Method for producing artificial vitreous fibers

By introducing metal aluminum into the electric furnace to control the FeO:Fe2O3 ratio, the problem of artificial glass fibers excessively shrinking at high temperatures is solved, its high temperature stability and fire resistance are improved, and the risk of thermal bridges and insulation gaps is reduced.

CN118894643APending Publication Date: 2024-11-05ROCKWOOL AS
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411145791.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2020-01-30
Filing Date
2021-01-29
Publication Date
2024-11-05

AI Technical Summary

Technical Problem

When using a molybdenum electrode to make artificial glass fibers, the product may experience excessive shrinkage at high temperatures, resulting in the formation of thermal bridges and insulation gaps, affecting its fire resistance and high temperature stability.

Method used

By introducing metal aluminum into the furnace to combine with other mineral materials, the redox reaction is promoted and the FeO:Fe2O3 ratio is controlled to reduce the shrinkage of the fiber.

Benefits of technology

It effectively reduces the shrinkage degree of consolidated MMVF products, improves its high temperature stability and fire resistance, and reduces the risk of forming thermal bridges and insulation gaps.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118894643A_ABST
    Figure CN118894643A_ABST
Patent Text Reader

Abstract

The present invention relates to a method of manufacturing artificial vitreous fibers, and provides a method of manufacturing artificial vitreous fibers (MMVF) comprising providing an electric furnace having a molybdenum electrode, providing a mineral feedstock wherein the mineral feedstock comprises (a) a particulate material comprising metallic aluminum and (b) a further mineral component, introducing the mineral feedstock into the furnace, the method includes melting the mineral feedstock to form a mineral melt, and forming MMVF from the mineral melt, the method being advantageous for reducing shrinkage of the consolidated MMVF product.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] This patent application is application number 2021800214827 and application date is January 2021

[0002] On the 29th, a divisional application for a patent application entitled "Method for producing artificial vitreous fiber" was filed. Technical Field

[0003] The present invention relates to a method for producing man-made vitreous fiber (MMVF) by melting ore in an electric furnace. Background Art

[0004] The present invention relates to a method for manufacturing MMVF and consolidated MMVF products (e.g. insulation products). Typically, a mineral raw material (ore) having a desired overall chemical composition is melted in a furnace, the mineral melt is removed and fed to a fiberizing device, such as an external or internal centrifugal device,

[0005] The fibers are then collected, further processed if necessary and formed into an insulation batt, usually with a binder.

[0006] There are a number of reasons why it is preferable to use an electric furnace instead of a coal, oil or gas fired furnace. Electric furnaces have the potential to be powered by renewable energy, so the environmental profile of an electric furnace may be better than a combustion furnace. It may also be advantageous if renewable electricity is used because it is cheaper, at least in part due to lower carbon taxes. Using an electric and / or gas fired furnace also eliminates the need to clean up sulfur dioxide compared to a coal or oil fired furnace.

[0007] However, in the case of electric furnaces using molybdenum electrodes, the resulting MMVF products may show excessive shrinkage due to sintering at high temperatures. Shrinkage can lead to the formation of thermal bridges, which can be critical if the product is used for fire protection. In general, low-density products show greater shrinkage than high-density products.

[0008] Standard electric furnaces for MMVF production use molybdenum or carbon electrodes. These electrodes provide the energy required to melt the mineral material through the Joule effect. Typically, molybdenum electrodes with Mo purity >99% are inert to the molten mineral material and therefore do not participate in the Fe 2 O 3 To the reduction of FeO oxides. In consolidated MMVF products, FeO is an important component to limit fiber shrinkage, provide fire resistance and high temperature stability.

[0009] It would be desirable to provide a method by which a melt suitable for processing into MMVF can be produced using an electric furnace with molybdenum electrodes to provide the melt without excessive shrinkage in the product.

[0010] The sintering shrinkage of the consolidated MMVF product under high temperature or fire conditions is required to be within an acceptable range. Shrinkage should be avoided or at least reduced as much as possible, because thermal bridges and insulation gaps will form when the consolidated MMVF product shrinks under high temperature conditions.

[0011] It is desirable to further reduce the degree of shrinkage in consolidated MMVF products. Summary of the invention

[0012] The inventors have solved the problem of reducing the shrinkage of consolidated MMVF products using the method of claim 1.

[0013] Molybdenum electrodes, unlike the main electrode type of choice for mineral melting furnaces (i.e., graphite electrodes), do not produce reducing conditions in the mineral melt. This results in a lower ratio of Fe(II) to Fe(III) than is required for a fireproof MMVF product, since reducing conditions are required to increase this ratio. It is desirable to increase the ratio of Fe(II) to Fe(III) to improve the high temperature stability of the MMVF product and increase its fire resistance. In particular, a higher ratio will minimize or even prevent shrinkage of the MMVF in a fire or other high temperature situation.

[0014] The method of claim 1 solves this problem by introducing metallic aluminum into the furnace, either in combination with other mineral materials or added alone, thereby creating the reducing conditions required to achieve the desired ratio of Fe(II) to Fe(III). This is because a redox reaction occurs in the method of the invention, whereby metallic aluminum is oxidized to form Al 2 O 3 And Fe 2 O 3 Reduction to form FeO. Therefore, FeO:Fe 2 O 3 ratio.

[0015] The material containing metallic aluminum may contain 0.5 wt % to 10 wt % of metallic aluminum, and preferably 1 wt % to 5 wt % of metallic aluminum.

[0016] The material containing metallic aluminum may further contain 50 wt % to 90 wt % of aluminum oxide in addition to metallic aluminum. Aluminum oxide is an important component of MMVF, so it is beneficial to include it together with metallic aluminum.

[0017] The material containing metallic aluminum may be in granular form, with 90% by weight of the particles being less than 1 mm. This may facilitate uniform premixing of the metallic aluminum source with other mineral components, thereby enabling the mineral melt to have a consistent composition. Preferably, the material is aluminum slag.

[0018] Aluminum slag is a granular waste material from the aluminum processing industry, consisting mainly (usually 50 to 90 wt %) of Al 2O 3 , and about 0.5 wt % to 10 wt % of metallic aluminum. The aluminum slag may account for 5 wt % to 30 wt %, such as about 10 wt %, of the total ore.

[0019] The aluminum slag contains 0.5 to 10 wt % of metallic aluminum, 50 to 90 wt % of aluminum oxide Al 2 O 3 and 0 wt % to 49.5 wt % of other materials. Preferably, the aluminum slag contains 2 wt % to 6 wt % of metallic aluminum. Other materials may include SiO 2 , MgO and Fe 2 O 3 Preferably, the aluminum slag comprises oxides of corundum, spinel and mullite.

[0020] The aluminum slag may have a controlled particle size distribution. For example, the aluminum slag may have a particle size distribution such that 90% of the particles by weight are less than 1 mm, preferably 90% of the particles by weight are less than 200 μm. The average particle size of the aluminum slag may be 10 μm to 100 μm, such as 20 μm to 30 μm.

[0021] The content of metallic aluminum and aluminum oxide (and other components) is on a dry basis and can be determined using standard methods. For example, the content of metallic aluminum can be determined by reacting the material with a strong base (such as NaOH). The amount of metallic aluminum can be determined from the amount of hydrogen released.

[0022] Aluminum slag may preferably be a waste product derived from secondary mining of aluminum. In particular, the aluminum casting process provides a special alumina-rich waste material, commonly referred to as "aluminum slag". Aluminum slag often contains a significant proportion of metallic aluminum and is therefore processed to recover metallic aluminum. The aluminum slag is usually crushed, ground and screened. This produces some aluminum for resale and an aluminum-rich portion, which is sent to a furnace for reuse. As a by-product, an alumina-rich powder is also produced. In the method of the present invention, the powder can be used as a source of metallic aluminum. This alumina-rich powder produced by processing aluminum slag (crushed aluminum slag) may contain, for example, 1% to 10%, preferably 1% to 8% of halogen materials (by weight). Halogens include fluorides and chlorides in particular.

[0023] The aluminum-rich fraction, optionally together with other aluminum-containing waste materials, is remelted in a furnace. The furnace may be a rotary furnace or a kiln. The aluminum waste may be subjected to plasma heating. Conventional furnaces may be used. Salt is usually added to the furnace to reduce the surface tension of the aluminum and reduce oxidation. The process produces an aluminum fraction for resale, more aluminum slag and salt slag material. The salt slag may be treated by a wet chemical process (including water washing and high temperature treatment) to produce a salt fraction (which is recycled to the furnace) and a further alumina-rich powder (which may also be used as a metallic aluminum source in the present invention). This product tends to have a lower content of halogen materials (such as fluorides) than the alumina-rich powder produced by aluminum slag treatment (crushed aluminum slag). Its halogen content (by weight) tends to be 0 to 5%, usually at least 0.5% or 1%, preferably not more than 3%.

[0024] Aluminum slag is a granular waste material from the aluminum processing industry, consisting mainly (usually 50 to 90 wt %) of Al 2 O 3 , and about 0.5 wt % to 10 wt % metallic aluminum. The aluminum slag may comprise 5 wt % to 30 wt %, for example about 10 wt %, of the total ore charge. Using an amount within this range reduces the need to use virgin raw materials for the alumina component of the MMVF composition while maintaining the desired effect of minimizing shrinkage of the consolidated MMVF product.

[0025] In some embodiments, the material containing metallic aluminum contains 45% to 100% by weight of metallic aluminum, preferably at least 85% by weight of metallic aluminum. This higher percentage of metallic aluminum means that the percentage of this material in the total mineral raw material may be lower. For example, the mineral raw material may contain 0.05% to 10% by weight of the material containing 45% to 100% by weight of metallic aluminum in terms of metallic aluminum. The material containing 45% to 99% by weight of metallic aluminum can be in any suitable physical form. Suitable materials include aluminum pellets and one or more metallic aluminum blocks.

[0026] The amount of aluminum pellets required as part of the total ore charge is much lower than the amount of aluminum slag required for the same amount of metallic aluminum, and is about 0.2 weight % of the total ore charge, such as 0.1 weight % to 0.5 weight % of the total ore charge, such as 0.2 weight % to 0.4 weight % of the total ore charge, calculated as metallic aluminum.

[0027] The block may take any suitable form, such as a rod, a bar, a lump or other shape. The block may contain 45% to 99% by weight of metallic aluminum and is preferably substantially entirely metallic aluminum. When one or more blocks are used as a source of metallic aluminum, it is preferred that the block is in the form of a rod.

[0028] Aluminum in the form of rods or other bulk forms can be inserted directly into the mineral melt in the furnace. This method avoids premature oxidation of the aluminum, thereby improving process efficiency.

[0029] To avoid premature oxidation of its metallic aluminum component, aluminum pellets can be added directly to the molten pool. For example, aluminum can be added through a burner or lance, such as an oxy-fuel burner with a central tube for transporting the aluminum pellets.

[0030] As a raw material component containing only aluminum pellets, the aluminum pellets can be added alone. Alternatively, it can be pre-mixed with a filler and the mixture of aluminum pellets and filler is added to the furnace as a mixed raw material component. Suitable fillers include various raw materials that can be used as additional raw materials. For example, the aluminum pellets can be mixed with filtered fines (i.e., fine particle raw materials extracted from the exhaust filter of the process) before being injected into the cyclone furnace. In the mixture with the filler, a suitable percentage of aluminum pellets is 1% to 90%, such as 10% to 70%, such as 15% to 50%. Using a mixture of aluminum pellets and other raw materials can improve the dosage control of metallic aluminum in the process.

[0031] Since the density of the melt and metallic aluminum are similar, the aluminum particles are well mixed with the melt.

[0032] Furthermore, aluminum pellets are a purer material than aluminum slag.

[0033] The particle size (average particle size, where the particle size adopts the maximum dimension of the particle, whether or not the particle is spherical) of the aluminum particles may be no greater than 15 mm, such as less than 10 mm, such as less than 5 mm. In a preferred embodiment, the particle size (average particle size, where the particle size adopts the maximum dimension of the particle, whether or not the particle is spherical) of the aluminum particles may be no greater than 3 mm, such as less than 2 mm, such as less than 1 mm.

[0034] In the present invention, the mineral raw material may contain 0.1 wt% to 0.5 wt% of metallic aluminum.

[0035] In a preferred embodiment, the MMVF has the following element contents, expressed in wt. % of oxides:

[0036] SiO 2 : At least 30, 32, 35 or 37; not more than 51, 48, 45 or 43

[0037] CaO: at least 8 or 10; not more than 30, 25 or 20

[0038] MgO: at least 2 or 5; not more than 25, 20 or 15

[0039] FeO (including Fe 2 O 3 ): At least 4 or 5; not more than 15, 12 or 10

[0040] FeO+MgO: at least 10, 12 or 15; not more than 30, 25 or 20

[0041] Na 2 O+K 2 O: 0 or at least 1; not more than 10

[0042] CaO+Na 2 O+K 2 O: At least 10 or 15; no more than 30 or 25

[0043] TiO 2 : 0 or at least 1; not more than 6, 4 or 2

[0044] TiO 2 +FeO: at least 4 or 6; not more than 18 or 12

[0045] B 2 O 3 : 0 or at least 1; not more than 5 or 3

[0046] P 2 O 5 : 0 or at least 1; not more than 8 or 5

[0047] Others: 0 or at least 1; not more than 8 or 5.

[0048] The fibers preferably have a sintering temperature above 800°C, more preferably above 1000°C.

[0049] The MMVF produced by the method of the present invention preferably has the following composition, in wt %:

[0050] SiO 2 35 to 50

[0051] Al 2 O 3 12 to 30

[0052] TiO 2 Up to 2

[0053] Fe 2 O 3 3 to 12

[0054] CaO 5 to 30

[0055] MgO up to 15

[0056] Na 2 O 0 to 15

[0057] K 2 O 0 to 15

[0058] P 2 O 5 Up to 3

[0059] MnO up to 3

[0060] B 2 O 3 Up to 3.

[0061] Another preferred composition of MMVF is as follows, in wt %:

[0062] SiO 2 39% to 55%, preferably 39% to 52%,

[0063] Al 2 O 3 16% to 27%, preferably 16% to 26%,

[0064] CaO 6% to 20%, preferably 8% to 18%,

[0065] MgO 1% to 5%, preferably 1% to 4.9%,

[0066] Na 2 O 0% to 15%, preferably 2% to 12%,

[0067] K 2 O 0% to 15%, preferably 2% to 12%,

[0068] R 2 O(Na 2 O+K 2 O) 10% to 14.7%, preferably 10% to 13.5%,

[0069] P 2 O 5 0% to 3%, preferably 0% to 2%,

[0070] Fe 2 O 3 (iron total) 3% to 15%, preferably 3.2% to 8%,

[0071] B 2 O 3 0% to 2%, preferably 0% to 1%,

[0072] TiO 2 0% to 2%, preferably 0.4% to 1%,

[0073] Others 0% to 2.0%.

[0074] The composition may be suitably used as a fiberizing device in conjunction with an internal centrifugal device.

[0075] SiO 2The preferred range of CaO is 39% to 44%, especially 40% to 43%. The preferred range of CaO is 9.5% to 20%, especially 10% to 18%.

[0076] Al 2 O 3 The content is preferably between 16% and 27%, preferably greater than 17% and / or preferably less than 25%, SiO 2 and Al 2 O 3 The sum of the alkali metal (sodium and potassium) oxides (R 2 The amount of magnesium oxide is preferably relatively high, but is limited to 10% to 14.7%, preferably 10% to 13.5%, wherein the amount of magnesium oxide is at least 1%.

[0077] Preferably, by weight, Al 2 O 3 The content of magnesium oxide is 17% to 25%, in particular 20% to 25%, in particular 21% to 24.5%, especially about 22% to 23% or 24%. Advantageously, the magnesium oxide content is at least 1.5%, in particular 2%, preferably 2% to 5%, particularly preferably >2.5% or 3%.

[0078] By weight, in Al 2 O 3 When the content of Al is at least 22%, the amount of magnesium oxide is preferably at least 1%, advantageously about 1% to 4%, preferably 1% to 2%, and in particular 1.2% to 1.6%. In order to maintain a sufficiently low liquidus temperature, Al 2 O 3 The content of Al is preferably limited to 25%. 2 O 3 When the content is lower, for example, about 17% to 22%, the amount of magnesium oxide is preferably at least 2%, especially about 2% to 5%.

[0079] The total amount of Fe and Mg oxides is important in controlling the shrinkage of MMVF insulation. In addition, the ratio of Fe(II):Fe(III) affects the insulation performance of MMVF under fire conditions, where oxidation of Fe(II) to Fe(III) is a favorable process.

[0080] Advantageously, the ratio of Fe(II):Fe(III) of the fibers is higher than 2, for example higher than 3. The proportion of Fe(3+) in the MMVF before the fiberizing step is generally less than 5%, preferably less than 3%, based on the total Fe content in the melt. This helps to prevent shrinkage.

[0081] The amounts of Fe(2+) and Fe(3+) can be determined using the formula described in “The ferric / ferrous ratio in basalt melts at different oxygen pressures” (Helgason et al., Hyperfine Interact., 45 (1989), pp. 287 to 294). Method determination.

[0082] The total iron in the entire melt or fiber composition is expressed as Fe based on the total oxides in the melt or fiber. 2 O 3 Calculation. This is the standard method of quoting the amount of iron present in such an MMVF, charge or melt. The FeO and Fe present 2 O 3 The actual weight percentage will vary depending on the iron oxide ratio and / or redox state of the melt. For example:

[0083]

[0084]

[0085] Table 1

[0086] Thus, one skilled in the art will appreciate that the actual weight percent of iron oxide present will depend on the ratio of Fe(2+) to Fe(3+).

[0087] The method of the present invention may further comprise consolidating the MMVF to form a consolidated product comprising the MMVF. The consolidated product may be used in many applications, including fireproof insulation products. In such applications, reducing shrinkage is particularly advantageous because it reduces the risk of thermal bridges or insulation gaps forming in critical situations.

[0088] Suitable furnaces for use in the process of the present invention include electric glass melting furnaces known to those skilled in the art, which use Joule heating with molybdenum electrodes to melt the mineral feedstock. Optionally, Joule heating may be supplemented with the combustion of a gaseous fuel.

[0089] The invention may also be implemented in a tank furnace in which the mineral feedstock is melted by the heat from the combustion of a gaseous fuel, aided by Joule heating of molybdenum electrodes. These types of furnaces are known to those skilled in the art.

[0090] As is known, the raw materials used as the remainder of the ore charge can be selected from a variety of sources. These include basalt, diabase, nepheline syenite, cullet, bauxite, quartz sand, limestone, borax, sodium tetraborate, dolomite, soda, olivine sand, potash. Waste materials can also be used.

[0091] MMV fibers can be made from mineral melts in a conventional manner. Typically, they are made by a centrifugal fiberization process.

[0092] For example, the fibers can be formed by a spinning rotor process, in which they are thrown outward through holes in the spinning rotor. The melt is fiberized by the spinning rotor technology (sometimes also called internal centrifugation). Before being directed to the spinning rotor, the melt preferably has a temperature in the range of 1260° C. to 1300° C. at the end of the feeder channel. When the melt is transferred from the feeder channel to the inner part of the spinning rotor, it is preferably cooled down so that the temperature of the melt when flowing through the holes of the spinning rotor is in the range of 1150° C. to 1220° C.

[0093] The viscosity of the melt in the spinning rotor is in the range of 50 Pa.s to 400 Pa.s, preferably in the range of 100 Pa.s to 320 Pa.s, and more preferably in the range of 150 Pa.s to 270 Pa.s. If the viscosity is too low, fibers of a desired thickness cannot be formed. If the viscosity is too high, the melt does not flow through the holes in the spinning rotor at an appropriate discharge rate, which may cause clogging of the holes in the spinning rotor.

[0094] The melt is preferably fiberized by a spinning rotor process at a temperature between 1160° C. and 1210° C. At the spinning temperature, the viscosity of the melt is preferably in the range of 100 Pa.s to 320 Pa.s.

[0095] In another fiber forming process, the melt may be thrown from a rotating disk and fiber formation may be promoted by passing a jet of injected gas through the melt.

[0096] In a preferred method, fiber formation is performed by pouring the melt onto the first rotor in a cascade spinneret. In this case, the melt is preferably poured onto the first of a set of two, three or four rotors, each rotating about a substantially horizontal axis, whereby the melt on the first rotor is primarily thrown onto the second (lower) rotor, although some may be thrown off the first rotor in the form of fibers, and the melt on the second rotor is thrown off in the form of fibers, although some may be thrown toward the third (lower) rotor, and so on.

[0097] MMVF can be collected and consolidated to form a consolidated product comprising MMVF. Typically, such products may include additional ingredients, such as a binder, wherein MMVF is the main ingredient. The fibers produced by the spinning process are preferably collected on a conveyor belt. The binder can be applied to the MMVF in the fiberization process or after fiberization. The binder can be applied by spraying the MMVF. The conventional type of binder used with rock wool fibers can be used. The binder is then cured to produce a final product. The MMVF with a binder is typically cured in a curing oven, typically by a hot air stream. A hot air stream can be introduced into the MMVF with a binder from below or above or from alternating directions in different regions in the length direction of the curing oven. After curing, the cured binder composition bonds the fibers to form a structurally adhered fiber matrix.

[0098] The MMVF may be consolidated after collection, for example by cross-lapping and / or longitudinal compression and / or vertical compression in a known manner. Typically consolidation occurs before the binder cures.

[0099] The MMVF produced by the method of the present invention and the MMVF of the present invention have excellent fire resistance at 1000°C. The MMVF can be made into products for any conventional application of MMVF (e.g., sound insulation or heat insulation or fire protection). Such products include insulation products such as insulation wool, particles, boards, rolls, pipe sections, and other products such as tiles and loose fibers. The product can be used in high temperature environments, such as at least 400°C to as high as 1000°C.

[0100] The product may have any density known in the art for the relevant application. For example, the density may be 20 kg / m 3 Up to 1200kg / m 3 In the range of 20kg / m 3 Up to 300kg / m 3 In the range of 20kg / m 3 Up to 150kg / m 3 Shrinkage can lead to the formation of thermal bridges, which can be critical if the product is used for fire protection. All product types have advantages in terms of shrinkage, but it has been observed that when the density of the product is relatively low (e.g. not more than 50kg / m 3 ), a particularly good reduction in shrinkage can be seen. BRIEF DESCRIPTION OF THE DRAWINGS

[0101] Figure 1 A typical electric furnace that can be used in the process of the present invention is shown.

[0102] Figure 2 Shows Figure 1 Electrode arrangement in cross section. DETAILED DESCRIPTION

[0103] Now refer to Figure 1 and 2 An exemplary method according to the invention is described.

[0104] exist Figure 1 and 2 An electric furnace 1 is schematically shown in FIG. A mineral feedstock is introduced into the furnace 1 through one or more inlets 2, 3 and forms a layer 4 on top of a molten pool 5. The mineral feedstock is melted by Joule heating facilitated by molybdenum electrodes 6. The electrodes 6 are Figure 1 and 2 1 is shown protruding from the side wall 7 of the furnace 1. In other configurations, the electrodes may emerge from the top, as long as the electrodes are protected by air. Alternatively, the electrodes may emerge from the bottom of the furnace. Various options for the basic arrangement of electric glass melting tank furnaces are generally known in the art.

[0105] The material containing metallic aluminium may be premixed with other mineral components and introduced as a homogenous charge into the furnace 1 through one or more inlets 2, 3. This option may be more preferred when aluminium slag is used as the material containing metallic aluminium.

[0106] Alternatively, the material containing metallic aluminum may be introduced separately from the remaining mineral material into the furnace 1. For example, the material containing metallic aluminum may be introduced into the furnace 1 through the inlet 2, while the other mineral material may be introduced into the furnace 1 through a separate inlet 3. This option may be more preferred when aluminum pellets or blocks are used as the material containing metallic aluminum.

[0107] When metallic iron is formed, an optional outlet 8 formed in the base 9 of the furnace 1 may be used to conduct away the metallic iron. Preferably, metallic iron is not formed in the process, so the outlet 8 may not be required.

[0108] The mineral melt from the molten bath 5 leaves the furnace 1 through a melt outlet 10. The melt outlet 10 is shown as being formed in the side wall 7 of the furnace 1, but could equally well be formed in the base 9.

[0109] On leaving the furnace 1, the mineral melt may optionally be subjected to a refining process. Alternatively, the mineral melt may be conveyed directly to a fiberizing device 11 to form man-made vitreous fibers (MMVF). Internal or external centrifugation may be used, so the details of the fiberizing device 11 are not shown. Suitable fiberizing devices are known to those skilled in the art.

[0110] The MMVF formed at the device 11 can be collected and stored, or they can be directly processed into a consolidated product at the processing line 12 (details not shown).

[0111] The flue gas outlet 13 is shown to be arranged at the top of the side wall 7 of the furnace 1. However, it may also be arranged at the top of the furnace, using arrangements known to those skilled in the art.

[0112] Aluminum slag

[0113] Test methods

[0114] The area shrinkage of the consolidated MMVF product can be measured according to the following test method:

[0115] 1) Cut, measure and weigh the test samples from the product test unit;

[0116] 2) Select representative test samples from the test unit;

[0117] 3) Remove the binder at 590°C;

[0118] 4) sintering the test sample at 1000°C + / - 20°C for 30 minutes; and

[0119] 5) Measure the area of ​​the test sample after sintering.

[0120] Shrinkage is measured as the percentage reduction in surface area of ​​each product. Shrinkage is measured on the principal surface of each product, which is the main surface that is visible in the finished product. For example, the reduction in length and width of a board is measured, but not its thickness.

Claims

1. A method of making a man-made vitreous fiber (MMVF) comprising at least 3% by weight of iron oxide measured as Fe2O3, the method comprising: An electric furnace having molybdenum electrodes is provided, Provide mineral raw materials, The mineral raw material comprises (a) a material containing metallic aluminum and (b) other mineral components, introducing said mineral raw material into said furnace, melting the mineral feedstock to form a mineral melt, and A MMVF is formed from the mineral melt.

2. The method according to any one of the preceding claims, wherein the material comprising metallic aluminum comprises 0.5 wt% to 10 wt% metallic aluminum.

3. The method according to any one of the preceding claims, wherein the material comprising metallic aluminum further comprises 50 wt% to 90 wt% aluminum oxide.

4. A method according to any one of the preceding claims, wherein the material comprising metallic aluminium is in granular form and wherein 90% by weight of the particles are smaller than 1 mm.

5. The method according to any one of the preceding claims, wherein the material comprising metallic aluminum is aluminum slag.

6. The method according to claim 4 or 5, wherein 5 to 30 wt. % of the mineral raw material is aluminum slag.

7. The method according to claim 1, wherein the material containing metallic aluminum contains 45 wt% to 100 wt% metallic aluminum.

8. The method according to claim 7, wherein the mineral raw material contains 0.05 wt% to 10 wt% of the material containing metallic aluminum, and the material containing metallic aluminum contains 45 wt% to 100 wt% of metallic aluminum.

9. The method according to claim 7, wherein the material containing metallic aluminum is aluminum pellets.

10. The method according to claim 9, wherein the average particle size of the aluminum particles is not greater than 3 mm.

11. The method according to any one of the preceding claims, wherein the mineral feedstock comprises 0.1 to 0.5 wt. % metallic aluminum.

12. The method according to any one of the preceding claims, wherein the MMVF has the following oxide content, in wt. %:

13. The method according to any one of claims 1 to 11, wherein the MMVF comprises the following oxide contents, in wt. %:

14. A method according to any one of the preceding claims, wherein the MMVF has a ratio of Fe(II):Fe(III) greater than 2, such as greater than 3.

15. The method of any one of the preceding claims, further comprising consolidating the MMVF to form a consolidated product comprising the MMVF.

Citation Information

Patent Citations

  • Melt composition for the production of man-made vitreous fibres

    CN104203851A

  • Process and apparatus for forming man-made vitreous fibres

    CN104918893A

  • Electric melting furnace arrangement as well as a method of influencing the composition of a mineral melt for producing wool

    US4697274A

  • Production of vitreous fibres using high halogen mineral waste as an ingredient

    US6698245B1

  • Apparatus and method for the production of man-made vitreous fibres

    WO1999028249A1