Continuous casting slab internal quality control method based on preset nucleation

By using high-purity iron powder to form a fine core during continuous casting, the grain refinement and pollution problems in the casting blank are solved, the density and mechanical properties of the casting blank are improved, and the cost and pollution are reduced.

CN118905173APending Publication Date: 2024-11-08SHANDONG IRON & STEEL CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410998780.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-24
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The prior art is difficult to effectively refine grains during continuous casting, resulting in the casting billet being prone to internal defects such as central segregation, loosening and shrinkage holes, and impurities contamination of iron powder affects the quality of the liquid steel.

Method used

High-purity iron powder (iron content ≥99%) is used to blow the argon plug rod, and preheat argon to spray the iron powder evenly into the steel water to form a fine and diffuse core, promote the refinement and uniform distribution of grains, and control the The solidification process of the casting billet.

Benefits of technology

It significantly reduces the central segregation and looseness of the casting billet, improves the internal density of the casting billet and the mechanical properties of the steel, reduces liquid steel pollution, reduces costs, and speeds up the solidification speed of the casting billet.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118905173A_ABST
    Figure CN118905173A_ABST
Patent Text Reader

Abstract

A continuous casting billet internal quality control method based on preset nucleation comprises the steps that in the molten steel casting process, argon is preheated, high-purity iron powder with the iron content larger than or equal to 99% is blown through an argon blowing stopper rod, the iron powder is mixed with steel flow along with the argon and enters a crystallizer through a submersed nozzle, and fine and dispersed nucleation cores are formed to finish refining of a continuous casting billet solidification structure. According to the method, the high-purity iron powder is injected to serve as a preset nucleating agent, so that the center segregation of the casting blank is remarkably reduced, the center segregation of the obtained Q460C casting blank is class-C first level, center porosity and middle cracks do not exist, and the center segregation of the obtained Q345B casting blank is class-C 0.5 level, and center porosity does not exist; compared with second-phase particles, the selected high-purity iron powder does not bring in other impurities, molten steel pollution can be effectively reduced, the iron powder is low in price, and the cost is reduced; and secondly, part of blown high-purity iron powder is melted, so that the superheat degree of molten steel can be reduced, the solidification speed is increased, the utilization rate of particles is high, and the grain refining effect is better.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of iron and steel metallurgy, and in particular relates to a method for controlling the internal quality of a continuous casting billet based on preset nucleation. Background Art

[0002] Continuous casting is the intermediate link between steelmaking and steel rolling, and is also the central link in the steel manufacturing process. The quality of continuous casting billets directly determines the production efficiency and quality of steel products. The continuous casting process is actually the process of molten steel nucleation and solidification. When the molten steel is supercooled to the actual liquidus temperature in the crystallizer, small atomic clusters begin to appear in the liquid phase after the incubation period and then form embryos. When the embryos reach a certain critical size, they become stable and spontaneously growing nuclei, which are called nucleation. Stable and rapid nucleation process is the key factor in determining the quality of continuous casting products.

[0003] There are two types of nucleation during the solidification of molten steel: homogeneous nucleation and heterogeneous nucleation. The main influencing factors of homogeneous nucleation are liquid steel temperature, heat flux density, pouring speed, etc. Its characteristic is that the probability of new phase nuclei appearing in each region of the liquid phase is approximately the same. It is a process that directly nucleates from the crystal embryo by relying on the energy change of the liquid metal. If the method of forming nuclei by attaching to some existing particles in the liquid metal is called heterogeneous nucleation. In the actual continuous casting process, the crystallization of molten steel mostly belongs to heterogeneous nucleation, which is easier than homogeneous nucleation and can be nucleated when the supercooling is not large. CN111451462A discloses a method of using an immersion nozzle to spray magnesium powder to refine the solidification structure of the continuous casting billet. During the molten steel casting process, magnesium powder is sprayed into the molten steel before solidification, and nanometer-level second phase particles are obtained with high efficiency and low cost, and the solidification structure of the continuous casting billet is refined to achieve the improvement of steel performance. In comparison, the magnesium powder has a larger particle size and a higher price, and the cost reduction is limited. CN1380427A discloses an iron powder cored wire for steelmaking, which consists of an outer skin and a wire core, wherein the outer skin is a soft steel strip and the wire core is iron powder, which is tightly filled in the outer skin. After the iron powder cored wire is added to the continuous casting molten steel, these fine iron powders, as particles for crystallization nucleation of the molten steel, quickly form a large number of equiaxed crystals, refine the grains, and reduce the internal defects such as center segregation, center looseness and shrinkage cavities of the continuous casting billet, especially small square billet and large square billet. However, the iron powder added by this process cannot be effectively dispersed, the degree of grain refinement is limited, and the iron content of the iron powder is only 95%. The large amount of harmful elements brought back will cause pollution to the molten steel, seriously affecting the quality of the steel grade.

[0004] Nucleation during solidification of molten steel is a very important process in the continuous casting process. Reasonable selection of nucleating agents and setting of parameters of the nucleation process can ensure the quality of the continuous casting billet, avoid a series of quality problems and improve production efficiency. Summary of the invention

[0005] Based on the above technical background, the present invention provides a method for controlling the internal quality of continuous casting billets based on preset nucleation, which utilizes an argon blowing plug rod to evenly and stably blow tiny high-purity iron powder into the molten steel in the tundish to form a fine dispersed nucleation core, thereby realizing preset nucleation during the solidification process, thereby accelerating the solidification speed of the core of the billet, and making the solidification of the billet balanced, so as to achieve the purpose of controlling the grain growth state of the continuous casting process and improving the internal quality of the billet, and avoiding internal defects such as looseness, shrinkage holes and segregation during the solidification process.

[0006] In order to achieve the above purpose, the technical solution adopted is:

[0007] A method for controlling the internal quality of a continuous casting billet based on preset nucleation. During the molten steel casting process, preheated argon is used to blow high-purity iron powder with an iron content of ≥99% through an argon blowing plug rod. The iron powder is mixed with the steel flow after being sprayed out with the argon and enters the crystallizer through an immersed water nozzle to form a fine and dispersed nucleation core, thereby completing the refinement of the solidification structure of the continuous casting billet.

[0008] The above technical solution includes the following steps:

[0009] (1) Preheating argon: Add high-purity iron powder into the powder spraying system and preheat the argon gas for spraying;

[0010] (2) Stopper rod argon blowing: Turn on the argon switch before the ladle is poured during the continuous casting process to blow argon into the stopper rod, but do not spray iron powder;

[0011] (3) Iron powder spraying: When the molten steel is poured in the tundish, the powder spraying system is turned on to start spraying iron powder. The iron powder is sprayed out from the plug rod tip along with the argon gas, mixed with the steel flow, and enters the crystallizer through the submerged nozzle and is evenly dissolved in the molten steel.

[0012] (4) Refinement of the solidification structure of the continuous casting billet: Continuously spraying iron powder generates a large amount of dispersed fine iron powder in the crystallizer to form a nucleation core, completing the refinement of the solidification structure of the continuous casting billet;

[0013] (5) End of powder spraying: Before the end of casting, turn off the powder spraying carrier gas and end the iron powder spraying.

[0014] Furthermore, the particle size of the high-purity iron powder in step (1) is ≥400 mesh.

[0015] Furthermore, the preheating temperature of the argon gas in step (1) is 200-300°C.

[0016] Furthermore, the stopper rod in step (2) is a single-hole argon-blown stopper rod, the diameter of the hole on the stopper rod for powder spraying is 0.1-5.0 mm, and the argon gas flow rate is 0.2-0.5 m 3 / h.

[0017] Furthermore, in step (3), the temperature of the tundish is 1520-1550° C., and the amount of iron powder sprayed is 0.01-0.1 kg / t steel.

[0018] Furthermore, the powder spraying system in step (3) adopts a dense phase pneumatic conveying method, and the solid-gas ratio ranges from 30 to 60.

[0019] Working principle of the present invention: The argon preheating and powder spraying system in the present invention is an existing device, and the stopper rod is an existing spare part. Its main function in the continuous casting process is to control the flow state and injection speed of molten steel. It is an important device for controlling steel pouring during the continuous casting process. See the schematic diagram of the high-purity iron powder spraying process and the argon blowing stopper rod structure diagram for details. Figure 1 , Figure 2 During the casting process, preheated argon is used to adopt the method of dense phase pneumatic conveying to spray high-purity iron powder into the space between the stopper rod and the upper nozzle of the tundish through the inner cavity of the argon-blown stopper rod. The iron powder is mixed with the molten steel flowing downward from the bowl mouth, and enters the crystallizer through the immersed nozzle along with the steel flow, and is evenly dissolved in the molten steel. Part of it enters the molten steel to form a solidification nucleation core. Partial melting can reduce the superheat of the molten steel in the crystallizer, promote the nucleation of grains, and inhibit the growth of grains, thereby optimizing the solidification structure of the continuous casting billet.

[0020] Beneficial effects:

[0021] (1) The present invention significantly reduces the center segregation of the ingot by spraying high-purity iron powder as a pre-nucleating agent. The center segregation of the obtained Q460C ingot is Class C Level 1, without center porosity and middle cracks. The center segregation of the Q345B ingot is Class C Level 0.5, without center porosity. The internal density of the ingot and the mechanical properties of the steel are improved. The obtained steel is uniform and dense, and the porosity and segregation are well controlled.

[0022] (2) Compared with the second phase particles, the iron content of the iron powder used in the present invention is ≥99%, and no other impurities are introduced, which can effectively reduce the pollution of molten steel; the particle size of the high-purity iron powder is ≥400 mesh, and the fine iron powder is dispersed in large quantities in the crystallizer, which can quickly form a nucleation core, and the iron powder is low in price, which reduces costs.

[0023] (3) The melting of part of the injected high-purity iron powder can reduce the superheat of the molten steel in the crystallizer, accelerate the solidification rate, increase the utilization rate of the particles, and achieve better grain refinement, which can significantly improve the quality of the continuous casting billet.

[0024] (4) The structure of the spraying system is simple, the spraying volume and spraying speed are easy to adjust, the equipment is easy to maintain, and the operating cost is low. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 This is a schematic diagram of the high-purity iron powder injection process;

[0026] Figure 2 This is the structural diagram of the argon blowing plug rod;

[0027] Figure 3 This is a low-magnification quality observation image of the Q460C ingot obtained in Example 1;

[0028] Figure 4 This is a low-magnification quality observation image of the Q460C ingot obtained in Comparative Example 1;

[0029] Figure 5 This is a low-magnification quality observation image of the Q345B ingot obtained in Example 2;

[0030] Figure 6 This is a low-magnification quality observation image of the Q345B ingot obtained in Comparative Example 2. DETAILED DESCRIPTION

[0031] In order to enable those skilled in the art to better understand the technical solutions in the present invention, the technical solutions in the embodiments of the present invention will be specifically described below in conjunction with the embodiments of the present invention. The described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention.

[0032] Example 1

[0033] The smelting steel grade is Q460C, with a specification of 250mm×1820mm. The composition of Q460C by weight is C: 0.160%, Si: 0.333%, Mn: 1.516%, P: 0.018%, S: 0.010%, Als: 0.028%, and the balance is iron and inevitable impurities. Its main process flow is converter smelting, LF refining, VD vacuum treatment, and continuous casting. During the continuous casting of molten steel, high-purity iron powder is sprayed using argon plug rods. The specific operation steps are as follows:

[0034] (1) Preheating argon: Add high-purity iron powder with an iron content of 99.26% and a particle size of 400 mesh into the powder spraying system, and preheat the argon gas for spraying at a preheating temperature of 250°C;

[0035] (2) Argon blowing with stopper rod: Turn on the argon control switch before pouring the ladle, and use a single-hole argon blowing stopper rod with a powder spraying aperture of 2 mm to blow argon. The argon flow rate is 0.35m 3 / h, but without spraying iron powder;

[0036] (3) Iron powder spraying: When the tundish with a temperature of 1531°C begins to pour the molten steel, the powder spraying system starts to spray iron powder, using dense phase pneumatic conveying, a solid-gas ratio of 40, and an iron powder addition amount of 0.022 kg / t steel. The iron powder is sprayed out from the plug rod tip along with argon gas, mixed with the steel flow, and enters the crystallizer through the submerged nozzle, where it is evenly dissolved in the molten steel.

[0037] (4) Refinement of the solidification structure of the continuous casting billet: Continuously spraying iron powder generates a large amount of dispersed fine iron powder in the crystallizer to form a nucleation core, completing the refinement of the solidification structure of the continuous casting billet;

[0038] (5) End of powder spraying: Before the end of casting, turn off the powder spraying carrier gas and end the iron powder spraying.

[0039] Comparative Example 1

[0040] The steel grade to be smelted is Q460C, with a specification of 250mm×1820mm. The composition of Q460C is C: 0.160%, Si: 0.333%, Mn: 1.516%, P: 0.018%, S: 0.010%, Als: 0.028% by weight, and the balance is iron and inevitable impurities. Its main process flow is converter smelting, LF refining, VD vacuum treatment, and continuous casting. The composition and smelting process flow of Q460C in this comparative example are the same as those in Example 1, except that high-purity iron powder is not sprayed during the continuous casting process.

[0041] The quality of the Q460C ingots obtained in Example 1 and Comparative 1 was observed at low magnification. Figure 3 As shown, the central segregation of the Q460C ingot obtained in Example 1 is Class C 1, with no central porosity and intermediate cracks; Figure 4 As shown, the central segregation of the Q460C ingot obtained in Comparative Example 1 is Class C 2.0, the central porosity is 0.5, and the middle crack is 0.5. It can be seen that the present invention reduces the central segregation of the Q460C ingot by spraying high-purity iron powder as a pre-nucleating agent, improves the internal density of the ingot and the mechanical properties of the steel.

[0042] Example 2

[0043] The smelting steel is Q345B, with a specification of 250mm×1820mm. The composition of Q345B is C: 0.180%, Si: 0.23%, Mn: 1.44%, P: 0.016%, S: 0.002%, Als: 0.03% by weight, and the balance is iron and inevitable impurities. The main process flow is converter smelting, LF refining, VD vacuum treatment, and continuous casting. During the continuous casting of molten steel, high-purity iron powder is sprayed using argon plug rods. The specific operation steps are as follows:

[0044] (1) Preheating argon: Add high-purity iron powder with an iron content of 99.29% and a particle size of 400 mesh into the powder spraying system, and preheat the argon gas for spraying at a preheating temperature of 260°C;

[0045] (2) Stopper rod argon blowing: Turn on the argon control switch before the ladle is poured during the continuous casting process, and use a single-hole argon blowing stopper rod with a powder spraying hole diameter of 2 mm to blow argon. The argon flow rate is 0.4m 3 / h, but without spraying iron powder;

[0046] (3) Iron powder spraying: When the tundish with a temperature of 1540°C begins to pour the molten steel, the powder spraying system starts to spray iron powder, using dense phase pneumatic conveying, with a solid-gas ratio of 38 and an iron powder addition amount of 0.018 kg / t steel. The iron powder is sprayed out from the plug rod tip along with argon gas, mixed with the steel flow, and enters the crystallizer through the submerged nozzle, where it is evenly dissolved in the molten steel.

[0047] (4) Refinement of the solidification structure of the continuous casting billet: Continuously spraying iron powder generates a large amount of dispersed fine iron powder in the crystallizer to form a nucleation core, completing the refinement of the solidification structure of the continuous casting billet;

[0048] (5) End of powder spraying: Before the end of casting, turn off the powder spraying carrier gas and end the iron powder spraying.

[0049] Comparative Example 2

[0050] The smelting steel is Q345B, with a specification of 250mm×1820mm. The composition of Q345B is C: 0.180%, Si: 0.23%, Mn: 1.44%, P: 0.016%, S: 0.002%, Als: 0.03% by weight, and the balance is iron and inevitable impurities. Its main process flow is converter smelting, LF refining, VD vacuum treatment, and continuous casting. The composition and smelting process flow of Q345B in this comparative example are the same as those in Example 2, except that high-purity iron powder is not sprayed and added during the continuous casting process.

[0051] The Q345B ingots obtained in Example 2 and Comparative Example 2 were observed at low magnification. Figure 5 As shown, the center segregation of the Q345B ingot obtained in Example 2 is Class C 0.5, and there is no center porosity; Figure 6 As shown, the center segregation of the Q345B ingot obtained in Comparative Example 2 is Class C 2.0, and the center porosity is 0.5. It can be seen that the present invention reduces the center segregation and center porosity of the Q345B ingot by spraying high-purity iron powder as a pre-nucleating agent, improves the internal density of the ingot and the mechanical properties of the steel, and the obtained Q345B steel is uniform and dense, and the porosity and segregation are well controlled.

Claims

1. A method for controlling the internal quality of continuous casting billets based on preset nucleation, characterized in that During the molten steel casting process, preheated argon is used to blow high-purity iron powder with an iron content of ≥99% through an argon plug rod. The iron powder is sprayed out with the argon and mixed with the steel flow and enters the crystallizer through the submerged nozzle to form a fine and dispersed nucleation core, completing the refinement of the solidification structure of the continuous casting billet.

2. The method for controlling the internal quality of continuous casting slab according to claim 1, characterized in that: The method comprises the following steps: (1) Preheating argon: Add high-purity iron powder into the powder spraying system and preheat the argon gas for spraying; (2) Stopper rod argon blowing: Turn on the argon switch before the ladle is poured during the continuous casting process to blow argon into the stopper rod, but do not spray iron powder; (3) Iron powder spraying: When the molten steel is poured in the tundish, the powder spraying system is turned on to start spraying iron powder. The iron powder is sprayed out from the plug rod tip along with the argon gas, mixed with the steel flow, and enters the crystallizer through the submerged nozzle and is evenly dissolved in the molten steel. (4) Refinement of the solidification structure of the continuous casting billet: Continuously spraying iron powder generates a large amount of dispersed fine iron powder in the crystallizer to form a nucleation core, completing the refinement of the solidification structure of the continuous casting billet; (5) End of powder spraying: Before the end of casting, turn off the powder spraying carrier gas and end the iron powder spraying.

3. The method for controlling the internal quality of continuous casting slab according to claim 2, characterized in that: The high purity iron powder in step (1) has a particle size of ≥400 mesh.

4. The method for controlling the internal quality of continuous casting slab according to claim 2, characterized in that: The preheating temperature of the argon gas in step (1) is 200-300°C.

5. The method for controlling the internal quality of continuous casting slab according to claim 2, characterized in that: The stopper rod in step (2) is a single-hole argon-blown stopper rod, the diameter of the hole on the stopper rod for powder spraying is 0.1-5.0 mm, and the argon gas flow rate is 0.2-0.5 m 3 / h.

6. The method for controlling the internal quality of continuous casting slab according to claim 2, characterized in that: In step (3), the temperature of the tundish is 1520-1550°C, and the iron powder spraying amount is 0.01-0.1 kg / t steel.

7. The method for controlling the internal quality of continuous casting slab according to claim 2, characterized in that: The powder spraying system in step (3) adopts dense phase pneumatic conveying, and the solid-gas ratio ranges from 30 to 60.

Citation Information

Patent Citations

  • Method for refining continuous casting billet solidification structure by blowing magnesium powder through submerged nozzle

    CN111451462A

  • Powdered iron core-covered wire for smelting steel

    CN1380427A