Rubber composition and tire
By using polyolefins and silica with hydrolyzable condensable silane groups in the rubber composition, the problem that tire rubber is difficult to have high processability, elongation of break, hardness and low heat generation at the same time is solved, and high performance is achieved rubber composition.
Patent Information
- Application Number
- CN202380029401.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-05-26
- Filing Date
- 2023-05-16
- Publication Date
- 2024-11-08
Smart Images

Figure BDA0005054284060000061 
Figure BDA0005054284060000081 
Figure BDA0005054284060000101
Abstract
Description
Technical Field
[0001] The present invention relates to a rubber composition and a tire using the same, and more particularly to a rubber composition having excellent processability, maintaining high hardness and low heat build-up while maintaining elongation at break, and a tire using the same. Background Art
[0002] In the production of tire rubber, it is necessary to reduce the viscosity of the rubber, which can achieve excellent rubber extrudability, sheet processability, etc.
[0003] On the other hand, from the perspective of the global environment, the demand for low fuel consumption of automobiles is increasing, and it is desired to develop tires with good rolling resistance. Therefore, many technologies for adding silica or silane coupling agents to diene rubbers have been proposed, but such rubbers have a problem of deteriorating processability as the viscosity increases.
[0004] In addition, in recent years, tires are particularly strongly required to improve the handling stability such as braking performance when driving at high speeds, and it is necessary to make the rubber harder. Therefore, a large number of methods such as compounding fillers can be seen, but such compounding has the problem of increasing the rolling resistance of the rubber composition.
[0005] In addition, there is a method of adding sulfur or a filler to impart durability to the tire, but there is a problem that heat generation and elongation at break deteriorate.
[0006] As described above, it is difficult in this industry to impart high levels of processability, elongation at break, hardness, and low heat build-up to a rubber composition.
[0007] In addition, Patent Document 1 below discloses a rubber composition in which 2 to 75 parts by weight of high-density polyethylene is blended with 100 parts by weight of the rubber component and kneaded at a temperature higher than the melting point of the blended resin. However, regarding the use of a rubber composition having a hydrolytically condensable silyl group in the molecule (B) required for the present invention described below and having a density of less than 0.950 g / cm 3 The technical idea of providing a rubber composition having high levels of processability, elongation at break, hardness, and low heat build-up properties by using a polyolefin is neither disclosed nor suggested in Patent Document 1.
[0008] Prior art literature
[0009] Patent Literature
[0010] Patent Document 1: Japanese Patent No. 3657839 Summary of the invention
[0011] Problems to be solved by the invention
[0012] Therefore, an object of the present invention is to provide a rubber composition having sufficient processability and hardness and having low heat build-up while maintaining elongation at break.
[0013] Solution
[0014] The present inventors have conducted intensive studies and have found that the above-mentioned problems can be solved by adding a polyolefin having a hydrolytically condensable silyl group in its molecule and having a specific density range to a rubber component in a specific amount, thereby completing the present invention.
[0015] That is, the present invention provides a rubber composition characterized in that 1 to 100 parts by mass of (B) a polyolefin having a hydrolyzable silyl group in its molecule (excluding a polyolefin having a density of 0.950 g / cm 3 (except high-density polyethylene above).
[0016] Effects of the Invention
[0017] The rubber composition of the present invention comprises 1 to 100 parts by mass of (B) a polyolefin having a hydrolyzable silyl group in its molecule (excluding a polyolefin having a density of 0.950 g / cm 3 Therefore, it is possible to provide a rubber composition having sufficient processability and hardness, maintaining elongation at break and low heat build-up, and a tire using the rubber composition.
[0018] The polyolefin (B) used in the present invention acts as a softener at high temperature when not vulcanized, thereby improving processability. In addition, after vulcanization, the polyolefin condenses and crosslinks by hydrolysis of the silyl groups while entangled with the rubber molecules, and the polyolefin aggregates in the practical temperature range of the tire, thereby improving the elongation at break and the hardness.
[0019] In addition, in the rubber composition of the silica compound system, the silyl group reacts with the silanol group on the surface of the silica to form a rubber molecule-silane coupling agent and a matrix through the silica, so that it does not become a foreign matter in the sulfur-crosslinked rubber matrix and exerts the effects of elongation at break and low heat generation. Furthermore, in the rubber composition of the silica compound system, the shear force during kneading is transmitted to the silica agglomerates by reacting with silica during kneading, thereby being able to release the agglomerates, improve dispersion, and improve low heat generation. DETAILED DESCRIPTION
[0020] Hereinafter, the present invention will be described in more detail.
[0021] (A) Rubber component
[0022] The rubber component used in the present invention is not particularly limited, and examples thereof include natural rubber (NR), isoprene rubber (IR), butadiene rubber (BR), styrene-butadiene copolymer rubber (SBR), acrylonitrile-butadiene copolymer rubber (NBR), or hydrogenated products thereof, among which, from the viewpoint of improving the effect of the present invention, a combination of NR and / or IR and BR, or hydrogenated products of SBR or NBR are preferred. In addition, there are no particular restrictions on the molecular weight and microstructure of the rubber component, and the terminal may be modified with amine, amide, silyl, alkoxysilyl, carboxyl, hydroxyl, etc., or epoxidized.
[0023] (B) Polyolefin
[0024] The polyolefin (B) used in the present invention is a polyolefin having a hydrolyzable silyl group in its molecule (density 0.950 g / cm 3 The density in the present invention can be measured by the method described in JIS K 7112, and refers to the density of the unmodified polyolefin as the base resin before having a hydrolyzable condensable silyl group.
[0025] Examples of the base resin polyolefin include polyethylene (density less than 0.950 g / cm2) such as low-density polyethylene (LDPE), linear low-density polyethylene (LLDPE), and ultra-low-density polyethylene (ULDPE). 3 From the viewpoint of improving the effect of the present invention, it is preferred to use polyolefins having as the main skeleton ethylene-α-olefin copolymers, ethylene-vinyl acetate copolymers, ethylene-methyl acrylate copolymers, or propylene-ethylene copolymers and propylene-ethylene-butene copolymers, which are also called "random polypropylene", such as ethylene-α-olefin copolymers, ethylene-(meth)acrylate copolymers, ethylene-vinyl acetate copolymers (EVA), propylene-ethylene copolymers, propylene-ethylene-butene copolymers, etc. Furthermore, the amount of polar monomers contained in ethylene-(meth)acrylate copolymers and ethylene-vinyl acetate copolymers (EVA) is preferably 1 to 60% by mass.
[0026] From the viewpoint of enhancing the effects of the present invention, the density of the polyolefin (B) is preferably 0.850 g / cm in the case of polyethylene, for example. 3 Above and less than 0.950g / cm 3 , more preferably 0.870 g / cm 3 Above 0.940g / cm 3 Below, particularly preferably 0.900 g / cm 3 Above 0.930g / cm 3 the following.
[0027] In the case of ethylene-α-olefin copolymers, 0.850 g / cm 3 Above and less than 0.950g / cm 3 , more preferably 0.860 g / cm 3 Above 0.930g / cm 3 Below, particularly preferably 0.870 g / cm 3 Above 0.920g / cm 3 the following.
[0028] In the case of ethylene-(meth)acrylate copolymer, the preferred value is 0.910 g / cm 3 Above 1.000g / cm 3 Below, more preferably 0.920 g / cm 3 Above 0.970g / cm 3 the following.
[0029] In the case of ethylene-vinyl acetate copolymer (EVA), it is preferably 0.910 g / cm 3 Above 1.000g / cm 3 Below, more preferably 0.920 g / cm 3 Above 0.970g / cm 3 the following.
[0030] In the case of propylene-ethylene copolymer or propylene-ethylene-butene copolymer, the preferred value is 0.850 g / cm 3 Above 0.920g / cm 3 Below, more preferably 0.870 g / cm 3 Above 0.910g / cm 3 the following.
[0031] From the viewpoint of enhancing the effects of the present invention, the melting point of the polyolefin (B) is preferably from 110°C to 155°C, more preferably from 130°C to 150°C.
[0032] In addition, when the (B) polyolefin is random polypropylene, the melt flow rate (MFR) measured at a temperature of 230° C. and a load of 2.16 kg is preferably 5 g / 10 minutes or more, more preferably 20 g / 10 minutes or more. The upper limit of MFR is, for example, preferably 5000 g / 10 minutes or less, more preferably 1000 g / 10 minutes or less, and particularly preferably 500 g / 10 minutes or less.
[0033] In the description of this specification, the melting point is measured by differential scanning calorimetry (DSC) according to ASTM D3418 at a heating rate of 10°C / min, and the melt flow rate (MFR) is measured under a load of 2.16 kg as described above in accordance with "Plastics - Test method for melt flow rate (MFR) of thermoplastics" specified in JIS K 7210:1999. In addition, under the above-mentioned measurement conditions of MFR, a temperature of 230°C is applicable to homopolypropylene, block polypropylene, and random polypropylene, and a temperature of 190°C is applicable to other polyolefins.
[0034] The (B) polyolefin used in the present invention may be a silane-grafted polyolefin grafted with a hydrolytically condensable silane compound. Such a silane-grafted polyolefin can be produced by a reaction process of grafting a hydrolytically condensable silane compound onto a polyolefin as a base resin. Specifically, a polyolefin and a free radical generator are allowed to coexist, and the free radical generator is decomposed by heating. The generated free radicals extract hydrogen from the polyolefin to generate polymer radicals, and the hydrolytically condensable silane compound is added thereto to obtain the (B) polyolefin used in the present invention.
[0035] Examples of the hydrolytically condensable silane compound include vinyl trimethoxysilane, vinyl triethoxysilane, and vinyl tri(β-methoxyethoxy)silane; aminosilane compounds such as γ-aminopropyl trimethoxysilane, γ-aminopropyl triethoxysilane, N-β-(aminoethyl) γ-aminopropyl trimethoxysilane, β-(aminoethyl) γ-aminopropyl methyl dimethoxysilane, and N-phenyl-γ-aminopropyl trimethoxysilane; and β-(3,4- Epoxy silane compounds such as epoxycyclohexyl)ethyltrimethoxysilane, γ-glycidyloxypropyltrimethoxysilane, γ-glycidyloxypropylmethyldiethoxy, acryl silane compounds such as γ-methacryloxypropyltrimethoxysilane, polysulfide silane compounds such as bis(3-(triethoxysilyl)propyl)disulfide and bis(3-(triethoxysilyl)propyl)tetrasulfide, mercaptosilane compounds such as 3-mercaptopropyltrimethoxysilane and 3-mercaptopropyltriethoxysilane, etc.
[0036] Examples of the free radical generator include known organic peroxides, such as dicumyl peroxide, benzoyl peroxide, 1,1-bis(tert-butylperoxy)-3,3,5-trimethylcyclohexane, tert-butylperoxyisopropyl carbonate, tert-butyl peroxybenzoate, 2,5-dimethyl-2,5-bis(benzoylperoxide)hexane, methyl ethyl ketone peroxide, 2,2-bis(tert-butylperoxy)butane, and isopropylbenzene hydroperoxide.
[0037] As the conditions of the above reaction process for graft copolymerizing the polyolefin as the base resin with the hydrolysis-condensation silane compound, for example, 0.1 to 10 parts by mass of the hydrolysis-condensation silane compound is added to 100 parts by mass of the polyolefin as the base resin, and the obtained compound is mixed at a temperature above the melting point of the above polyolefin. In addition, the amount of the free radical generator added is, for example, about 0.01 to 0.5 parts by mass relative to 100 parts by mass of the above polyolefin. In addition, the reaction conditions of the above graft copolymerization are well known, for example, disclosed in Japanese Patent Gazette No. 5768696, etc. In addition, in the above reaction process, well-known additives such as antioxidants may also be added to the reaction system.
[0038] (Carbon Black)
[0039] Carbon black may be blended into the rubber composition of the present invention. The carbon black used in the present invention has a nitrogen adsorption specific surface area (N 2 SA) preferably:
[0040] Nitrogen adsorption specific surface area (N 2 SA) is 20~300m 2 / g, more preferably 40 to 150 m 2 / g.
[0041] In addition, the nitrogen adsorption specific surface area (N 2 SA) is a value obtained according to JIS K6217-2.
[0042] (Silicon Dioxide)
[0043] The rubber composition of the present invention may be blended with silica. From the viewpoint of improving the effect of the present invention, the nitrogen adsorption specific surface area N of the silica used in the present invention is preferably 2 SA is preferably 20 to 300 m 2 / g, more preferably 80 to 250 m 2 / g.
[0044] (Ratio of rubber composition)
[0045] The rubber composition of the present invention is characterized by blending (B) a polyolefin having a hydrolytically condensable silyl group in its molecule (density 0.950 g / cm 3 The above high-density polyethylene is excluded) 1 to 100 parts by mass.
[0046] When the amount of the polyolefin (B) is less than 1 part by mass, the effect of the present invention cannot be achieved. On the contrary, when it exceeds 100 parts by mass, the rubber elasticity is significantly reduced.
[0047] In the rubber composition of the present invention, the amount of the polyolefin (B) is preferably 5 to 80 parts by mass, more preferably 10 to 50 parts by mass, based on 100 parts by mass of the rubber component.
[0048] In the rubber composition of the present invention, the amount of carbon black and / or silica blended is preferably 20 to 200 parts by mass per 100 parts by mass of the rubber component.
[0049] Specifically, in the rubber composition of the present invention, the amount of carbon black blended is preferably 5 to 200 parts by mass per 100 parts by mass of the rubber component, and the amount of silica blended is preferably 0 to 195 parts by mass, more preferably 5 to 100 parts by mass, per 100 parts by mass of the rubber component.
[0050] (Other ingredients)
[0051] In addition to the above-mentioned components, the rubber composition of the present invention may also be formulated with a vulcanizing or crosslinking agent; a vulcanizing or crosslinking accelerator; various fillers, such as clay, talc, calcium carbonate, aluminum hydroxide; an anti-aging agent; a plasticizer; a resin; a curing agent; a silane coupling agent; a processing aid, and the like, which are various additives that can be generally formulated in a rubber composition. These additives can be mixed by a general method to form a composition and then used for vulcanization or crosslinking. The amount of these additives may also be the general amount in the past as long as it does not violate the purpose of the present invention.
[0052] The rubber composition of the present invention has excellent processability, can maintain high hardness while maintaining elongation at break, and has low heat generation, and is therefore suitable for use in tire treads. In addition, the tire of the present invention is preferably a pneumatic tire that can be filled with inert gas such as air, nitrogen, or other gases.
[0053] Example
[0054] The present invention will be further described below by way of Examples and Comparative Examples, but the present invention is not limited to the following Examples.
[0055] (Synthesis Examples 1 to 7 of Silane-Grafted Polyolefin)
[0056] The following materials were used.
[0057] Base polymer A: ethylene-1-octene copolymer resin (ENGAGE 8100 manufactured by Dawuchemika Co., Ltd., density = 0.870 g / cm 3 , melting point = 60°C, MFR = 1.0 g / 10 min)
[0058] Base polymer B: ethylene-propylene copolymer resin (KEP110 manufactured by KUMHOPOLYCHEM Co., Ltd., density = 0.865 g / cm 3 , Mooney viscosity (ML1+4 100℃)=40,propylene content=48.0%)
[0059] Base polymer C: ethylene-vinyl acetate copolymer resin (Novatech EVA LV430 manufactured by Japan Polyethylene Co., Ltd., density = 0.940 g / cm 3 , melting point = 89°C, MFR = 1.0 g / 10 min)
[0060] Base polymer D: high pressure low density polyethylene (Novatech LDYF30 manufactured by Japan Polyethylene Co., Ltd., density = 0.920 g / cm 3 , melting point = 108°C, MFR = 1.1 g / 10 minutes)
[0061] Base polymer E: linear low-density polyethylene (Novatech LL UF240 manufactured by Japan Polyethylene Co., Ltd., density = 0.920 g / cm 3 , melting point = 123°C, MFR = 2.1 g / 10 min)
[0062] Base polymer F: high-density polyethylene (Novatech LDHY430 manufactured by Japan Polyethylene Co., Ltd., density = 0.956 g / cm 3 , melting point = 135°C, MFR = 0.8 g / 10 min)
[0063] Base polymer G: random polypropylene (Novatech PPMG05ES manufactured by Nippon Polypro Co., Ltd., density = 0.900 g / cm 3 , melting point = 148°C, MFR = 45g / 10min)
[0064] ·Hydrolysis-condensation silane compound 1: Vinyltrimethoxysilane (KBM1003 manufactured by Shin-Etsu Chemical Co., Ltd.)
[0065] ·Hydrolysis-condensation silane compound 2: Vinyltriethoxysilane (KBE1003 manufactured by Shin-Etsu Chemical Co., Ltd.)
[0066] Free radical generator: dicumyl peroxide
[0067] · Antioxidant: Irganox 1010 manufactured by BASF Japan Ltd.
[0068] The above base polymer, hydrolytic condensable silane compound, free radical generator and antioxidant were subjected to graft reaction in the formulation (parts by mass) shown in Table 1 below by using the following extruder to obtain silane-grafted polyolefins of Synthesis Examples 1 to 7.
[0069] As an extruder, an extruder with L / D=28 and a screw outer diameter of 65 mm was used, and the temperature of each zone in the temperature conditions was as follows. That is, the first zone: 160°C, the second zone: 180°C, the third zone: 200°C, the fourth zone: 230°C, the head zone: 230°C, and the die zone: 230°C. Under the above conditions, after extrusion into strands, water cooling was performed and pelletization was performed by a pelletizer.
[0070]
[0071] Preparation of samples of Examples 1 to 6 and Comparative Examples 1 to 5
[0072] The components (mass parts) shown in Table 2 except the vulcanization system (vulcanization accelerator, sulfur) were mixed in a Banbury mixer at 80°C for 5 minutes. The reaching temperature at this time was 150°C, which exceeded the melting point of various polyolefins as base resins. Then, the vulcanization system was added and mixed using a roller to obtain a rubber composition, and the following evaluation was performed.
[0073] <Compound Processability (Processability of Each Rubber Composition)>
[0074] For each rubber composition (unvulcanized) obtained, the processability as a composite is evaluated by measuring Mooney viscosity (ML). The Mooney viscosity of each rubber composition is measured according to JIS K6300 using an L-type rotor (38.1 mm diameter, 5.5 mm thick) in a Mooney viscometer under the conditions of 1 minute preheating time, 4 minutes of rotor rotation time, 100 ° C, and 2 rpm. As a result, the reciprocal of the obtained numerical value is indexed. Specifically, the value of Comparative Example 1 is set to 100. The larger the index, the lower the viscosity, and the more excellent the processability. In addition, if the index is 100, it is considered to have sufficient processability in practice.
[0075] <Preparation of Vulcanized Rubber Sheets for Evaluation>
[0076] Each of the obtained rubber compositions (unvulcanized) was press-vulcanized in a mold (15 cm×15 cm×0.2 cm) at 170° C. for 10 minutes to prepare a vulcanized rubber sheet (vulcanized rubber test piece).
[0077] <Elongation at break>
[0078] For the vulcanized rubber test piece made as described above, a JIS No. 3 dumbbell-shaped test piece (thickness 2 mm) was punched out according to JIS K6251, and the test was carried out at a tensile speed of 500 mm / min to determine the tensile elongation at break. As a result, the obtained numerical value was indexed. Specifically, the value of Comparative Example 1 was set to 100. The larger the index, the larger the tensile elongation at break, and the better the mechanical properties.
[0079] <Heat generation: tanδ(60℃)>
[0080] For the vulcanized rubber test piece prepared as described above, a viscoelasticity spectrometer (manufactured by Toyo Seiki Seisaku-sho Co., Ltd.) was used to measure the loss tangent tanδ (60°C) at a temperature of 60°C under the conditions of an initial strain of 10%, an amplitude of ±2%, and a frequency of 20 Hz to evaluate the heat generation. As a result, the reciprocal of the obtained value was indexed. Specifically, the value of Comparative Example 1 was set to 100. The larger the index, the better the low heat generation when the tire is made.
[0081] <Hardness>
[0082] The tire was measured at 20°C according to JIS K6253. The reciprocal of the obtained value was indexed. Specifically, the value of Comparative Example 1 was set to 100. The larger the index, the higher the tire hardness. If the index is 100, it is considered to have sufficient hardness for practical use.
[0083] The results are shown in Table 2.
[0084]
[0085] *1: NR(SIR20)
[0086] *2: BR (Nipol BR1220 manufactured by Nippon Seon Co., Ltd., number average molecular weight = 1.8×10 5 )
[0087] *3: Silica 1 (Zeosil 1085GR manufactured by Solvay Japan Co., Ltd., nitrogen adsorption specific surface area (N 2 SA)=90m 2 / g, CTAB specific surface area = 80m 2 / g)
[0088] *4: Carbon black (trade name: Carbon Black N339, manufactured by Kirin Co., Ltd., nitrogen adsorption specific surface area (N) 2 SA)=88m 2 / g, CTAB specific surface area = 90m 2 / g)
[0089] *5: Silane coupling agent (Si69, bis(3-triethoxysilylpropyl)tetrasulfide manufactured by Ebonick Degussa Co., Ltd.
[0090] *6: Zinc oxide (three types of zinc oxide manufactured by Shoto Chemical Industry Co., Ltd.)
[0091] *7: Stearic acid (Stearic acid YR manufactured by NOF Corporation)
[0092] *8: Anti-aging agent (SANTOFLEX 6PPD produced by Flexsys)
[0093] *9: Sulfur (Karuizawa Refinery Co., Ltd. oil processing sulfur)
[0094] *10: Vulcanization accelerator 1 (Noxela CZ-G manufactured by Ouchi Shinko Chemical Industry Co., Ltd.)
[0095] *11: Vulcanization accelerator 2 (Noxela D manufactured by Ouchi Shinko Chemical Industry Co., Ltd.)
[0096] Examples 7 to 10 and Comparative Example 6
[0097] As shown in Table 3 below, the above-mentioned "Examples 1 to 6 and Comparative Examples 1 to 5" were repeated except that the blending amount of each material was changed, and evaluation was performed. In addition, each evaluation result was indexed with the value of Comparative Example 6 being 100. The results are shown in Table 3.
[0098]
[0099] Example 11 and Comparative Examples 7 to 8
[0100] As shown in Table 4 below, the above-mentioned "Examples 1 to 6 and Comparative Examples 1 to 5" were repeated except that the blending amount of each material was changed, and evaluation was performed. In addition, each evaluation result was indexed with the value of Comparative Example 7 being 100. The results are shown in Table 4.
[0101]
[0102] Example 12 and Comparative Example 9
[0103] As shown in Table 5 below, except for changing the compounding amount of each material, the above-mentioned "Examples 1 to 6 and Comparative Examples 1 to 5" were repeated and evaluated. In addition, in <Preparation of vulcanized rubber sheet for evaluation>, the press vulcanization conditions were changed to 30 minutes at 170°C to prepare a vulcanized rubber sheet. In addition, the value of Comparative Example 9 was indexed as 100 in each evaluation result. The results are shown in Table 5. In addition, as a hydrogenated nitrile rubber, Zetpol 2320L manufactured by Zeon Co., Ltd. of Japan was used (bonded acrylonitrile content 36.2%, iodine value 56.60 mg / 100 mg, Mooney viscosity 57.5).
[0104]
[0105] Examples 13 to 15 and Comparative Example 10
[0106] As shown in Table 6 below, the above-mentioned "Examples 1 to 6 and Comparative Examples 1 to 5" were repeated except that the blending amount of each material was changed, and evaluation was performed. In addition, each evaluation result was indexed with the value of Comparative Example 10 being 100. The results are shown in Table 6.
[0107]
[0108] *12: Silylated random polypropylene (Linkron PM700N manufactured by Mitsubishi Chemical Co., Ltd., density before silylation = about 0.880 g / cm 3 , melting point = 77°C, MFR = 17 g / 10 min)
[0109] *13: Silica 2 (Zeosil 1165mp manufactured by Solvay Japan Co., Ltd., nitrogen adsorption specific surface area (N 2 SA)=160m 2 / g, CTAB specific surface area = 159m 2 / g)
[0110] Example 16 and Comparative Example 11
[0111] As shown in Table 7 below, the above-mentioned "Examples 1 to 6 and Comparative Examples 1 to 5" were repeated except that the blending amount of each material was changed, and evaluation was performed. In addition, each evaluation result was indexed with the value of Comparative Example 16 being 100. The results are shown in Table 7.
[0112]
[0113] *14:SBR (Nipol 1502 manufactured by Nippon Alon Co., Ltd.)
[0114] As can be seen from the results in the above tables, the rubber compositions of the examples are characterized by blending 1 to 100 parts by mass of (B) a polyolefin having a hydrolyzable silyl group in its molecule (density 0.950 g / cm 3 Therefore, compared with Comparative Examples 1, 6, 7, 9, 10 or 11, it has sufficient processability and hardness and can have low heat generation while maintaining the elongation at break.
[0115] On the other hand, Comparative Examples 2 to 4 in Table 2 are examples in which base polymer A, C or D is used instead of polyolefin (B), and thus the elongation at break and heat generation are deteriorated. Comparative Example 5 is an example in which a base polymer having a density of 0.950 g / cm 3 The above examples of high-density polyethylene therefore deteriorate in processability, elongation at break, and heat build-up.
[0116] Examples 7 to 10 in Table 3 are examples in which the blending amount of the (B) polyolefin was variously changed. However, similar to the results in Table 1, it is found that the compositions have sufficient processability and hardness, and have low heat build-up while maintaining elongation at break.
[0117] In addition, Example 11 in Table 4 is a test of a system without silica, but it is known that it has sufficient processability and hardness, and has low heat generation while maintaining elongation at break, as in the results of Table 1. Comparative Example 8 is an example in which base polymer A is used instead of (B) polyolefin, and therefore the effect of the present invention cannot be achieved.
[0118] In addition, Example 12 in Table 5 is an example in which an additive is used as the rubber component (A), and it is found that the rubber component has sufficient processability and hardness, and has low heat generation while maintaining the elongation at break.
[0119] In addition, Examples 13 and 14 in Table 6 are examples using random PP as the (B) polyolefin, and it is known that they have sufficient processability and hardness, and have low heat generation while maintaining the elongation at break. Example 15 is an example using 100% by mass of natural rubber as the (A) rubber component, and it is known that they have sufficient processability and hardness, and have low heat generation while maintaining the elongation at break.
[0120] The present disclosure includes the following inventions.
[0121] Invention [1]. A rubber composition characterized in that 1 to 100 parts by mass of (B) a polyolefin having a hydrolyzable silyl group in its molecule (excluding a polyolefin having a density of 0.950 g / cm 3 (except high-density polyethylene above).
[0122] Invention [2]. The rubber composition according to Invention [1], wherein the polyolefin (B) is a silane-grafted polyolefin grafted with a hydrolyzable condensable silane compound.
[0123] Invention [3]. The rubber composition according to invention [1] or [2], characterized in that 20 to 200 parts by mass of carbon black and / or silica are further compounded with respect to 100 parts by mass of the rubber component (A).
[0124] Invention [4]. A rubber composition according to any one of Inventions [1] to [3], wherein the rubber component (A) is natural rubber (NR), isoprene rubber (IR), butadiene rubber (BR), styrene-butadiene copolymer rubber (SBR), acrylonitrile-butadiene copolymer rubber (NBR) or hydrogenated products thereof.
[0125] Invention [5]. A rubber composition according to any one of Inventions [1] to [4], wherein the (B) polyolefin has an ethylene-α-olefin copolymer, an ethylene-vinyl acetate copolymer, an ethylene-methyl acrylate copolymer, a propylene-ethylene copolymer or a propylene-ethylene-butene copolymer as a main skeleton.
[0126] Invention [6]. A method for producing a rubber composition, characterized in that the density of the rubber composition is 0.950 g / cm2 relative to 100 parts by mass of a base resin. 3 A polyolefin other than the above high-density polyethylene is mixed with 0.1 to 10 parts by mass of a hydrolyzable condensable silane compound, and the resulting mixture is mixed at a temperature above the melting point of the base resin to obtain the (B) polyolefin having a hydrolyzable condensable silyl group in the molecule, and further 1 to 100 parts by mass of the (B) polyolefin is mixed with 100 parts by mass of the (A) rubber component and mixed.
[0127] Invention [7]. A tire using the rubber composition according to any one of Inventions [1] to [5].
Claims
1. A rubber composition, characterized in that: 1 to 100 parts by mass of (B) a polyolefin having a hydrolyzable silyl group in its molecule (excluding a polyolefin having a density of 0.950 g / cm 3 (except high-density polyethylene above).
2. The rubber composition according to claim 1, characterized in that The (B) polyolefin is a silane-grafted polyolefin to which a hydrolytically condensable silane compound is grafted.
3. The rubber composition according to claim 1, characterized in that 20 to 200 parts by mass of carbon black and / or silica are further compounded with respect to 100 parts by mass of the (A) rubber component.
4. The rubber composition according to claim 1, characterized in that The rubber component (A) is natural rubber (NR), isoprene rubber (IR), butadiene rubber (BR), styrene-butadiene copolymer rubber (SBR), acrylonitrile-butadiene copolymer rubber (NBR) or hydrogenated products thereof.
5. The rubber composition according to claim 1, characterized in that The (B) polyolefin has an ethylene-α-olefin copolymer, an ethylene-vinyl acetate copolymer, an ethylene-methyl acrylate copolymer, a propylene-ethylene copolymer or a propylene-ethylene-butene copolymer as a main skeleton.
6. A method for producing a rubber composition, characterized in that: The density of the base resin is 0.950 g / cm 3 A polyolefin other than the above high-density polyethylene is mixed with 0.1 to 10 parts by mass of a hydrolyzable condensable silane compound, and the resulting mixture is mixed at a temperature above the melting point of the base resin to obtain the (B) polyolefin having a hydrolyzable condensable silyl group in the molecule, and further 1 to 100 parts by mass of the (B) polyolefin is mixed with 100 parts by mass of the (A) rubber component and mixed.
7. A tire using the rubber composition according to claim 1.