Improved smelting and preparation method of aluminum-silicon alloy casting

By adopting the quantitative ratio of near/overeutectic aluminum-silicon alloy and pure aluminum in the production of aluminum silicon alloy castings, the weight melting amount of aluminum matrix is ​​reduced, and the problems of high energy consumption and carbon emissions in the production of aluminum silicon alloy castings are solved, thus achieving the goal of achieving high energy consumption and carbon emissions. It has low cost, low consumption and low emission production results, and is suitable for the development of recycled aluminum alloys.

CN118910444APending Publication Date: 2024-11-08CITIC DICASTAL CO LTD +1
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411269069.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-11
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The high energy consumption and carbon emission problems caused by repeated melting of aluminum matrix in the production of aluminum silicon alloy castings. The traditional preparation methods have problems such as high labor intensity, high cost, and large equipment investment, and the recycled aluminum treatment technology is immature.

Method used

The near/overeutectic aluminum-silicon alloy is used as the intermediate alloy and the quantitative ratio with pure aluminum. The subeutectic aluminum-silicon alloy of the target component is obtained through a series of smelting processes, and the castings are directly produced, reducing the weight melting of aluminum matrix, reducing energy consumption and Carbon emissions and are suitable for existing equipment conditions, suitable for the development of recycled aluminum alloys.

Benefits of technology

It effectively reduces the weight melting amount of aluminum matrix, reduces energy consumption and carbon emissions, reduces production costs, improves production efficiency, is suitable for the development of recycled aluminum alloys, makes up for the shortcomings of traditional processes, and is in line with the theme of green and low-carbon development.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118910444A_ABST
    Figure CN118910444A_ABST
Patent Text Reader

Abstract

The invention discloses an improved smelting and preparation method of an aluminum-silicon alloy casting. Relates to the technical field of aluminum-silicon alloy casting production, and the method comprises the following steps: taking a near / hypereutectic aluminum-silicon alloy Al-xSi (10 < = x < = 22) cast ingot as an aluminum-silicon intermediate alloy, putting the aluminum-silicon intermediate alloy and a pure aluminum ingot according to a certain ratio (1: a) in a casting processing factory, heating and melting, adding pure magnesium, Al-Ti-B, Al-Sr and the like to carry out molten aluminum component adjustment and melt transformation, and carrying out melt transformation to obtain the aluminum-silicon alloy casting. And after the components of the molten aluminum are qualified, the molten aluminum is subjected to the processes of standing, refining, degassing and the like, and then subsequent processing such as casting forming and the like is directly carried out, so that the production process is simplified by reducing repeated melting of an aluminum matrix in the casting production process, the energy consumption is saved, the carbon emission is reduced, and the production cost is reduced. And the method can be directly applied to equipment conditions of current production lines, is wide in application range, is particularly suitable for development and application of regenerated high-silicon aluminum alloy, does not need extra investment, and is beneficial to industrial popularization.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of aluminum-silicon alloy casting production, and in particular to an improved method for smelting and preparing aluminum-silicon alloy castings. Background Art

[0002] Cast aluminum silicon alloy is an alloy with aluminum and silicon (4%-22% Si) as the main components. It has the characteristics of light weight, high specific strength, good thermal conductivity, wear resistance, corrosion resistance, and good casting performance. It is widely used in automobile manufacturing, machinery manufacturing and other fields. With the rise of the new energy vehicle market and the development of lightweight vehicles, my country's cast aluminum silicon alloy industry has shown an increasing demand and positive development trend.

[0003] At present, the aluminum-silicon alloy casting industry has a mature industrial chain of upstream smelting, midstream processing and downstream application. According to production statistics, the comprehensive energy consumption of natural gas required to melt 1 ton of aluminum is about 60-100m 3 According to national energy statistics, carbon emissions per cubic meter of natural gas is about 2.16kgCO2. At the same time, with the advancement of the country's "dual carbon" policy, green, low-carbon, energy-saving and environmentally friendly sustainable development models have become the theme, such as limiting the production capacity of electrolytic aluminum, promoting direct alloying of aluminum liquid, and promoting the application of recycled aluminum. The country also encourages enterprises to coordinate energy and resource conservation and comprehensive utilization, and promote the promotion and application of new technologies and new materials.

[0004] There is still room for improvement in my country's casting aluminum-silicon alloy industry. On the one hand, the traditional preparation of aluminum-silicon alloy ingots generally involves adding pure aluminum ingots to a smelting furnace first, and then adding alloying elements such as silicon after the aluminum ingots are heated and melted to 730-760°C. After all the components are prepared, they are cast into ingots. The ingots are then transported to the processing plant, where they are remelted for processing and production. The traditional preparation method produces 100 units of Al-ySi castings, and the amount of aluminum remelted is (100-y)×2. Direct alloying of aluminum water can reduce the repeated melting of the aluminum matrix by 50%, but this has geographical limitations close to the electrolytic aluminum plant, and requires a certain amount of investment in plant construction and construction land planning, etc. Therefore, there is still a considerable amount of alloy ingots in China that use traditional preparation processes. In addition, due to market factors, some of the purchased international A00 pure aluminum raw materials have the phenomenon of high quality and low price.

[0005] On the other hand, the development trend of recycled aluminum is unstoppable, but the overall recycled aluminum processing technology in my country is not mature, the scale of recycled aluminum enterprises is small, and there are certain restrictions on the recycling of waste materials and production and sales (currently, the recycled aluminum waste in my country is mainly aluminum-silicon alloy). Generally, the recycled waste is alloyed and cast into ingots after pretreatment and other processes; then the alloy ingots are transported to the processing plant for remelting and casting production. At present, the recycled high-silicon aluminum alloy produced by some companies needs to be cast after adding pure aluminum to make a low-silicon alloy, and then remelted in the processing plant, which increases the amount of aluminum remelting and energy consumption.

[0006] Therefore, based on the high energy consumption and high carbon emission caused by repeated melting of the aluminum matrix of aluminum-silicon alloy castings and the current status of domestic industrial production, there is a need for an industrial smelting and preparation method of energy-saving and emission-reducing aluminum-silicon alloy castings with "low input, low consumption, low emissions and high efficiency". Summary of the invention

[0007] The purpose of the present invention is to propose an improved smelting and preparation method of aluminum-silicon alloy castings, which can effectively reduce the remelting amount of aluminum matrix, save energy consumption, reduce carbon emissions, improve the production process, and be directly applied to the equipment and process conditions of various current production lines.

[0008] In order to solve the above problems, the technical solution of the present invention is: an improved method for smelting and preparing aluminum-silicon alloy castings, using near / hypereutectic aluminum-silicon alloy (Al-xSi: 10≤x≤22) ingot as the master alloy, quantitatively proportioning the master alloy and pure aluminum according to the feed ratio of 1:a (0≤a≤4.5), obtaining the required hypoeutectic aluminum-silicon alloy (Al-ySi: 4≤y≤10) target component aluminum liquid through a series of smelting processes, and then directly carrying out subsequent production of castings, which specifically includes the following steps: (1) Determine the target composition Al-ySi alloy according to the casting standard, determine the ratio of the master alloy to pure aluminum as 1:a, and then determine the composition of the Al-xSi master alloy, where x=(1+a)×y. Control the content of each element in the master alloy according to the target composition and feed ratio to obtain the master alloy ingot; (2) The melting furnace temperature is 730-750°C, the intermediate alloy ingot and pure aluminum are quantitatively put into the material tower / melting continuous production furnace group, the content of the main alloy elements is detected and controlled, and the aluminum liquid is introduced into the static furnace; (3) The temperature of the static furnace is 730-750°C. After the aluminum liquid is introduced into the static furnace, it is melt treated to control the content of the main alloy elements to be qualified, and the aluminum liquid is introduced into the transfer ladle; (4) The aluminum liquid in the ladle is transferred for refining, degassing and slag removal. The smelting process ends after the alloy composition is tested to be qualified; (5) The aluminum liquid becomes a commercial casting after die casting, heat treatment, machining and qualified testing; Production process control and finished product performance testing of aluminum-silicon alloy castings: Through casting X-ray yield, mechanical properties, and reliability tests, the industrial smelting and preparation methods of aluminum-silicon alloy castings are monitored in real time and the feasibility is verified.

[0009] Furthermore, using near / hypereutectic aluminum-silicon alloy (Al-xSi: 12≤x≤20) ingot as the intermediate alloy, the intermediate alloy and pure aluminum are quantitatively proportioned according to the feed ratio of 1:a (0.5≤a≤3), and after a series of smelting processes to obtain the required hypoeutectic aluminum-silicon alloy (Al-ySi: 5≤y≤8) target composition aluminum liquid, subsequent production of castings is directly carried out to obtain hypoeutectic aluminum-silicon alloy castings, and the hypoeutectic aluminum-silicon alloy castings include A355, A356, and A357.

[0010] Furthermore, the target alloy composition was selected as A356 (Al-7Si alloy), with the main element content standards of 6.5-7.5% Si, 0.25-0.45% Mg, 0.1-0.15% Ti, ≤0.15% Fe and no more than 0.05% impurity elements, and the rest being Al.

[0011] Furthermore, in step (1), the feed ratio of the master alloy to the pure aluminum is determined to be 1:1. The main element content of the master alloy obtained according to the 1:1 ratio is theoretically 13-15% Si, 0.5-0.9% Mg, 0.2-0.3% Ti, ≤0.3% Fe and no more than 0.05% impurity elements, and the rest is Al; According to the actual smelting process: the elements that are not easy to burn out are controlled to 13.5-14.5% Si and 0.2-0.26% Ti; the lower limit of the element Mg that is easy to burn out is controlled to 0.5-0.56%; the harmful element Fe is ≤0.22%.

[0012] Furthermore, in step (2), pure aluminum and the intermediate alloy are added cyclically in proportion, with pure aluminum being added first and the intermediate alloy being added second, and the single amount of each alloy added is not more than 1000 kg; aluminum ingots are added to 90% of the aluminum liquid capacity of the melting furnace, stirred, and the composition is measured to ensure that Si, Ti, and Fe are qualified, and the adjustment amount of Mg is calculated.

[0013] Furthermore, when the aluminum liquid from the melting furnace is poured into the static furnace in step (2), the easily burnable element Mg is added in the form of pure Mg blocks (≥99.5%) and placed in the launder between the melting furnace and the static furnace.

[0014] Furthermore, in step (3), the aluminum liquid in the static furnace is allowed to stand for at least 60 minutes to ensure that Si, Mg, Ti and Fe are qualified; the addition amount of Al-Sr10 modifier rod and Al-5Ti-B refiner rod used for melt modification is 0.2% of the mass of aluminum liquid in the ladle, and they are placed in the flow channel between the static furnace and the transfer ladle.

[0015] Furthermore, in step (4), Si, Mg, Ti, Fe and Sr need to be tested and qualified.

[0016] Furthermore, according to the method, the remelting amount of aluminum matrix to produce Al-ySi castings (based on 100 unit mass) with the intermediate alloy and pure aluminum in a 1:a ratio is: [100 / (1+a)-y]×2+{(100-y)-[100 / (1+a)-y]}=(100-y)+[100 / (1+a)-y]; the remelting amount of aluminum to produce Al-ySi castings by traditional preparation methods or recycled aluminum-silicon alloys is: (100-y)×2; therefore, for every 100 unit mass of Al-ySi castings produced, the remelting amount of aluminum can be reduced by: (100-y)-[100 / (1+a)-y].

[0017] Furthermore, based on the production of 100 unit mass of castings: when the intermediate alloy Al-22Si and pure aluminum are matched with Al-4Si alloy in a ratio of 1:4.5, the reduced remelting amount of the aluminum matrix is ​​about 81.8 unit mass, and the reduction ratio is 42.6%; when the intermediate alloy Al-14Si and pure aluminum are matched with Al-7Si alloy in a ratio of 1:1, the reduced remelting amount of the aluminum matrix is ​​about 50 unit mass, and the reduction ratio is 26.8%.

[0018] The beneficial effects achieved by the present invention are as follows: (1) Based on the current status of aluminum casting processing in China, compared with the traditional preparation process, the present method can directly switch with the existing equipment conditions, reduce the amount of aluminum melted in the alloy ratio, reduce labor intensity, and reduce labor costs. Taking the production of 100 units of castings as an example, the amount of aluminum remelting can be reduced by (100-y)-[100 / (1+a)-y]: Specifically, for the production of 100,000 tons of A356 castings, the 1:1 ratio process can reduce about 50,000 tons of aluminum remelting and about 3-5 million cubic meters of natural gas; (2) Compared with the direct alloying measures of molten aluminum, the present method is not limited by additional investment in new plant / equipment and geographical factors, and can achieve low-cost reduction of aluminum remelting, with the highest reduction ratio reaching 42.6%; (3) At present, there is still a considerable amount of aluminum alloy ingots prepared and processed in China using traditional processes, which are difficult to be completely replaced within a period of time. This method The proposed method makes up for the shortcomings of these output energy conservation and emission reduction, and is a reasonable supplement to the existing technology; (4) This method is suitable for the development and application of recycled aluminum alloys, which can further reduce carbon emissions, and is particularly suitable for the development and application of recycled high-silicon aluminum alloys; (5) This method can improve the tolerance of aluminum-silicon alloy ingots to harmful elements Fe, and is particularly suitable for the development and application of recycled aluminum-silicon alloys, which is conducive to reducing production difficulty and cost, and is an effective improvement to the existing technology; (6) This method reduces the remelting of aluminum by integrating industrial chain resources and production processes, and has the characteristics of low cost, low consumption and low emissions, which promotes the structural optimization and upgrading of the industry and complies with national policies and the theme of green development; (7) This method has been batch verified in the casting production line, using recycled or non-recycled high-silicon aluminum ingot ratios, with stable production efficiency and stable yield, reduced energy consumption, and has practical applicability and promotion feasibility. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1 This is the aluminum-silicon binary phase diagram.

[0020] Figure 2 (A) is a schematic diagram of the ingot remelting process for producing traditional aluminum-silicon alloy castings; (B) is a schematic diagram of the ingot remelting process for producing non-regenerative aluminum-silicon alloy castings using this method.

[0021] Figure 3 (A) is a schematic diagram of the ingot remelting process for the current production of recycled aluminum-silicon alloy castings; (B) is a schematic diagram of the ingot remelting process for the production of recycled aluminum-silicon alloy castings using this method.

[0022] Figure 4 Schematic diagram of the A356 casting production process.

[0023] Figure 5 This is a schematic diagram of the production furnace group for the smelting process. DETAILED DESCRIPTION

[0024] The following description is used to explain the technical solution of the present invention so that those skilled in the art can implement the present invention. The preferred embodiments described below are only examples, and those skilled in the art can think of other obvious variations. The basic principles of the present invention defined in the following description can be applied to other implementation schemes, variations, improvements, equivalent solutions, and other technical solutions that do not deviate from the spirit and scope of the present invention. At the same time, it is worth noting that the features or characteristics described in the text in conjunction with a certain embodiment are not necessarily limited to this specific embodiment, nor are they mutually exclusive with other embodiments. Within the scope of the capabilities of those skilled in the art, different combinations of various features in different embodiments can be considered.

[0025] By introducing the intermediate alloy ingot, and then remelting it with pure aluminum, the casting can be directly processed, which can reduce the remelting of aluminum at a low cost and achieve the effect of energy saving and emission reduction. The following will further explain the two preparation methods of aluminum-silicon intermediate alloy ingots (traditional preparation and recycled preparation).

[0026] According to the improved smelting and preparation method of aluminum-silicon alloy castings implemented by the present invention, the traditional preparation process is improved, which can effectively reduce the amount of aluminum matrix remelting, save energy consumption, reduce carbon emissions, improve the production process, and be directly applied to the equipment and process conditions of various current production lines. Compared with the direct alloying of molten aluminum to reduce aluminum remelting by 50%, this method has no restrictions such as additional investment in new plants / equipment and geographical factors, and can achieve low-cost reduction of aluminum remelting, with the highest reduction ratio reaching 42.6%. In addition, there is still a considerable amount of aluminum alloy ingots prepared and processed in China using traditional processes, which are difficult to be completely replaced. The proposal of this method makes up for the shortcomings of these production energy conservation and emission reduction, and is a reasonable supplement to the existing technology.

[0027] According to the improved aluminum-silicon alloy casting smelting and preparation method implemented by the present invention, in view of the current situation that the social recycling and reprocessing technology of waste aluminum is immature, it is difficult for casting processing plants to process it by themselves, forming an industrial model of direct application of molten aluminum, and the technical barriers of waste aluminum recycling are high and the investment consumption is large. Therefore, this method is suitable for the application and improvement of the current recycled aluminum technology, which is in line with the development trend. At the same time, this method improves the tolerance of aluminum-silicon alloy ingots to harmful elements Fe, and is particularly suitable for the development and application of recycled casting high-silicon aluminum alloys. It is also conducive to reducing production difficulty and cost, and is an effective improvement to the application of existing technologies.

[0028] Figure 1 The Al-Si phase diagram provides support for the implementation of the method. The silicon content range of the intermediate aluminum-silicon alloy Al-xSi is determined according to the liquidus temperature curve to suit existing equipment, process and other conditions, while also including the alloy range of aluminum-silicon recycled materials. Figure 2 (A) is a schematic diagram of the ingot remelting process for the production of traditional aluminum-silicon alloy castings; Figure 2 (B) is a schematic diagram of the ingot remelting process for producing non-regenerated aluminum-silicon alloy castings using this method; the comparative advantages are obvious. Figure 3 (A) is a schematic diagram of the ingot remelting process for the current production of recycled aluminum-silicon alloy castings; Figure 3 (B) is a schematic diagram of the ingot remelting process for producing recycled aluminum-silicon alloy castings using this method; the comparative advantages are obvious. Figure 4 It is a schematic diagram of the production process of A356 castings in a specific embodiment. Figure 5 This is a schematic diagram of the continuous production furnace group for smelting of the A356 casting production line, in which the aluminum chip furnace is used to recycle aluminum chips such as machining waste chips in the processing workshop.

[0029] An improved smelting and preparation method for aluminum-silicon alloy castings, using near / hypereutectic aluminum-silicon alloy (Al-xSi: 10≤x≤22) ingots as master alloys, quantitatively proportioning the master alloys with pure aluminum according to a feed ratio of 1:a (0≤a≤4.5), obtaining the required hypoeutectic aluminum-silicon alloy (Al-ySi: 4≤y≤10) target composition aluminum liquid through a series of smelting processes, and then directly carrying out subsequent production of castings, specifically comprising the following steps: (1) Determine the target composition Al-ySi alloy according to the casting standard, determine the ratio of the master alloy to pure aluminum as 1:a, and then determine the composition of the Al-xSi master alloy, where x = (1 + a) × y. Control the content of each element in the master alloy according to the target composition and feed ratio to obtain the master alloy ingot. The master alloy ingot is prepared by two methods: traditional process and aluminum-silicon alloy recycled material regeneration process.

[0030] (2) The temperature of the melting furnace is 730-750℃. The intermediate alloy ingots and pure aluminum are quantitatively fed into the material tower / melting continuous production furnace group. The content of the main alloy elements is detected and controlled, and the aluminum liquid is introduced into the static furnace. Specifically, pure aluminum and intermediate alloy are cyclically fed in proportion, with pure aluminum being given priority, followed by intermediate alloy. The single amount of each alloy fed is not more than 1000 kg. Aluminum ingots are fed into the 90% capacity of the aluminum liquid in the melting furnace, stirred, and the composition is measured to ensure that Si, Ti, and Fe are qualified, and the adjustment amount of Mg is calculated. When the aluminum liquid from the melting furnace is poured into the static furnace, the easily burnt element Mg is added in the form of pure Mg blocks (≥99.5%) and placed in the flow channel between the melting furnace and the static furnace.

[0031] (3) The temperature of the standing furnace is 730-750℃. After the aluminum liquid is introduced into the standing furnace, it is melt treated to control the content of the main alloy elements to be qualified, and then the aluminum liquid is introduced into the transfer ladle. Specifically, the aluminum liquid in the standing furnace is allowed to stand for at least 60 minutes to ensure that Si, Mg, Ti, and Fe are qualified. The addition amount of Al-Sr10 modifier rod and Al-5Ti-B refiner rod used for melt modification is 0.2% of the mass of the aluminum liquid in the ladle, and they are placed in the flow channel between the standing furnace and the transfer ladle.

[0032] (4) The aluminum liquid in the ladle is transferred for refining, degassing and slag removal. The smelting process is completed after the alloy composition is tested and qualified; specifically, Si, Mg, Ti, Fe and Sr need to be tested and qualified.

[0033] (5) The aluminum liquid becomes a commercial casting after die casting, heat treatment, machining and qualified testing; Production process control and finished product performance testing of aluminum-silicon alloy castings: X-ray yield, mechanical properties, reliability testing of castings, real-time monitoring and feasibility verification of industrial smelting and preparation methods of aluminum-silicon alloy castings.

[0034] A near / hypereutectic aluminum-silicon alloy (Al-xSi: 12≤x≤20) ingot is used as an intermediate alloy, the intermediate alloy and pure aluminum are quantitatively proportioned according to a feed ratio of 1:a (0.5≤a≤3), and after a series of smelting processes, the required hypoeutectic aluminum-silicon alloy (Al-ySi: 5≤y≤8) target composition aluminum liquid is obtained, and then subsequent casting production is directly carried out to obtain hypoeutectic aluminum-silicon alloy castings, and the hypoeutectic aluminum-silicon alloy castings include A355, A356, and A357.

[0035] The production raw materials and preparation process of the intermediate aluminum-silicon alloy ingot mainly include the following two types: 1. Traditional preparation process, industrial pure aluminum + industrial pure silicon + other alloy preparation; 2. Recycled aluminum preparation process, recycled waste processing + other alloy preparation; According to the method, the intermediate alloy and pure aluminum are mixed in a ratio of 1:a to produce the aluminum matrix remelting amount of Al-ySi castings (based on 100 unit mass): [100 / (1+a)-y]×2+{(100-y)-[100 / (1+a)-y]}=(100-y)+[100 / (1+a)-y]; The aluminum remelting amount of Al-ySi castings produced by the traditional preparation method or recycled aluminum-silicon alloy is: (100-y)×2; therefore, for every 100 unit mass of Al-ySi castings produced, the aluminum remelting amount can be reduced: (100-y)-[100 / (1+a)-y].

[0036] Based on the production of 100 units of castings: when the intermediate alloy Al-22Si and pure aluminum are matched in a ratio of 1:4.5 to Al-4Si alloy, the reduced remelting amount of the aluminum matrix is ​​about 81.8 units of mass, and the reduction ratio is 42.6%; when the intermediate alloy Al-14Si and pure aluminum are matched in a ratio of 1:1 to Al-7Si alloy, the reduced remelting amount of the aluminum matrix is ​​about 50 units of mass, and the reduction ratio is 26.8%.

[0037] The present method is specifically described below by means of specific Example 1, and is analyzed and verified by subsequent examples and comparative examples.

[0038] Embodiment 1: An improved method for smelting and preparing aluminum-silicon alloy castings, comprising the following steps: (1) The composition standard of the casting product is determined to be A356 (Al-7Si alloy), and the main element content standard is 6.5-7.5% Si, 0.25-0.45% Mg, 0.1-0.15% Ti, ≤0.15% Fe and no more than 0.05% impurity elements, and the rest is Al; the ratio with pure aluminum is determined to be 1:1, and the Al-14Si master alloy is obtained according to the 1:1 ratio and the actual smelting process, and its main element content is controlled to be 13.5-14.5% Si, 0.5-0.56% Mg, 0.2-0.26% Ti, ≤0.22% Fe and other impurity elements no more than 0.05%; the aluminum-silicon master alloy is prepared by traditional technology (prepared by 43 units of pure Al + 7 units of industrial pure Si, etc.).

[0039] (2) The temperature of the melting furnace is 730-750℃, and pure aluminum and aluminum-silicon alloy ingots are put in a 1:1 cycle. 500kg of pure aluminum is put in first, and then 500kg of aluminum-silicon alloy ingots are put in. The aluminum ingots are put into 90% of the capacity of the melting furnace. The aluminum liquid is stirred and the composition is measured. If Si, Ti and Fe are qualified, the adjustment amount of Mg is calculated, and the pure Mg block is placed in the flow channel between the melting furnace and the standing furnace. The aluminum liquid is then introduced into the standing furnace. The aluminum liquid in the standing furnace is self-treated aluminum liquid without adding waste chips from the factory.

[0040] (3) The temperature of the static furnace is 730-750℃, the aluminum liquid is left to stand for at least 60 minutes, and the Si, Mg, Ti, and Fe are qualified; the Al-Sr10 modifier rod and Al-5Ti-B refiner rod used for melt modification are added in an amount of 0.2% of the mass of the aluminum liquid in the ladle, and are placed in the flow channel between the static furnace and the transfer ladle, and then the aluminum liquid is introduced into the transfer ladle.

[0041] (4) The aluminum liquid in the ladle is transferred for refining, degassing, and slag removal. After the alloy composition is tested and qualified, it is ready to be transferred to the die-casting machine for hydraulic casting.

[0042] (5) The aluminum liquid is processed into finished castings through die casting, heat treatment, machining, painting and other processes. The pass rate of die casting X-ray inspection (full inspection) of process control is 97.3%; the mechanical properties (sampling inspection) YS, UTS, EL results are all qualified, and the specific casting edge performance is YS223MPa, UTS315MPa, EL12.7%; the casting reliability performance (sampling inspection) bench test is qualified, and the specific 13° / 90° impact is qualified, and the radial / bending fatigue is qualified.

[0043] Embodiment 2: An improved method for smelting and preparing aluminum-silicon alloy castings, comprising the following steps: (1) The composition standard of the casting product is determined to be A356 (Al-7Si alloy), and the ratio with pure aluminum is determined to be 1:1. According to the 1:1 ratio and the actual smelting process, the Al-14Si intermediate alloy is obtained, and its main element content is controlled to be 13.5-14.5% Si, 0.5-0.56% Mg, 0.2-0.26% Ti, ≤0.22% Fe and other impurity elements not exceeding 0.05%; the intermediate alloy is prepared by traditional technology (prepared by 43 units of pure Al + 7 units of pure Si, etc.).

[0044] (2) The temperature of the melting furnace is 730-750℃, and pure aluminum and aluminum-silicon alloy ingots are put in a 1:1 cycle. 500kg of pure aluminum is put in first, and then 500kg of aluminum-silicon alloy ingots are put in. Put the aluminum ingots into 90% of the capacity of the melting furnace, stir, measure the composition, and if Si, Ti, and Fe are qualified, calculate the adjustment amount of Mg, put the pure Mg block in the flow channel between the melting furnace and the standing furnace, and then introduce the aluminum liquid into the standing furnace, and at the same time add the self-processed aluminum water such as waste chips in the factory.

[0045] (3) The temperature of the static furnace is 730-750℃, the aluminum liquid is left to stand for at least 60 minutes, and the Si, Mg, Ti, and Fe are qualified; the Al-Sr10 modifier rod and Al-5Ti-B refiner rod used for melt modification are added in an amount of 0.2% of the mass of the aluminum liquid in the ladle, and are placed in the flow channel between the static furnace and the transfer ladle, and then the aluminum liquid is introduced into the transfer ladle.

[0046] (4) The aluminum liquid in the ladle is transferred for refining, degassing, and slag removal. After the alloy composition is tested and qualified, it is ready to be transferred to the die-casting machine for hydraulic casting.

[0047] (5) The aluminum liquid is processed into finished castings through die casting, heat treatment, machining, painting and other processes. The pass rate of die casting X-ray inspection (full inspection) of process control is 97.1%; the mechanical properties (sampling inspection) YS, UTS, EL results are all qualified, and the specific casting edge performance is YS219MPa, UTS311MPa, EL11.9%; the casting reliability performance (sampling inspection) bench test is qualified, and the specific 13° / 90° impact is qualified, and the radial / bending fatigue is qualified.

[0048] Comparative Example 1: A method for smelting and preparing aluminum-silicon alloy castings, comprising the following steps: (1) The composition standard of the casting product is determined to be A356 (Al-7Si alloy), and an A356 alloy ingot is prepared; the A356 alloy ingot is prepared by a traditional process (93 units of pure Al + 7 units of pure Si, etc.).

[0049] (2) The temperature of the melting furnace is 730-750℃. Put the aluminum ingot into the melting furnace to fill 90% of the aluminum liquid. Stir and measure the composition. If Si, Ti and Fe are qualified, calculate the adjustment amount of Mg. Put the pure Mg block in the flow channel between the melting furnace and the standing furnace. Then, introduce the aluminum liquid into the standing furnace. At the same time, add the self-processed aluminum water such as waste chips in the factory.

[0050] (3) The temperature of the static furnace is 730-750℃, the aluminum liquid is left to stand for at least 60 minutes, and the Si, Mg, Ti, and Fe are qualified; the Al-Sr10 modifier rod and Al-5Ti-B refiner rod used for melt modification are added in an amount of 0.2% of the mass of the aluminum liquid in the ladle, and are placed in the flow channel between the static furnace and the transfer ladle, and then the aluminum liquid is introduced into the transfer ladle.

[0051] (4) The aluminum liquid in the ladle is transferred for refining, degassing, and slag removal. After the alloy composition is tested and qualified, it is ready to be transferred to the die-casting machine for hydraulic casting.

[0052] (5) The aluminum liquid is processed into finished castings through die casting, heat treatment, machining, painting and other processes. The pass rate of die casting X-ray inspection (full inspection) of process control is 96.9%; the mechanical properties (sampling inspection) YS, UTS, EL results are all qualified, and the specific casting edge performance is YS218MPa, UTS312MPa, EL12.5%; the casting reliability performance (sampling inspection) bench test is qualified, and the specific 13° / 90° impact is qualified, and the radial / bending fatigue is qualified.

[0053] In order to more clearly show the key preparation parameters and process monitoring of each process of non-regeneration aluminum silicon castings, the embodiments and comparative examples are summarized as follows:

[0054] Embodiment 3: An improved method for smelting and preparing aluminum-silicon alloy castings, comprising the following steps: (1) The composition standard of the casting product is determined to be A356 (Al-7Si alloy), and the ratio with pure aluminum is determined to be 1:1. According to the 1:1 ratio and the actual smelting process, the Al-14Si aluminum-silicon master alloy is obtained, and its main element content is controlled to be 13.5-14.5% Si, 0.5-0.56% Mg, 0.2-0.26% Ti, ≤0.22% Fe and other impurity elements not exceeding 0.05%; the source of social recycled waste aluminum is about Al-18Si, and the aluminum-silicon master alloy is prepared by a regeneration process (that is, processed recycled waste aluminum + pure aluminum, etc., including 43 units of mass Al matrix + 7 units of mass Si).

[0055] (2) The temperature of the melting furnace is 730-750℃, and pure aluminum and aluminum-silicon alloy ingots are put in a 1:1 cycle. 500kg of pure aluminum is put in first, and then 500kg of aluminum-silicon alloy ingots are put in. Put the aluminum ingots into 90% of the capacity of the melting furnace, stir, measure the composition, and if Si, Ti, and Fe are qualified, calculate the adjustment amount of Mg, put the pure Mg block in the flow channel between the melting furnace and the standing furnace, and then introduce the aluminum liquid into the standing furnace, and at the same time add the self-processed aluminum water such as waste chips in the factory.

[0056] (3) The temperature of the static furnace is 730-750℃, the aluminum liquid is left to stand for at least 60 minutes, and the Si, Mg, Ti, and Fe are qualified; the Al-Sr10 modifier rod and Al-5Ti-B refiner rod used for melt modification are added in an amount of 0.2% of the mass of the aluminum liquid in the ladle, and are placed in the flow channel between the static furnace and the transfer ladle, and then the aluminum liquid is introduced into the transfer ladle.

[0057] (4) The aluminum liquid in the ladle is transferred for refining, degassing, and slag removal. After the alloy composition is tested and qualified, it is ready to be transferred to the die-casting machine for hydraulic casting.

[0058] (5) The aluminum liquid is processed by die casting, heat treatment, machining, painting and other processes to become finished castings. The pass rate of die casting X-ray inspection (full inspection) of its process control is 96.9%; the mechanical properties (sampling inspection) YS, UTS, EL results are all qualified, and the specific casting edge performance is YS221MPa, UTS315MPa, EL12.1%; the casting reliability performance (sampling inspection) bench test is qualified, specifically 13° / 90° impact qualified, radial / bending fatigue qualified.

[0059] Embodiment 4: An improved method for smelting and preparing aluminum-silicon alloy castings, comprising the following steps: (1) The composition standard of the casting product is determined to be A356 (Al-7Si alloy), and the ratio of the intermediate alloy to pure aluminum is determined to be 1:1.5. According to the 1:1.5 ratio and the actual smelting process, the Al-17.5Si intermediate alloy is obtained, and its main element content is controlled to be 17-18% Si, 0.6-0.66% Mg, 0.25-0.32% Ti, ≤0.28% Fe and other impurity elements not exceeding 0.05%; the source of social recycled waste aluminum is about Al-18Si, and the intermediate alloy is prepared by a regeneration process (that is, processed recycled waste aluminum + pure aluminum, etc., including 33 units of mass Al matrix + 7 units of mass Si).

[0060] (2) The temperature of the melting furnace is 730-750℃, and pure aluminum and aluminum-silicon alloy ingots are put in a 1.5:1 cycle. 750kg of pure aluminum is put in first, and then 500kg of aluminum-silicon alloy ingots are put in. Put the aluminum ingots into 90% of the capacity of the melting furnace, stir, measure the composition, and if Si, Ti, and Fe are qualified, calculate the adjustment amount of Mg, put the pure Mg block in the flow channel between the melting furnace and the standing furnace, and then introduce the aluminum liquid into the standing furnace, and at the same time add the self-processed aluminum water such as waste chips in the factory.

[0061] (3) The temperature of the static furnace is 730-750℃, the aluminum liquid is left to stand for at least 60 minutes, and the Si, Mg, Ti, and Fe are qualified; the Al-Sr10 modifier rod and Al-5Ti-B refiner rod used for melt modification are added in an amount of 0.2% of the mass of the aluminum liquid in the ladle, and are placed in the flow channel between the static furnace and the transfer ladle, and then the aluminum liquid is introduced into the transfer ladle.

[0062] (4) The aluminum liquid in the ladle is transferred for refining, degassing, and slag removal. After the alloy composition is tested and qualified, it is ready to be transferred to the die-casting machine for hydraulic casting.

[0063] (5) The aluminum liquid is processed into finished castings through die casting, heat treatment, machining, painting and other processes. The pass rate of die casting X-ray inspection (full inspection) of process control is 97.1%; the mechanical properties (sampling inspection) YS, UTS, EL results are all qualified, and the specific casting edge performance is YS218MPa, UTS308MPa, EL12.0%; the casting reliability performance (sampling inspection) bench test is qualified, and the specific 13° / 90° impact is qualified, and the radial / bending fatigue is qualified.

[0064] Comparative Example 2: A method for smelting and preparing aluminum-silicon alloy castings, comprising the following steps: (1) The composition standard of the casting product is determined to be A356 (Al-7Si alloy), and A356 alloy ingots are prepared; the source of recycled aluminum scrap is about Al-18Si, and the A356 alloy ingot is prepared through a regeneration process (i.e., processed recycled aluminum scrap + pure aluminum, etc., including 93 units of Al matrix and pure aluminum + 7 units of Si).

[0065] (2) The temperature of the melting furnace is 730-750℃. Put the aluminum ingot into the melting furnace to fill 90% of the aluminum liquid. Stir and measure the composition. If Si, Ti and Fe are qualified, calculate the adjustment amount of Mg. Put the pure Mg block in the flow channel between the melting furnace and the standing furnace. Then, introduce the aluminum liquid into the standing furnace. At the same time, add the self-processed aluminum water such as waste chips in the factory.

[0066] (3) The temperature of the static furnace is 730-750℃, the aluminum liquid is left to stand for at least 60 minutes, and the Si, Mg, Ti, and Fe are qualified; the Al-Sr10 modifier rod and Al-5Ti-B refiner rod used for melt modification are added in an amount of 0.2% of the mass of the aluminum liquid in the ladle, and are placed in the flow channel between the static furnace and the transfer ladle, and then the aluminum liquid is introduced into the transfer ladle.

[0067] (4) The aluminum liquid in the ladle is transferred for refining, degassing, and slag removal. After the alloy composition is tested and qualified, it is ready to be transferred to the die-casting machine for hydraulic casting.

[0068] (5) The aluminum liquid is processed into finished castings through die casting, heat treatment, machining, painting and other processes. The pass rate of die casting X-ray inspection (full inspection) of process control is 97.0%; the mechanical properties (sampling inspection) YS, UTS, EL results are all qualified, and the specific casting edge performance is YS220MPa, UTS310MPa, EL11.8%; the casting reliability performance (sampling inspection) bench test is qualified, and the specific 13° / 90° impact is qualified, and the radial / bending fatigue is qualified.

[0069] In order to more clearly show the key preparation parameters and process monitoring of each process of recycled aluminum silicon castings, the embodiments and comparative examples are summarized as follows:

[0070] The feasibility and reliability of the method of the present invention are verified through the above-mentioned embodiments and comparative examples, and the energy consumption and CO2 emission are reduced by reducing the amount of aluminum remelting.

[0071] So far, the technical solutions of the present invention have been described in conjunction with the preferred embodiments shown in the accompanying drawings. However, it is easy for those skilled in the art to understand that the protection scope of the present invention is obviously not limited to these specific embodiments. Without departing from the principle of the present invention, those skilled in the art can make equivalent changes or substitutions to the relevant technical features, and the technical solutions after these changes or substitutions will fall within the protection scope of the present invention.

[0072] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. An improved method for melting and preparing aluminum-silicon alloy castings, characterized in that: The near / hypereutectic aluminum-silicon alloy (Al-xSi: 10≤x≤22) ingot is used as the master alloy, and the master alloy and pure aluminum are quantitatively proportioned according to the feed ratio of 1:a (0≤a≤4.5). After a series of smelting processes to obtain the required hypoeutectic aluminum-silicon alloy (Al-ySi: 4≤y≤10) target composition aluminum liquid, the subsequent production of castings is directly carried out, which specifically includes the following steps: (1) Determine the target composition Al-ySi alloy according to the casting standard, determine the ratio of the master alloy to pure aluminum as 1:a, and then determine the composition of the Al-xSi master alloy, where x=(1+a)×y. Control the content of each element in the master alloy according to the target composition and feed ratio to obtain the master alloy ingot; (2) The melting furnace temperature is 730-750°C, the intermediate alloy ingot and pure aluminum are quantitatively put into the material tower / melting continuous production furnace group, the content of the main alloy elements is detected and controlled, and the aluminum liquid is introduced into the static furnace; (3) The temperature of the static furnace is 730-750°C. After the aluminum liquid is introduced into the static furnace, it is melt treated to control the content of the main alloy elements to be qualified, and the aluminum liquid is introduced into the transfer ladle; (4) The aluminum liquid in the ladle is transferred for refining, degassing and slag removal. The smelting process ends after the alloy composition is tested and qualified; (5) The aluminum liquid becomes a commercial casting after die casting, heat treatment, machining and qualified testing; Production process control and finished product performance testing of aluminum-silicon alloy castings: Through casting X-ray yield, mechanical properties, and reliability tests, the industrial smelting and preparation methods of aluminum-silicon alloy castings are monitored in real time and the feasibility is verified.

2. The improved method for smelting and preparing aluminum-silicon alloy castings according to claim 1, characterized in that: A near / hypereutectic aluminum-silicon alloy (Al-xSi: 12≤x≤20) ingot is used as an intermediate alloy, the intermediate alloy and pure aluminum are quantitatively proportioned according to a feed ratio of 1:a (0.5≤a≤3), and after a series of smelting processes, the required hypoeutectic aluminum-silicon alloy (Al-ySi: 5≤y≤8) target composition aluminum liquid is obtained, and then subsequent casting production is directly carried out to obtain hypoeutectic aluminum-silicon alloy castings, and the hypoeutectic aluminum-silicon alloy castings include A355, A356, and A357.

3. The improved method for smelting and preparing aluminum-silicon alloy castings according to claim 2, characterized in that: The target alloy composition is selected as A356 (Al-7Si alloy), and the main element content standards are 6.5-7.5% Si, 0.25-0.45% Mg, 0.1-0.15% Ti, ≤0.15% Fe and no more than 0.05% impurity elements, and the rest is Al.

4. The improved method for smelting and preparing aluminum-silicon alloy castings according to claim 3, characterized in that: In step (1), the feed ratio of the master alloy to pure aluminum is determined to be 1:

1. The main element content of the master alloy obtained according to the 1:1 ratio is theoretically 13-15% Si, 0.5-0.9% Mg, 0.2-0.3% Ti, ≤0.3% Fe and no more than 0.05% impurity elements, and the rest is Al; According to the actual smelting process: the elements that are not easy to burn out are controlled to 13.5-14.5% Si and 0.2-0.26% Ti; the lower limit of the element Mg that is easy to burn out is controlled to 0.5-0.56%; the harmful element Fe is ≤0.22%.

5. The improved method for smelting and preparing aluminum-silicon alloy castings according to claim 4, characterized in that: In step (2), pure aluminum and intermediate alloy are added cyclically in proportion, with pure aluminum being added first and intermediate alloy being added second. The single amount of each alloy added is not more than 1000 kg. Aluminum ingots are added to 90% of the aluminum liquid capacity of the melting furnace, stirred, and the composition is measured to ensure that Si, Ti, and Fe are qualified, and the adjustment amount of Mg is calculated.

6. The improved method for smelting and preparing aluminum-silicon alloy castings according to claim 5, characterized in that: When the aluminum liquid from the melting furnace is poured into the static furnace in step (2), the easily burnt element Mg is added in the form of pure Mg blocks (≥99.5%) and placed in the flow channel between the melting furnace and the static furnace.

7. The improved method for smelting and preparing aluminum-silicon alloy castings according to claim 6, characterized in that: In step (3), the aluminum liquid in the static furnace is allowed to stand for at least 60 minutes to ensure that Si, Mg, Ti and Fe are qualified; the amount of Al-Sr10 modifier rod and Al-5Ti-B refiner rod used for melt modification is 0.2% of the mass of the aluminum liquid in the ladle, and they are placed in the flow channel between the static furnace and the transfer ladle.

Citation Information

Cited By

  • Green low-carbon renewable resource aluminum-silicon intermediate alloy and preparation method thereof

    CN119876665A

  • Integrated management system and method for molten aluminum processing technology

    CN120108567A