resveratrol and a preparation method and application thereof, so as to enhance the repair effect of the stent on the alveolar bone and improve the therapeutic effect of the stent on periodontitis when the number of implanted stents is limited. Summary of the invention

[0005] In order to overcome the problems in the background technology, the present invention provides a composite microsphere biomaterial loaded with resveratrol on the one hand, by utilizing the adjustable degradation rate of biphasic calcium phosphate and the effect of bone induction, on the one hand, it is mixed with the cavity structure mesoporous silica loaded with resveratrol to make a scaffold, which can adjust the degradation rate of the entire scaffold so that the overall degradation rate of the scaffold is at an appropriate level, and on the other hand, it can make up for the weaker effect of resveratrol in promoting bone tissue growth, so that the scaffold has a more comprehensive therapeutic effect when the quantity is limited, and improves the therapeutic effect of the scaffold made of the composite microsphere biomaterial on periodontitis. Another invention of the present invention provides a method for preparing a composite microsphere biomaterial loaded with resveratrol, so as to prepare a composite microsphere biomaterial mixed with cavity structure mesoporous silica loaded with resveratrol and biphasic calcium phosphate, and the aforementioned biomaterial is made into a scaffold for the treatment of periodontitis.

[0006] In order to achieve the above object, the present invention is implemented by the following technical solutions:

[0007] The composite microsphere biomaterial uses mesoporous silica as a shell to form microspheres with a cavity structure, and resveratrol is loaded on the microspheres, and biphasic calcium phosphate is mixed to form the composite microsphere biomaterial.

[0008] The preparation method comprises the following steps:

[0009] (1) Preparation of polystyrene microspheres (PS): 1.42 g of polyvinyl pyrrolidone (PVP) was dissolved in 400 ml of deionized water, and then 80 g of styrene monomer was added to the solution. The solution was stirred and nitrogen was continuously introduced, and then heated in an oil bath. After the solution was heated to a certain temperature and stabilized by heat, 1.2 g of 2,2-azobis(2-methylpropylimidamide) dihydrochloride was added to the solution. After emulsification for a certain period of time, the solution was washed with deionized water and anhydrous ethanol respectively, and then centrifuged and dried to obtain polystyrene microspheres.

[0010] (2) Preparation of hollow structure mesoporous silica microspheres: 1 g of the polystyrene microspheres prepared in step (1) was added to deionized water containing 16 ml of triethanolamine (TEOA) and 0.7 g of hexadecyltrimethylammonium bromide (CATB) for ultrasonic dispersion, and then 140-180 μl of tetraethyl orthosilicate (TEOS) was added for reaction. After the reaction, the microspheres were washed with deionized water and anhydrous ethanol respectively, and then centrifuged to obtain the product, which was then calcined to obtain hollow structure mesoporous silica microspheres.

[0011] (3) Hollow structure mesoporous silica microspheres (MSNs) loaded with resveratrol (Res): 10 mg of the hollow structure mesoporous silica microspheres prepared in step (2) are ultrasonically dispersed in anhydrous ethanol, and resveratrol is added. After constant temperature and light-proof oscillation in a water bath shaker, the complex solution is poured out, washed with ultrapure water and anhydrous ethanol respectively, and dried in an oven. After drying, hollow structure mesoporous silica microspheres loaded with resveratrol are obtained, and the amount of resveratrol added is sufficient to add 1 to 5 mg of resveratrol per milliliter of anhydrous ethanol.

[0012] (4) Preparation of mixed biomaterials: The resveratrol-loaded hollow structure mesoporous silica microspheres obtained in step (3) are mixed with biphasic calcium phosphate (BCP) at a mass ratio of 1:10 for the hollow structure mesoporous silica microspheres loaded with resveratrol: biphasic calcium phosphate, and after uniform mixing, a mixed biomaterial of the resveratrol-loaded hollow structure mesoporous silica microspheres and biphasic calcium phosphate is obtained.

[0013] Preferably, in step (1), the oil bath is heated to 90° C. and the emulsification time is 24 hours.

[0014] Preferably, in step (1), the stirring and continuous nitrogen introduction time is 30 minutes.

[0015] Preferably, in step (2), the reaction time after adding tetraethyl orthosilicate is 2 hours.

[0016] Preferably, during the calcination of the product of step (2), the temperature is raised to 550°C at a rate of 5°C / min, and the product is calcined at 550°C for 4h to 4.5h.

[0017] Preferably, the constant temperature and light-proof oscillation temperature in step (3) is 36.5° C. to 37° C., and the oscillation time is 48 h.

[0018] Preferably, in step (3), the drying temperature is 40-50° C. and the drying time is 20-24 hours.

[0019] The prepared resveratrol-loaded composite microsphere biomaterial is used to make a scaffold for the treatment of periodontitis.

[0020] Beneficial effects of the present invention:

[0021] 1. The present invention utilizes biphasic calcium phosphate to adjust the calcium-phosphorus ratio to regulate the crystal microphase structure, thereby achieving the characteristic of adjustable degradation rate, and is mixed with the cavity structure mesoporous silica loaded with resveratrol to adjust the overall degradation rate of the scaffold made of the composite microsphere biomaterial, so that the scaffold has a more moderate degradation rate during the treatment process, thereby improving the therapeutic effect of the scaffold on periodontitis.

[0022] 2. The present invention utilizes the bone-inducing effect of biphasic calcium phosphate to promote bone tissue growth and repair alveolar bone defects during the treatment of periodontitis, thereby compensating for the weak bone-promoting effect of resveratrol. When the number of implanted stents is limited, the stents are provided with more comprehensive functions, thereby improving the therapeutic effect of the stents made of composite microspheres on periodontitis.

[0023] 3. The present invention increases the specific surface area of ​​mesoporous silica microspheres by preparing mesoporous silica with a cavity structure. At the same time, the mesoporous silica cavity can also be loaded with resveratrol. Therefore, when the implanted stent is limited, the loading amount of resveratrol in the mesoporous silica with a cavity structure in each stent is effectively increased, further improving the therapeutic effect of the stent on periodontitis.

[0024] 4. The present invention adopts in-situ polymerization of polystyrene microspheres to prepare cavity structure mesoporous silica microspheres, with high yield and uniform particle size distribution.

[0025] 5. The present invention loads resveratrol through cavity-structured mesoporous silica, so that resveratrol can be slowly released through the sustained-release effect of mesoporous silica, so as to achieve the purpose of long-term treatment of periodontitis. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 It is a process flow chart of the preparation method of the present invention.

[0027] Figure 2 These are the TEM images of the cavity mesoporous silica and the SEM morphology images of the mixed biomaterials prepared in the present invention, wherein Figure A is the TEM image of the cavity mesoporous silica, and Figure B is the SEM morphology image of the mixed biomaterial.

[0028] Figure 3 This is a Fourier infrared spectrum analysis diagram of the stent made of the mixed biomaterial of the present invention.

[0029] Figure 4 This is an X-ray diffraction analysis diagram of the stent made of the mixed biomaterial of the present invention.

[0030] Figure 5 This is a degradation performance analysis diagram of the scaffold made of the mixed biomaterial of the present invention, the scaffold made of BCP single material, and the scaffold made of MSNs single material.

[0031] Figure 6 This is an analysis diagram of the sustained-release performance of drugs in a stent made of the mixed biomaterial of the present invention.

[0032] Figure 7Figures showing cell adhesion experiments on scaffolds made of mixed biomaterials of the present invention, wherein (A) is a figure showing cell adhesion experiments on a scaffold supported by mixed biomaterials in Example 1; (B) is a figure showing cell adhesion experiments on a scaffold supported by mixed biomaterials in Example 2; (C) is a figure showing cell adhesion experiments on a scaffold supported by mixed biomaterials in Example 3; (D) is a figure showing cell adhesion experiments on a scaffold supported by mixed biomaterials in Example 4; and (E) is a figure showing cell adhesion experiments on a scaffold supported by mixed biomaterials in Example 5. DETAILED DESCRIPTION

[0033] The present invention is further described in detail below in conjunction with specific embodiments.

[0034] In the examples of the present invention, chemical reagents not otherwise specified were all commercially available analytically pure for the experiments.

[0035] Example 1

[0036] In this example, the resveratrol-loaded microsphere mixed biomaterial is prepared by the following steps:

[0037] (1) Preparation of PS microspheres: Using a 500 ml round-bottom flask, 1.42 g of PVP was dissolved in 400 ml of deionized water, and then 80 g of styrene monomer was added to the solution. The mixture was stirred and nitrogen was continuously introduced for 30 min. The mixture was then heated in an oil bath to 90 °C. After the solution was thermally stabilized, 1.2 g of 2,2-azobis(2-methylpropylimidamide) dihydrochloride was added to the solution. After emulsification for 24 h, the solution was first washed with deionized water and then with anhydrous ethanol. The PS microspheres were then obtained by centrifugation and drying.

[0038] (2) Preparation of hollow structure mesoporous silica microspheres (MSNs): 1g PS microspheres were added to deionized water containing 16ml TEOA and 0.7g CATB for ultrasonic dispersion, and then 140μl TEOS was added for 2h. After the reaction, the microspheres were washed with deionized water and then with anhydrous ethanol, and then centrifuged to obtain the product. The product was placed in a calcination furnace, heated at a rate of 5℃ / min, and calcined at 550℃ for 4h to obtain hollow structure mesoporous silica microspheres (MSNs). Transmission electron microscopy experiments were performed on the obtained hollow structure mesoporous silica microspheres, and the TEM image was as follows: Figure 2 As shown in A.

[0039] (3) MSNs loaded with Res: 10 mg of MSNs were ultrasonically dispersed in anhydrous ethanol, and Res was added. After constant temperature and light-proof oscillation at 37°C in a water bath shaker for 48 h, the complex solution was poured out, washed three times with ultrapure water, and then washed three times with anhydrous ethanol. The complex solution was placed in an oven for drying at 40°C for 24 h. After drying, Res-loaded MSNs were obtained. The amount of resveratrol added was 5 mg per ml of anhydrous ethanol.

[0040] (4) Preparation of mixed biomaterial: The Res-loaded MSNs obtained in step (3) and BCP were mixed in a mass ratio of resveratrol-loaded hollow structure mesoporous silica microspheres: biphasic calcium phosphate = 1:10, and after mixing evenly, a mixed biomaterial of resveratrol-loaded hollow structure mesoporous silica microspheres and biphasic calcium phosphate was obtained. The mixed biomaterial prepared in this example was subjected to a scanning electron microscopy experiment, and the results were as follows: Figure 2 As shown in B.

[0041] The mixed biomaterial prepared in this example was used as a raw material to make an implant stent, and the stent was analyzed by Fourier transform infrared spectroscopy. The results are as follows: Figure 3 shown.

[0042] The mixed biomaterial prepared in this example was used as a raw material to make an implant stent, and an X-ray diffraction experiment was performed on the stent. The results are as follows: Figure 4 shown.

[0043] The mixed biomaterial prepared in this example was used as a raw material to make an implant stent, and a 30-day degradation experiment was performed on the stent to measure its degradation performance. The results are as follows: Figure 5 shown.

[0044] The mixed biomaterial prepared in this example was used as a raw material to make an implant stent, and the drug release performance of the stent was tested. The results are as follows: Figure 6 shown.

[0045] The mixed biomaterial prepared in this example was used as a raw material to make an implant scaffold, and a cell adhesion experiment was performed on the scaffold. The results are as follows: Figure 7 shown.

[0046] Example 2

[0047] In this example, the resveratrol-loaded microsphere mixed biomaterial is prepared by the following steps:

[0048] (1) Preparation of PS microspheres: Using a 500 ml round-bottom flask, 1.42 g of PVP was dissolved in 400 ml of deionized water, and then 80 g of styrene monomer was added to the solution. The mixture was stirred and nitrogen was continuously introduced for 30 min. The mixture was then heated in an oil bath to 90 °C. After the solution was thermally stabilized, 1.2 g of 2,2-azobis(2-methylpropylimidamide) dihydrochloride was added to the solution. After emulsification for 24 h, the solution was first washed with deionized water and then with anhydrous ethanol. The PS microspheres were then obtained by centrifugation and drying.

[0049] (2) Preparation of hollow structure mesoporous silica microspheres (MSNs): 1 g of PS microspheres was added to deionized water containing 16 ml of TEOA and 0.7 g of CATB for ultrasonic dispersion, and then 160 μl of TEOS was added to react for 2 h. After the reaction, the microspheres were washed with deionized water and then with anhydrous ethanol, and then centrifuged to obtain the product. The product was placed in a calcination furnace, heated at a rate of 5 °C / min, and calcined at 550 °C for 4.2 h to obtain hollow structure mesoporous silica microspheres (MSNs).

[0050] (3) MSNs loaded with Res: 10 mg of MSNs were ultrasonically dispersed in anhydrous ethanol, and Res was added. After constant temperature and light-proof oscillation at 36.8°C in a water bath shaker for 48 h, the complex solution was poured out, washed three times with ultrapure water, and then washed three times with anhydrous ethanol. The complex solution was placed in an oven for drying at 45°C for 22 h. After drying, Res-loaded MSNs were obtained. The amount of resveratrol added was 4 mg per ml of anhydrous ethanol.

[0051] (4) Preparation of mixed biomaterials: The Res-loaded MSNs obtained in step (3) are mixed with BCP in a mass ratio of resveratrol-loaded hollow structure mesoporous silica microspheres: biphasic calcium phosphate = 1:10, and after uniform mixing, a mixed biomaterial of resveratrol-loaded hollow structure mesoporous silica microspheres and biphasic calcium phosphate is obtained.

[0052] The mixed biomaterial prepared in this example was used as a raw material to make an implant stent, and the drug release performance of the stent was tested. The results are as follows: Figure 6 shown.

[0053] The mixed biomaterial prepared in this example was used as a raw material to make an implant scaffold, and a cell adhesion experiment was performed on the scaffold. The results are as follows: Figure 7 shown.

[0054] Other properties of the mixed biomaterial prepared in this example are similar to those of the mixed biomaterial prepared in Example 1.

[0055] Example 3

[0056] In this example, the resveratrol-loaded microsphere mixed biomaterial is prepared by the following steps:

[0057] (1) Preparation of PS microspheres: Using a 500 ml round-bottom flask, 1.42 g of PVP was dissolved in 400 ml of deionized water, and then 80 g of styrene monomer was added to the solution. The mixture was stirred and nitrogen was continuously introduced for 30 min. The mixture was then heated in an oil bath to 90 °C. After the solution was thermally stabilized, 1.2 g of 2,2-azobis(2-methylpropylimidamide) dihydrochloride was added to the solution. After emulsification for 24 h, the solution was first washed with deionized water and then with anhydrous ethanol. The PS microspheres were then obtained by centrifugation and drying.

[0058] (2) Preparation of hollow structure mesoporous silica microspheres (MSNs): 1 g of PS microspheres was added to deionized water containing 16 ml of TEOA and 0.7 g of CATB for ultrasonic dispersion, and then 180 μl of TEOS was added to react for 2 h. After the reaction, the microspheres were washed with deionized water and then with anhydrous ethanol, and then centrifuged to obtain the product. The product was placed in a calcination furnace, heated at a rate of 5 °C / min, and calcined at 550 °C for 4.5 h to obtain hollow structure mesoporous silica microspheres (MSNs).

[0059] (3) MSNs loaded with Res: 10 mg of MSNs were ultrasonically dispersed in anhydrous ethanol, and Res was added. After constant temperature and light-proof oscillation at 36.5°C in a water bath shaker for 48 h, the complex solution was poured out, washed three times with ultrapure water, and then washed three times with anhydrous ethanol. The complex solution was placed in an oven for drying at 50°C for 20 h. After drying, Res-loaded MSNs were obtained. The amount of resveratrol added was 3 mg per ml of anhydrous ethanol.

[0060] (4) Preparation of mixed biomaterials: The Res-loaded MSNs obtained in step (3) are mixed with BCP in a mass ratio of resveratrol-loaded hollow structure mesoporous silica microspheres: biphasic calcium phosphate = 1:10, and after uniform mixing, a mixed biomaterial of resveratrol-loaded hollow structure mesoporous silica microspheres and biphasic calcium phosphate is obtained.

[0061] The mixed biomaterial prepared in this example was used as a raw material to make an implant stent, and the drug release performance of the stent was tested. The results are as follows: Figure 6 shown.

[0062] The mixed biomaterial prepared in this example was used as a raw material to make an implant scaffold, and a cell adhesion experiment was performed on the scaffold. The results are as follows: Figure 7 shown.

[0063] Other properties of the mixed biomaterial prepared in this example are similar to those of the mixed biomaterial prepared in Example 1.

[0064] Example 4

[0065] This example adopts the same method as that of Example 1 to prepare the composite microsphere biomaterial, except that in this example, the amount of resveratrol added is 2 mg per milliliter of anhydrous ethanol.

[0066] The mixed biomaterial prepared in this example was used as a raw material to make an implant stent, and the drug release performance of the stent was tested. The results are as follows: Figure 6 shown.

[0067] The mixed biomaterial prepared in this example was used as a raw material to make an implant scaffold, and a cell adhesion experiment was performed on the scaffold. The results are as follows: Figure 7 shown.

[0068] Other properties of the mixed biomaterial prepared in this example are similar to those of the mixed biomaterial prepared in Example 1.

[0069] Example 5

[0070] This example adopts the same method as that of Example 1 to prepare the composite microsphere biomaterial, except that in this example, the amount of resveratrol added is 1 mg per milliliter of anhydrous ethanol.

[0071] The mixed biomaterial prepared in this example was used as a raw material to make an implant stent, and the drug release performance of the stent was tested. The results are as follows: Figure 6 shown.

[0072] The mixed biomaterial prepared in this example was used as a raw material to make an implant scaffold, and a cell adhesion experiment was performed on the scaffold. The results are as follows: Figure 7 shown.

[0073] Other properties of the mixed biomaterial prepared in this example are similar to those of the mixed biomaterial prepared in Example 1.

[0074] pass Figure 2 It can be seen that MSNs and the mixed biomaterials finally prepared by the present invention have excellent dispersibility. When the mixed biomaterials prepared by the present invention are used to make scaffolds and implanted in the affected area, they can better provide the elements required for osteogenesis and achieve excellent drug release effects in terms of drug administration.

[0075] The specific surface area of ​​the cavity structure mesoporous silica prepared in Example 1 of the present invention was tested and found to be 1232 m 2 / g, and the pore size is about 4nm. The ultra-small mesopore size and large specific surface area indicate that the preparation method of the present invention can successfully obtain cavity-structured mesoporous silica particles, providing an ideal carrier for subsequent drug loading.

[0076] pass Figure 3 It can be seen that 1000cm -1 Nearby is PO4 3- Stretching vibration peak, 3400cm -1 The stretching vibration peak of -OH is 560-640cm -1 The peak of -OH bending vibration can prove the presence of hydroxyapatite (HA) and β-tricalcium phosphate (β-TCP) in the mixed biomaterial prepared by the present invention. -1 The peak at 1675 cm is caused by the introduction of aromatic hydrocarbons from resveratrol. -1 The peak at 1500cm is the bending vibration peak of C=O. -1 The absorption peak of Si-O is shown in FIG. 4 , which indicates that the mixed biomaterial of cavity-structured mesoporous silica and biphasic calcium phosphate loaded with resveratrol can be successfully prepared by the method of the present invention, and the two substances in the mixed material will not have a negative impact on each other.

[0077] pass Figure 4 It can be seen that on the PDF standard card of hydroxyapatite (HA#09-0432), there are three characteristic peaks at 2θ angles of 31.75°, 32.18°, and 32.98°, which are the three strongest peaks of HA. On the PDF standard card of β-tricalcium phosphate (β-TCP#09-0169), there are three characteristic peaks at 2θ angles of 30.96°, 34.12°, and 46.79°, which are the three strongest peaks of β-TCP. On the PDF standard card of silicon dioxide (SiO2#45-1374), there are three characteristic peaks at 2θ angles of 30.22°, 40.10°, and 45.81°, which are the three strongest peaks of SiO2. It shows that the HA, β-TCP and silicon dioxide prepared by the method of the present invention are three-phase powder composite materials, and the three-phase composite will not destroy the respective crystal phase structures.

[0078] pass Figure 5It can be seen that the degradation rate of MSNs is the slowest. This is because MSNs are slowly decomposed into small molecules of silica in a weakly alkaline environment in simulated body fluids. These silicas will be deposited on the surface of MSNs that are not in contact with simulated body fluids, so that the degradation rate of MSNs tends to be flat in the later stage. Since there are two phases in BCP, the degradation rate of HA is slow and the degradation rate of β-TCP is faster. The ratio of the two in BCP is β-TCP: HA = 3:7. At about 12 days, the calcium ions in HA are slowly deposited on the surface of the BCP scaffold, making the deposition rate greater than the degradation rate. At about 20 days, the deposition rate is also greater than the degradation rate due to the deposition of silica and calcium ions. The degradation rate of the scaffold made of the mixed biomaterial prepared by the present invention is between BCP and MSNs, so that the degradation rate of the scaffold is more balanced, and it is more suitable for the use of the scaffold for periodontitis treatment in actual processes.

[0079] Resveratrol has a certain ultraviolet absorbance and can diffuse into the cavity of hollow mesoporous silica through osmotic pressure. Its release amount is measured using an ultraviolet spectrophotometer. Figure 6 It can be seen that as the concentration of Res increases, the drug loading is between 30% and 40%, and the drug release is maintained between 50% and 60%, indicating that the large-volume cavity structure mesoporous silica prepared by the present invention has a significant increase in the loading capacity of resveratrol, which helps to increase the content of effective ingredients in the stent when the implantation of the stent is limited, and enhance the therapeutic effect of the stent on periodontitis.

[0080] pass Figure 7 The cell adhesion phenomenon can be seen, indicating that the porous mixed biomaterial prepared by the present invention provides a larger adhesion surface for seed cells, exhibits a certain aggregation growth, promotes cell differentiation, and helps promote the formation or regeneration of bone tissue.

[0081] In summary, the mixed biomaterial is prepared by the method of the present invention, and the scaffold is made of the mixed biomaterial as the raw material. When the number of implanted scaffolds is limited, the loading amount of the effective ingredients can be increased, and the scaffold can have a more complete therapeutic effect, thereby effectively improving the therapeutic effect of the scaffold on periodontitis.

[0082] Finally, it should be noted that the above preferred embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. Although the present invention has been described in detail through the above preferred embodiments, those skilled in the art should understand that various changes can be made in form and details without departing from the scope defined by the claims of the present invention.

Claims

1. A resveratrol-loaded microsphere mixed biomaterial, characterized in that: The mixed biomaterial uses mesoporous silica as a shell to form microspheres with a cavity structure, and resveratrol is loaded in the microspheres and the cavity, and is mixed with biphasic calcium phosphate to form a mixed biomaterial.

2. The method for preparing the resveratrol-loaded microsphere mixed biomaterial according to claim 1, characterized in that: The preparation method comprises the following steps: (1) Preparation of polystyrene microspheres: 1.42 g of polyvinyl pyrrolidone was dissolved in 400 ml of deionized water, and then 80 g of styrene monomer was added to the solution. The solution was stirred and nitrogen was continuously introduced, and then heated in an oil bath. After the solution was heated to a certain temperature and stabilized by heat, 1.2 g of 2,2-azobis(2-methylpropylimidamide) dihydrochloride was added to the solution. After emulsification for a certain period of time, the solution was washed with deionized water and anhydrous ethanol respectively, and then centrifuged and dried to obtain polystyrene microspheres. (2) Preparation of hollow structure mesoporous silica microspheres: 1 g of the polystyrene microspheres prepared in step (1) was added to deionized water containing 16 ml of triethanolamine and 0.7 g of hexadecyltrimethylammonium bromide, and ultrasonically dispersed, and then 140-180 μl of tetraethyl orthosilicate was added for reaction. After the reaction, the microspheres were washed with deionized water and anhydrous ethanol respectively, and then centrifuged to obtain a product, which was then calcined to obtain hollow structure mesoporous silica microspheres; (3) Resveratrol-loaded hollow structure mesoporous silica microspheres: 10 mg of the hollow structure mesoporous silica microspheres prepared in step (2) are ultrasonically dispersed in anhydrous ethanol, and resveratrol is added. After constant temperature and light-proof oscillation in a water bath shaker, the complex solution is poured out, washed with ultrapure water and anhydrous ethanol respectively, and dried in an oven. After drying, hollow structure mesoporous silica microspheres loaded with resveratrol are obtained, and the amount of resveratrol added is such that 1 to 5 mg of resveratrol is added per milliliter of anhydrous ethanol; (4) Preparation of mixed biomaterials: The resveratrol-loaded hollow structure mesoporous silica microspheres obtained in step (3) and biphasic calcium phosphate are mixed in a mass ratio of resveratrol-loaded hollow structure mesoporous silica microspheres: biphasic calcium phosphate = 1:10, and the mixed biomaterials of resveratrol-loaded hollow structure mesoporous silica microspheres and biphasic calcium phosphate are obtained.

3. The method for preparing a microsphere mixed biomaterial loaded with resveratrol according to claim 2, characterized in that: In the step (1), the oil bath is heated to 90° C. and the emulsification time is 24 hours.

4. The method for preparing a microsphere mixed biomaterial loaded with resveratrol according to claim 2, characterized in that: In the step (1), the stirring and continuous nitrogen introduction time is 30 minutes.

5. The method for preparing a microsphere mixed biomaterial loaded with resveratrol according to claim 2, characterized in that: In the step (2), the reaction time after adding tetraethyl orthosilicate is 2 hours.

6. The method for preparing a microsphere mixed biomaterial loaded with resveratrol according to claim 2, characterized in that: During the calcination of the product of step (2), the temperature is raised to 550° C. at a rate of 5° C. / min, and the product is calcined at 550° C. for 4 h to 4.5 h.

7. The method for preparing a resveratrol-loaded microsphere mixed biomaterial according to claim 2, characterized in that: In the step (3), the constant temperature and light-proof oscillation temperature is 36.5° C. to 37° C., and the oscillation time is 48 hours.

8. The method for preparing a resveratrol-loaded microsphere mixed biomaterial according to claim 2, characterized in that: In the step (3), the drying temperature is 40 to 50° C. and the drying time is 20 to 24 hours.

9. Use of a scaffold made of a resveratrol-loaded microsphere mixed biomaterial prepared by the preparation method according to any one of claims 2 to 8 in treating periodontitis.

Citation Information

Cited By

  • Resveratrol-based nano pesticide delivery system as well as construction method and application thereof

    CN121100919A