Cobalt and nickel separation method
By leaching using a treatment solution of sulfuric acid and hydrogen peroxide in lithium-ion secondary batteries, combined with hydrogen sulfide compound precipitation and redissolution technology of fine bubble generators, the high cost and process of recycling cobalt and nickel in the prior art is solved. Complex problems achieve efficient and low-cost separation and recycling of cobalt and nickel.
Patent Information
- Application Number
- CN202380029544.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-31
- Filing Date
- 2023-03-30
- Publication Date
- 2024-11-08
AI Technical Summary
The prior art method of recovering cobalt and nickel in lithium-ion secondary batteries is costly and complicated in process, especially the cost of using hydrogen peroxide as an oxidant, and the sulfide leaching method requires autoclave heating and long-term oxidation, which cannot be effective. Leaching sulfide.
The lithium-ion secondary battery electrode material is leached in the treatment solution containing sulfuric acid and hydrogen peroxide, and the copper precipitation process is used to precipitate copper, followed by pH adjustment and filtration using alkali metal hydroxide, and hydrogen sulfide compound is added to make cobalt and nickel The sulfide is formed, and then the sulfide is dissolved in dilute sulfuric acid through a fine bubble generator to reduce the amount of hydrogen peroxide used.
It is realized that cobalt and nickel are separated and recovered from lithium-ion secondary batteries at low cost and high accuracy, simplifying the process, reducing costs, and improving the leaching rate and purity of cobalt and nickel.
Smart Images

Figure CN118922569A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a method for separating cobalt and nickel, which can accurately separate and recover cobalt and nickel contained in a lithium ion secondary battery from other metals.
[0002] This application claims priority based on patent application No. 2022-060241 filed in Japan on March 31, 2022, and the contents are incorporated herein by reference. Background Art
[0003] Lithium-ion secondary batteries are used as power sources in a wide range of fields, from small objects such as various electronic devices to large objects such as electric vehicles. When these lithium-ion secondary batteries are discarded, useful metals need to be recovered and reused.
[0004] Lithium-ion secondary batteries are formed by dividing the negative electrode material and the positive electrode material with a porous separator such as polypropylene, stacking them in layers, and sealing them in a casing such as aluminum or stainless steel together with an electrolyte such as lithium hexafluorophosphate (LiPF6) and an electrolyte solution.
[0005] The negative electrode material of the lithium-ion secondary battery is formed by coating a negative electrode active material such as graphite mixed with a binder on a negative electrode collector composed of copper foil, etc. In addition, the positive electrode material is formed by coating a positive electrode active material such as lithium manganate, lithium cobaltate, lithium nickelate, etc. mixed with a binder on a positive electrode collector composed of aluminum foil, etc.
[0006] Thus, the positive electrode active material of the lithium ion secondary battery contains a large amount of cobalt and nickel, but the positive electrode active material that has been crushed and separated in advance during the recycling process contains manganese, copper, aluminum, lithium, etc. in addition to cobalt and nickel. Therefore, in order to separate and recover cobalt and nickel from the lithium ion secondary battery with a high yield, it is necessary to accurately remove metals other than cobalt and nickel.
[0007] Conventionally, as a method for separating and recovering cobalt and nickel contained in lithium ion secondary batteries, for example, Patent Documents 1 and 2 disclose a method for recovering valuable metals from used lithium ion secondary batteries. In this recovery method, a positive electrode active material is taken out from the lithium ion secondary battery, and the positive electrode active material is subjected to acid leaching to obtain a leachate in which metals are leached, and cobalt and nickel are separated from the leachate by solvent extraction.
[0008] In Patent Documents 1 and 2, a precipitate (sulfide) containing cobalt and nickel is generated in the middle of the process, and then the precipitate is redissolved using sulfuric acid and hydrogen peroxide as an oxidant to generate a solution containing cobalt and nickel. However, there are problems such as the high cost of hydrogen peroxide as an oxidant as a chemical, and the overall cost of the process for recovering cobalt and nickel contained in lithium-ion secondary batteries becomes high.
[0009] On the other hand, Patent Document 3 discloses a sulfide leaching method. In this method, a sulfide slurry whose temperature is set to 80°C or higher and lower than 115°C is added to a sulfuric acid acid solution contained in a reaction container, and an oxygen-containing gas is further supplied into the reaction container. Thus, sulfides containing cobalt or nickel are dissolved. It is believed that according to this method, sulfides containing cobalt and nickel can be dissolved in sulfuric acid without using expensive hydrogen peroxide.
[0010] Patent Document 1: Japanese Patent Application Publication No. 2016-113672
[0011] Patent Document 2: Japanese Patent Application Publication No. 2016-186118
[0012] Patent Document 3: Japanese Patent Application Publication No. 2018-193588
[0013] However, the sulfide leaching method disclosed in Patent Document 3 requires a laborious method of heating the sulfide slurry to 80° C. or higher and less than 115° C. using an autoclave. Furthermore, if only an oxygen-containing gas is supplied into the reaction vessel, the reaction time required for oxidation becomes long, and the sulfide cannot be leached efficiently. Summary of the invention
[0014] The present invention has been completed in view of the above situation, and its purpose is to provide a method for separating cobalt and nickel, which can separate cobalt and nickel contained in lithium-ion secondary batteries and other metals with high precision in fewer steps, thereby recovering cobalt and nickel from lithium-ion secondary batteries at a lower cost.
[0015] In order to solve the above-mentioned problems, a method for separating cobalt and nickel according to one embodiment of the present invention has the following characteristics.
[0016] [1] A method for separating cobalt and nickel from a lithium ion secondary battery, characterized in that it comprises: a leaching step, in which an electrode material of a lithium ion secondary battery is immersed in a treatment solution containing sulfuric acid and hydrogen peroxide to obtain a leachate; a copper precipitation step, in which a hydrogen sulfide compound is added to the leachate and stirred to precipitate copper in the form of copper sulfide; any one of a first treatment step and a second treatment step, wherein the first treatment step sequentially comprises: a first neutralization step, in which an alkali metal hydroxide is added to the mixed solution containing the precipitate obtained in the copper precipitation step to adjust the pH to obtain a first neutralized solution; and a first filtration step, in which the first neutralized solution is subjected to solid-liquid separation to obtain a first eluted solution containing cobalt and nickel and a residue containing copper sulfide, and the second treatment step sequentially comprises: a second filtration step, in which the eluted solution containing the copper sulfide obtained in the copper precipitation step is subjected to solid-liquid separation to obtain a first eluted solution containing cobalt and nickel and a residue containing copper sulfide. The mixed liquid with the precipitate is subjected to solid-liquid separation to obtain a second eluent containing cobalt and nickel and a residue containing copper sulfide; and a second neutralization process, an alkali metal hydroxide is added to the second eluent to adjust the pH to obtain a second neutralized liquid; a cobalt-nickel separation step, a hydrogen sulfide compound is added to the first eluent obtained in the first treatment step or the second neutralized liquid obtained in the second treatment step and stirred to perform solid-liquid separation to obtain a precipitate containing cobalt sulfide and nickel sulfide and a residual liquid containing lithium; and a redissolution step, in which the cobalt and nickel contained in the precipitate are dissolved in a suspension obtained by suspending the precipitate separated in the cobalt-nickel separation step in dilute sulfuric acid to obtain a cobalt-nickel solution containing cobalt and nickel, and the redissolution step is a step of bubbling the suspension with an oxygen-containing oxidizing gas using a microbubble generator.
[0017] According to one embodiment of the present invention, when a precipitate containing cobalt sulfide and nickel sulfide is reacted with a re-dissolving solution containing sulfuric acid, bubbling with an oxidizing gas can reduce the amount of oxidizing agents such as hydrogen peroxide, which are expensive, and the precipitate can be re-dissolved in sulfuric acid at a low cost. Thus, cobalt and nickel can be recovered from lithium-ion secondary batteries at a low cost.
[0018] [2] The method for separating cobalt and nickel according to [1], characterized in that:
[0019] The pH of the suspension is set within a range of 2.0 to 7.0.
[0020] [3] The method for separating cobalt and nickel according to [1] or [2], characterized in that:
[0021] The bubbling in the redissolution step is performed by bubbling the oxidizing gas at a flow rate of 0.1 L / min to 5 L / min inclusive through 1000 mL of the suspension for 50 minutes to 12000 minutes inclusive.
[0022] [4] The method for separating cobalt and nickel according to any one of [1] to [3], characterized in that:
[0023] The oxygen concentration of the oxidizing gas used in the redissolution step is 20% by volume or more.
[0024] [5] The method for separating cobalt and nickel according to any one of [1] to [4], characterized in that:
[0025] In the re-dissolution step, the pH of the suspension during bubbling is within a range of 3.0 to 7.0.
[0026] [6] The method for separating cobalt and nickel according to any one of [1] to [5], characterized in that:
[0027] In the re-dissolving step, hydrogen peroxide is added to the suspension.
[0028] [7] The method for separating cobalt and nickel according to any one of [1] to [6], characterized in that:
[0029] The first treatment step is performed as a post-step of the copper precipitation step.
[0030] [8] The method for separating cobalt and nickel according to any one of [1] to [7], characterized in that:
[0031] As a pre-process of the leaching process, a pulverizing and sorting process is further provided: the lithium ion secondary battery is pulverized and classified to obtain an electrode material containing at least cobalt, nickel, copper and lithium.
[0032] [9] The method for separating cobalt and nickel according to any one of [1] to [8] is characterized in that it also comprises the following solvent extraction step: adding an extractant solution to the cobalt-nickel solution to obtain a cobalt extract and a nickel extract.
[0033]
[10] The method for separating cobalt and nickel according to any one of [1] to [9], characterized in that:
[0034] As a pre-step of the pulverization and separation step, a heat treatment step of heating the lithium ion secondary battery for heat treatment is further included.
[0035] According to one embodiment of the present invention, a method for separating cobalt and nickel can be provided, which can separate cobalt and nickel and metals other than cobalt and nickel contained in a lithium ion secondary battery with high accuracy in a simple process, thereby recovering cobalt and nickel from the lithium ion secondary battery. BRIEF DESCRIPTION OF THE DRAWINGS
[0036] Figure 1 This is a flowchart showing in stages the recycling method of the electrode material of the lithium ion secondary battery including the method for separating cobalt and nickel according to the first embodiment of the present invention.
[0037] Figure 2 This is a flowchart showing in stages a recycling method of an electrode material of a lithium ion secondary battery including a method for separating cobalt and nickel according to a second embodiment of the present invention.
[0038] Figure 3 This is a graph showing changes in the leaching rates of cobalt and nickel with the passage of bubbling time in the redissolution step in Example (1) of the present invention.
[0039] Figure 4 This is a graph showing changes in the leaching rates of cobalt and nickel in Example (2) of the present invention as the bubbling time in the redissolution step and the reaction time after the addition of hydrogen peroxide elapse. DETAILED DESCRIPTION
[0040] Hereinafter, a method for separating cobalt and nickel according to an embodiment of the present invention will be described with reference to the accompanying drawings. In addition, each embodiment shown below is specifically described for better understanding of the gist of the present invention, and the present invention is not limited thereto unless otherwise specified.
[0041] (First Embodiment)
[0042] Figure 1 This is a flowchart showing in stages the recycling method of the electrode material of the lithium ion secondary battery including the method for separating cobalt and nickel according to the first embodiment of the present invention.
[0043] (Heat treatment step S1)
[0044] As a pretreatment step for separating electrode materials constituting discarded lithium ion secondary batteries (hereinafter referred to as waste LIBs), waste LIBs are heated to about 500° C. in a heating furnace, for example, with superheated water vapor to perform heat treatment.
[0045] The heat treatment can be performed under vacuum or normal pressure, but it is preferably heated in an inert atmosphere free of oxygen. In waste LIBs, due to the presence of binders and electrolytes, the positive electrode active material, the negative electrode active material and the aluminum foil and copper foil as current collectors have a large adhesion. Therefore, by performing a heat treatment process at or above 400°C, it is easy to separate these active materials from the current collector. By setting the heating temperature of the waste LIB to below 650°C, it is possible to prevent aluminum from melting and being involved in the active material and cooling and solidifying, making it difficult to remove only the active material.
[0046] (Crushing and Sorting Process S2)
[0047] Next, the waste LIB after the heat treatment is pulverized, and then the electrode material is sorted and separated by sieving. The waste LIB is pulverized using, for example, a biaxial shearing crusher or a hammer mill.
[0048] Then, the crushed waste LIB is classified using a sieve with appropriate mesh size, and the battery container, aluminum foil, copper foil, and nickel terminal are recovered as the oversize, and the electrode material containing the positive electrode active material (LiCoO2, etc.) and the negative electrode active material (graphite) are recovered as the undersize. Such electrode materials can be materials that pass through a sieve with a mesh size of about 0.5 mm.
[0049] The separated electrode materials mainly include cobalt, nickel, manganese, copper, iron, aluminum, lithium, calcium, etc., which are constituent materials and impurities of the positive electrode active material, and carbon, etc., which are constituent materials of the negative electrode active material.
[0050] (Leaching step S3)
[0051] Next, the electrode material separated in the crushing and sorting step S2 is immersed in a treatment liquid to obtain a leachate. As the treatment liquid, a solution obtained by mixing sulfuric acid (H2SO4) and hydrogen peroxide (H2O2) is used.
[0052] Co and Ni contained in the waste LIB also include trivalent and tetravalent forms that are difficult to dissolve in sulfuric acid. Therefore, by using hydrogen peroxide as a reducing agent, they can be reduced to divalent Co and divalent Ni that are more easily soluble in sulfuric acid.
[0053] As an example of a treatment liquid, a solution obtained by mixing 5 ml or more of hydrogen peroxide with a concentration of 30% by weight with respect to 100 ml of dilute sulfuric acid with a concentration of 2 mol / L or more can be cited. By setting the concentration of dilute sulfuric acid to 2 mol / L or more and the amount of hydrogen peroxide added to 5 ml or more, the leaching rate of cobalt and nickel can be improved. Although there is no particular limitation, even if it is set to more than this, it is impossible to expect a further improvement in the leaching rate, so the upper limit of the sulfuric acid concentration is 18 mol / L, and the upper limit of the amount of hydrogen peroxide added is 30 ml.
[0054] A defoamer containing a saturated aliphatic alcohol (straight-chain saturated alcohol) having a carbon number of 8 or less may be added to the treatment solution. By adding the defoamer, bubbles generated by the reaction between the electrode material and sulfuric acid can be eliminated. Therefore, the electrode material can be effectively acid-leached in a short time without using excessive sulfuric acid.
[0055] As a specific example of the leaching step S3, for example, the powdered electrode material separated in the pulverizing and sorting step S2 is added to the treatment liquid heated to 60°C or higher, and immersed for 4 hours or more. At this time, it is preferable to further stir.
[0056] The leaching rate of cobalt and nickel can be increased by setting the treatment liquid temperature to 60°C or more and the leaching (immersion) time to 4 hours or more. Although there are no particular restrictions, even if it is set above, no further increase in the leaching rate can be expected, so the upper limit of the treatment liquid temperature is 90°C and the upper limit of the leaching time is 15 hours.
[0057] Through such a leaching step S3, in the electrode material, metal components (cobalt, nickel, manganese, copper, iron, aluminum, lithium, calcium, etc.) derived from the positive electrode active material are dissolved in the treatment solution, while carbon derived from the negative electrode active material is not dissolved and remains as carbon residue.
[0058] (Copper precipitation step S4)
[0059] Next, a hydrogen sulfide compound is added to the leachate obtained in the leaching step S3 and stirred to obtain a mixed solution in which the eluate containing cobalt and nickel and the precipitate containing copper sulfide (CuS) are mixed.
[0060] In this embodiment, the hydrogen sulfide compound refers to a compound containing sulfur and the sulfur component is in the form of H2S, HS - or S 2- The form of the compound.
[0061] As the hydrogen sulfide compound used in the copper separation step S4, water-soluble alkali metal hydrogen sulfide can be cited, and in this embodiment, an aqueous solution of sodium hydrogen sulfide (NaSH) is used. As a specific example of the copper separation step S4, the leachate is diluted with ion exchange water, and then the aqueous solution of sodium hydrogen sulfide is added to the diluted leachate and stirred.
[0062] The addition of the aqueous solution of sodium hydrogen sulfide is performed, for example, until the oxidation-reduction potential (vs Ag / AgCl) becomes 0 mV or less. By adding sodium hydrogen sulfide until the oxidation-reduction potential becomes 0 mV or less, almost all of the copper contained in the leachate can be precipitated.
[0063] The pH of the leachate from the start to the end of the addition of the hydrogen sulfide compound is preferably maintained at 2.0 or less, more preferably maintained at 1.0 or less. If the pH of the leachate exceeds 2.0, cobalt and nickel sulfides may be generated, and their recovery rate in the eluate may decrease.
[0064] As the hydrogen sulfide compound, in addition to sodium hydrogen sulfide, for example, sodium sulfide, sodium thiosulfate, or sodium disulfite may be mentioned.
[0065] By adding a hydrogen sulfide compound to the leachate, the hydrogen sulfide compound is dissolved in the metal components in the leachate, and copper reacts with sulfur to generate copper sulfide (CuS) and precipitate. On the other hand, metal components other than copper (cobalt, nickel, manganese, iron, aluminum, lithium, calcium, etc.) remain in the liquid phase, thereby obtaining an eluate containing cobalt and nickel.
[0066] (First treatment step S5A)
[0067] Next, as the first treatment step S5A, a first neutralization process S5A-1 and a first filtration process S5A-2 are sequentially performed.
[0068] In the first neutralization step S5A-1, an alkali metal hydroxide is added to the mixed solution containing the precipitate obtained in the copper precipitation step S4 to adjust the pH, thereby obtaining a first neutralized solution.
[0069] In the copper precipitation step S4 as the previous step, the pH of the leachate from the start to the end of the addition of the hydrogen sulfide compound is maintained below 2.0. Therefore, in the case of maintaining this state, in the cobalt-nickel separation step S6 as the subsequent step, the hydrogen sulfide compound may not react easily with cobalt and nickel, but the pH of the eluate will decrease with the addition of the hydrogen sulfide compound. After the pH adjustment, if the pH is less than 3.0 when the hydrogen sulfide compound is added, the pH will drop excessively before the addition of the hydrogen sulfide compound is completed, and the pH needs to be adjusted again. Therefore, in the previous step of the cobalt-nickel separation step S6, it is more effective to set the pH to 3.0 or above.
[0070] Furthermore, when adjusting the pH, if the pH is set to a value exceeding 4.0, the pH adjustment takes time, and if a hydrogen sulfide compound is added, the pH immediately drops to 4.0 or less, which is inefficient. Therefore, the pH adjustment range is preferably 3.0 to 4.0.
[0071] Furthermore, in the first neutralization process S5A-1, the pH of the mixed solution containing the precipitate obtained in the copper precipitation step S5 is set to about 3.0 to 4.0 using sodium hydroxide (NaOH), so that the aluminum contained in the mixed solution can be precipitated as aluminum hydroxide (Al(OH)3).
[0072] In the first neutralization step S5A-1 of pH adjustment as a pretreatment of the cobalt-nickel separation step S6, potassium hydroxide (KOH) can be used as a pH adjustment liquid in addition to sodium hydroxide (NaOH), and if the pH exceeds 4.0, an acid (e.g., sulfuric acid) can be further used as a pH adjustment liquid. In this embodiment, the pH of the eluent is adjusted within the range of 3.0 to 4.0, for example, to 3.5.
[0073] Next, in the first filtering process S5A-2, the first neutralized liquid obtained in the first neutralization process S5A-1 is subjected to solid-liquid separation to separate the first eluent containing cobalt and nickel and the residue containing copper sulfide (CuS). Thus, the solid phase and the first eluent (liquid phase) are separated, and the solid phase includes: the carbon residue produced in the leaching process S3, the precipitation residue containing copper sulfide (CuS) produced in the copper precipitation process S4, and the aluminum hydroxide (Al(OH)3) produced in the first neutralization process S5A-1. The saturated aliphatic alcohol (straight-chain saturated alcohol) with a carbon number of 8 or less contained in the defoaming agent used in the leaching process S3 is transferred to the first eluent.
[0074] In addition, in this embodiment, the carbon residue generated in the leaching process S3 is also filtered out through solid-liquid separation in the first filtration process S5A-2, but by performing solid-liquid separation in the leaching process S3, the carbon residue can be separated in advance before performing the first filtration process S5A-2.
[0075] The solid phase separated in the first filtration step S5A-2 may be treated as waste after repulping (adding water to the solid phase to resuspend it and then purifying it by dehydration) or washing the filter cake.
[0076] (Cobalt-Nickel Separation Step S6)
[0077] Next, by adding a water-soluble hydrogen sulfide compound to the first eluate obtained in the first treatment step S5A, cobalt and nickel contained in the eluate are precipitated as water-insoluble cobalt sulfide (CoS) and nickel sulfide (NiS), respectively.
[0078] As the hydrogen sulfide compound used to sulfide the cobalt-nickel, for example, a water-soluble alkali metal hydrogen sulfide can be mentioned. The hydrogen sulfide compound can be the same as or different from the compound used in the copper precipitation step S4. In this embodiment, an aqueous solution of sodium hydrogen sulfide with a concentration of 250 g / L is used.
[0079] The addition of the aqueous solution of sodium hydrogen sulfide is performed, for example, until the oxidation-reduction potential (vs Ag / AgCl) reaches -400 mV or less. By adding sodium hydrogen sulfide until the oxidation-reduction potential reaches -400 mV or less, almost all of the cobalt and nickel contained in the eluent can be precipitated.
[0080] The pH of the leachate is preferably maintained in the range of 2.0 to 5.0, preferably in the range of 2.0 to 3.5, from the start to the end of the addition of the hydrogen sulfide compound. When the pH of the leachate is less than 2.0, a reaction between sodium hydrogen sulfide and sulfuric acid (NaSH+H2SO4→H2S+Na2SO4) will occur, and the sodium hydrogen sulfide will be consumed, making it difficult to sulfide cobalt and nickel. On the other hand, if the pH of the leachate exceeds 5.0, hydroxides of other metals may be generated and the purity of the precipitate may decrease. In addition, it is difficult to control the pH in the high range.
[0081] In addition, the cobalt sulfide mentioned here may include cobalt sulfide (II), cobalt disulfide (CoS2), cobalt octasulfide (Co9S8), etc. Cobalt sulfide compounds of various compositions. Similarly, nickel sulfide (NiS) may include nickel sulfide (II), nickel disulfide (NiS2), nickel tetrasulfide (Ni3S4), nickel disulfide (Ni3S2), etc. Nickel sulfide compounds of various compositions.
[0082] On the other hand, in the liquid phase (remaining liquid) after the addition of the hydrogen sulfide compound, metal components (manganese, iron, aluminum, lithium, calcium, etc.) other than cobalt and nickel remain. The liquid phase obtained here can be separated and recovered by solvent extraction using pH adjustment.
[0083] (Redissolution Step S7)
[0084] Next, a re-dissolving liquid containing dilute sulfuric acid is added to the sulfide (precipitate) containing cobalt and nickel obtained in the cobalt-nickel separation step S6 to react, thereby obtaining a cobalt-nickel solution containing cobalt and nickel.
[0085] In the redissolution step S7, for example, a precipitate is added to a redissolution solution heated to 50 to 60°C to obtain a suspension, and an oxidizing gas is blown into the suspension using a fine bubble generator to bubble the suspension. If the temperature of the suspension is lower than 50°C, the oxidation reaction is weakened, and if the temperature of the suspension exceeds 60°C, too much heat energy is required to maintain the temperature. In addition, the pH of the suspension is preferably in the range of 2.0 to 7.0, more preferably in the range of 3.0 to 7.0. The pH of the suspension may also be referred to as the pH of the suspension before bubbling. If the pH is less than 2.0, sulfur is not easily dissolved and forms a hard foam together with the gas blown into sulfur. If the pH exceeds 7.0, the dissolved cobalt and nickel become hydroxides and take away the hydroxide ions, so it is necessary to add an alkali agent to maintain the pH above 7.0, and the chemical cost becomes higher than sulfuric acid.
[0086] The oxygen concentration of the oxidizing gas used for bubbling is preferably 20 volume % or more. The oxidizing gas can be a gas containing oxygen, for example, air (oxygen concentration is about 20 volume %). In addition, an oxidizing gas having an oxygen concentration higher than that of air can also be used, for example, a gas having an oxygen concentration of 90 volume % or more or pure oxygen can be used as the oxidizing gas. If air is used as the oxidizing gas, the suspension can be bubbled at low cost. On the other hand, if an oxidizing gas having an oxygen concentration of 90 volume % or more is used, the dissolution time of cobalt and nickel can be accelerated, thereby enabling the redissolution process S7 to be effectively performed.
[0087] The fine bubbles (fine bubbles) used for bubbling in the redissolution step S7 may be any of microbubbles (bubble diameter of 1 μm or more and less than 100 μm) and ultrafine bubbles (nanobubbles: bubble diameter less than 1 μm). Such fine bubbles can be generated by using an air shearing microbubble generator or a nanobubble generator.
[0088] Furthermore, during bubbling, not only are fine bubbles blown into the container to which the suspension has been added, but the suspension is also sucked from the container to which the suspension has been added by a pump, etc., and fine bubbles are blown into the sucked suspension and caused to flow back into the container, thereby enabling the sulfide (precipitate) containing cobalt and nickel to be further effectively oxidized.
[0089] When bubbling of an oxidizing gas is performed into the suspension in the redissolution step S7 , cobalt sulfide (CoS) is dissolved in the suspension by reactions represented by the following formulas (1), (2), and (3).
[0090] CoS+O2+H2SO4→CoSO4+S+H2O……(1)
[0091] CoS+O2+H2O→Co(OH)2+S+H2O……(2)
[0092] S+O2+→SO4 2- ……(3)
[0093] Furthermore, nickel sulfide (NiS) is dissolved in the suspension through the reactions of the following formulas (4), (5), and (6).
[0094] NiS+O2+H2SO4→NiSO4+S+H2O……(4)
[0095] NiS+O2+H2O→Ni(OH)2+S+H2O……(5)
[0096] S+O2+→SO4 2- ……(6)
[0097] After the suspension is just started to be bubbled, since the suspension is acidic, the reactions of formula (1) and formula (4) are carried out, thereby increasing the pH of the suspension. If the suspension is neutral, the reactions of formula (2) and formula (5) occur. In addition, as the bubbling continues, the cobalt sulfide or nickel sulfide decreases, so the reactions of formula (3) and formula (6) are dominant, and the pH of the suspension decreases.
[0098] The pH of the suspension during bubbling is preferably in the range of more than 3.0 and less than 7.0. By setting the pH of the suspension during bubbling to more than 3.0, the reactions of formula (3) and formula (6) are carried out. When the pH of the suspension during bubbling is less than 3.0, the sulfur remains intact and does not become sulfuric acid, and foam is formed by sulfur and the oxidizing gas blown in by bubbling. Since the foam is not easy to break, a large amount of droplets will be contained in the suspension, which may hinder the operation. By setting the pH of the suspension during bubbling to less than 7.0, the reactions of formula (2) and formula (5) can be suppressed. When the pH of the suspension during bubbling exceeds 7.0, the reactions of formula (2) and formula (5) will occur, and the circulation device may be blocked by the generated hydroxide.
[0099] The bubbling conditions in the redissolution step S7 can be, for example, as follows: 1000 mL of a suspension containing 150 g of a precipitate (containing cobalt sulfide and nickel sulfide) (undried) is bubbled with an oxidizing gas having an oxygen concentration of 20% by volume or more at a flow rate of 0.1 L / min or more and 5 L / min or less for a period of 50 minutes or more and 12,000 minutes or less. The bubbling time is preferably 60 minutes or more and 3,000 minutes or less.
[0100] Furthermore, under the condition that the oxidizing gas is supplied to 1000 mL of the suspension at a flow rate of 0.1 L / min or more and 5 L / min or less, when the oxygen concentration of the oxidizing gas is 20% by volume, the bubbling time is preferably 250 minutes or more and 12000 minutes or less. When the oxygen concentration of the oxidizing gas is 100% by volume, the bubbling time is preferably 50 minutes or more and 2500 minutes or less. Thus, it is preferred to adjust the bubbling time in consideration of the oxygen concentration of the oxidizing gas.
[0101] If the bubbling time is less than 50 minutes, unreacted cobalt sulfide and nickel sulfide may be generated. If the bubbling time exceeds 12,000 minutes, unreacted cobalt sulfide and nickel sulfide disappear, so the treatment time may be unnecessarily extended.
[0102] Furthermore, in the redissolution step S7, in addition to sulfuric acid, a redissolution solution to which hydrogen peroxide is added can also be used. As hydrogen peroxide, for example, a hydrogen peroxide solution having a concentration of 30 mass % or less can be used. Hydrogen peroxide is preferably added at a time point when cobalt sulfide and nickel sulfide begin to dissolve in the suspension containing sulfuric acid.
[0103] In this way, by bubbling with an oxidizing gas and adding hydrogen peroxide to the suspension, the dissolution rate of cobalt sulfide and nickel sulfide can be accelerated, so that the redissolution step S7 can be performed in a shorter time. On the other hand, compared with the conventional redissolution step without bubbling, if bubbling and the addition of hydrogen peroxide are used together, the amount of expensive hydrogen peroxide used can be reduced, so that the redissolution step S7 can be performed at a lower cost.
[0104] By the above-mentioned re-dissolution step S7, cobalt sulfide and nickel sulfide are dissolved in the re-dissolution liquid. In addition, impurities that are not dissolved in the re-dissolution liquid, elemental sulfur generated in the cobalt-nickel separation step S6, etc. remain as a solid phase. Thereafter, by performing solid-liquid separation using a filter material or the like, a (purified) cobalt-nickel solution with improved purity of cobalt and nickel can be obtained.
[0105] The cobalt-nickel solution thus obtained contains almost no other components of the electrode material (copper, iron, aluminum, lithium, calcium, etc.) other than cobalt and nickel, and is suitable as a high-purity recovery raw material for cobalt and nickel.
[0106] In addition, as a pre-step of the re-dissolution step S7, it is also preferable to remove impurities other than cobalt sulfide and nickel sulfide in advance by re-slurrying the precipitate.
[0107] In the first neutralization process S5A-1, the step of removing aluminum before solid-liquid separation is as described above, but if this step is not performed, aluminum compounds may be contained in the precipitate. In this case, the aluminum compounds can be removed by re-slurrying the precipitate.
[0108] (Solvent extraction step S8)
[0109] Next, the extractant solution is added to the cobalt-nickel solution obtained in the redissolution step S7 to obtain a cobalt extract and a nickel extract.
[0110] As the extractant solution, a mixed solution of a metal extractant and a diluent can be used. For example, a mixed solution of 20 vol% 2-ethylhexyl 2-ethylhexylphosphonate (PC88A: manufactured by DAIHACHI CHEMICAL INDUSTRY CO., LTD.) and 80 vol% kerosene (diluent) can be used.
[0111] The extractant solution is used to separate and recover cobalt sulfate (CoSO4) solution and nickel sulfate (NiSO4) solution from the cobalt-nickel solution through a mixer-settler.
[0112] Through the above steps, cobalt and nickel can be recovered from waste LIBs with high yields. For example, when the amounts of cobalt and nickel in the electrode material taken out from the waste LIB are respectively set to 100%, the cobalt and nickel separation method of this embodiment can respectively recover cobalt and nickel with high yields of more than 95%.
[0113] (Second Embodiment)
[0114] Figure 2 This is a flow chart showing in stages the method for separating cobalt and nickel according to the second embodiment of the present invention.
[0115] In the second embodiment described below, description of the same steps as those in the first embodiment will be omitted.
[0116] In the second embodiment, between the copper precipitation step S4 and the cobalt-nickel separation step S6 , the second treatment step S5B is performed instead of the first treatment step S5A.
[0117] As the second treatment process S5B, a second filtration process S5B-1 and a second neutralization process S5B-2 are sequentially performed.
[0118] In the second filtering process S5B-1, the mixed liquid containing the precipitate obtained in the copper precipitation step S4 is subjected to solid-liquid separation to separate the first eluate containing cobalt and nickel and the residue containing copper sulfide (CuS). Thus, a solid phase and a second eluate (liquid phase) are separated, and the solid phase includes: the carbon residue generated in the leaching step S3, and the precipitate residue containing copper sulfide (CuS) generated in the copper precipitation step S4.
[0119] The solid phase separated in the second filtration process S5B-1 can be treated as waste after reslurrying (adding water to the solid phase to resuspend it, and then purifying it by dehydration) or washing the filter cake.
[0120] In the second neutralization process S5B-2, an alkali metal hydroxide is added to the second eluate obtained in the second filtration process S5B-1 to adjust the pH, thereby obtaining a second neutralized solution.
[0121] In the copper precipitation step S4 as the previous step, the pH of the leachate from the start to the end of the addition of the hydrogen sulfide compound is maintained below 2.0. Therefore, if this state is maintained, the hydrogen sulfide compound may not react easily with cobalt and nickel in the cobalt-nickel separation step S6 as the subsequent step. However, the pH of the eluate decreases with the addition of the hydrogen sulfide compound. After the pH is adjusted, if the pH is less than 3.0 when the hydrogen sulfide compound is added, the pH will decrease excessively before the addition of the hydrogen sulfide compound is completed, and the pH needs to be adjusted again. Therefore, it is more effective to set the pH to 3.0 or above in the previous step of the cobalt-nickel separation step S6.
[0122] Furthermore, when adjusting the pH, if the pH is set to a value exceeding 4.0, the pH adjustment takes time, and if a hydrogen sulfide compound is added, the pH immediately drops to 4.0 or less, which is inefficient. Therefore, the pH adjustment range is preferably 3.0 to 4.0.
[0123] Furthermore, in the second neutralization process S5B-2, by using sodium hydroxide (NaOH), the pH of the second eluate obtained in the second filtration process S5B-1 is set to about 3.0 to 4.0, so that the aluminum contained in the second eluate can be precipitated as aluminum hydroxide (Al(OH)3).
[0124] In the second neutralization process S5B-2 for pH adjustment as a pretreatment of the cobalt-nickel separation step S6, as a pH adjustment liquid for adjusting the pH of the eluent of about pH 1.0 to pH 3.0-4.0, potassium hydroxide (KOH) can be used in addition to sodium hydroxide (NaOH), and if the pH exceeds 4.0, an acid (e.g., sulfuric acid) can be further used as the pH adjustment liquid. In the present embodiment, a sodium hydroxide aqueous solution having a concentration of 25% by weight is used to adjust the pH of the second eluent to within the range of 3.0-4.0 (e.g., 3.5).
[0125] The embodiments of the present invention are described above, but these embodiments are presented as examples and are not intended to limit the scope of the invention. These embodiments can be implemented in various other ways, and various omissions, substitutions and changes can be made without departing from the scope of the technical features of the invention. These embodiments or their modifications are included in the scope of the invention or the technical features of the invention, and are included in the scope of the invention and its equivalents recorded in the claims.
[0126] Example
[0127] The effect of the method for separating cobalt and nickel according to the present embodiment was verified.
[0128] (Steps of the Example of the Present Invention)
[0129] The electrode material extracted from the waste LIB was added to a treatment solution containing 2 mol / L sulfuric acid and 30 mass % hydrogen peroxide, and heated and stirred for 4 hours at a liquid temperature of 60°C (leaching process). After that, the obtained leachate was naturally cooled to room temperature, and an aqueous sodium hydrogen sulfide solution (stirred and dissolved in ion exchange water to reach 250 g / L) was added to the leachate and stirred until the oxidation-reduction potential (ORP (Oxidation-reduction Potential)) of the leachate reached 0 mV (vs Ag / AgCl) or less (copper separation process).
[0130] At this stage, the carbon of the negative electrode material of the waste LIB that was insoluble during sulfuric acid leaching and the residue (copper sulfide) generated were filtered to separate the solid and liquid. A sodium hydroxide solution with a concentration of 25% by mass was added to the eluate obtained here to adjust the pH to 3.5. A sodium hydrogen sulfide aqueous solution with a concentration of 250 g / L was added to the obtained neutralized solution while stirring until the ORP reached -400 mV (vs Ag / AgCl) or less.
[0131] Then, it was confirmed that enough black precipitates (cobalt sulfide and nickel sulfide) were generated, and then solid-liquid separation was performed to recover the precipitates (cobalt-nickel separation step). On the other hand, impurities such as manganese, aluminum, iron, lithium, and calcium remained in the remaining liquid, which was treated as metal-containing waste liquid.
[0132] To 254.7 g (undried) of precipitate containing cobalt sulfide and nickel sulfide, 2000 mL of distilled water was added, and the liquid temperature was set to 60° C., sulfuric acid was added to make the pH reach 3.0, thereby obtaining a suspension. Then, air (oxidizing gas) was supplied to the suspension at a rate of 3.0 L / min using an air shearing microbubble generator, and the suspension was bubbled with the generated microbubbles (redissolution process). During the reaction, the pH of the suspension gradually increased, but the pH was adjusted using sulfuric acid so that the pH of the suspension was within the range of 3.0 or more and 7.0 or less.
[0133] Then, the air supply was stopped after 4 hours from the start of bubbling, and the pH of the suspension was adjusted to 3.0. Next, 40 mL of hydrogen peroxide with a concentration of 30% by mass was added and stirred for 30 minutes to redissolve all the cobalt sulfide and nickel sulfide. The dissolved residue was 1.3 g (dried). The leaching rates for cobalt sulfide and nickel sulfide obtained in the previous step were 98.4% by mass of cobalt and 99.5% by mass of nickel, confirming that both nickel and cobalt could be fully redissolved.
[0134] From the cobalt-nickel solution thus obtained, a cobalt sulfate solution and a nickel sulfate solution were separated and recovered by a mixer-settler using an extractant solution prepared by mixing 20 vol% PC88A (manufactured by DAIHACHI CHEMICAL INDUSTRY CO., LTD.) as a metal extractant and 80 vol% kerosene (solvent extraction step).
[0135] In the above steps of the present invention example, when the cobalt and nickel in the electrode material taken out from the waste LIB are set to 100%, the cobalt obtained in the stripping solution by solvent extraction is 96.4% and the nickel is 95.3%. Therefore, it is confirmed that according to the separation method of cobalt and nickel of this embodiment, cobalt and nickel can be recovered from the waste LIB with a high yield.
[0136] In addition, the metal concentration was measured by ICP-AES, the pH was measured by a pH meter, and the ORP was measured by an ORP meter. The numerical values of % are based on mass.
[0137] In the redissolution step of the method for separating cobalt and nickel of the present embodiment, the leaching rates of cobalt and nickel were measured and calculated using the following formulas when the suspension was bubbled and when bubbling and hydrogen peroxide were added. In addition, the residue after redissolution was washed with distilled water to recover the washing liquid.
[0138] Leaching rate (%) = 100 × {(liquid volume of leached filtrate × metal concentration) + (liquid volume of cleaning liquid × metal concentration of cleaning liquid)} / {(liquid volume of leached filtrate × metal concentration) + (liquid volume of cleaning liquid × metal concentration of cleaning liquid) + (mass of residue × metal content)}
[0139] (1) When only bubbling is performed (Example (1) of the present invention)
[0140] Table 1 shows the test results of redissolving the precipitate containing cobalt sulfide and nickel sulfide only by bubbling. The time (minutes) in the table represents the time elapsed from the start of blowing air. In addition, the pH, temperature, ORP, and air flow rate in the table are the values at each time point, the cumulative addition amount (sulfuric acid, NaOH) is the total addition amount at each time point, and the concentration and transfer rate represent the values at each time point. In addition, the transfer rate was calculated using the following formula.
[0141] Transfer rate (%) = 100 × (liquid volume × metal concentration) / {(liquid volume after filtration × metal concentration after filtration) + (liquid volume of cleaning liquid × metal concentration of cleaning liquid) + (weight of residue × metal content)}
[0142] In the formula, the value at each time point is used as the numerator, and the value at the end of the re-dissolution step is used as the denominator.
[0143] To 282.9 g (undried) of a precipitate containing cobalt sulfide and nickel sulfide, 2000 mL of distilled water was added, and the mixture was stirred while being heated to a liquid temperature of 50°C (Example A1). Next, 15 mL of sulfuric acid having a concentration of 47% by weight was added to bring the pH to below 3.0 (Example A2). Next, the change over time from the start of blowing air was confirmed, and sulfuric acid having a concentration of 47% by weight and a sodium hydroxide solution having a concentration of 25% by weight were appropriately added to bring the pH to 3.0 to 7.0, while blowing was performed for 600 minutes using an aspirator as a microbubble device (Examples A3 to A13).
[0144] The sulfur residue generated during the blowing was separated into solid and liquid by filtration to obtain 1910 mL of leaching solution and 500 mL of washing solution. The cobalt and nickel contents of 4.22 g of the sulfur residue are shown in Table 2, and the cobalt and nickel concentrations of the washing solution are shown in Table 3. When the leaching rate is calculated with the total amount of cobalt and nickel in the reaction system as 100%, 96.7% of cobalt and 98.8% of nickel are leached.
[0145] In addition, as the aspirator used as the bubbling means, Model 1-689-04 (manufactured by AS ONE Corporation) was used. This aspirator was made of polytetrafluoroethylene (PTFE), and the liquid flow rate was set to 10 L / min.
[0146] [Table 1]
[0147]
[0148] [Table 2]
[0149]
[0150] [Table 3]
[0151]
[0152] exist Figure 3 In the example (1) of the present invention shown, the leaching rate of nickel exceeded 80% about 2 hours after the start of bubbling, and reached 98% about 9 hours after the start of bubbling. The final leaching rate was 98.8%. In addition, the leaching rate of cobalt exceeded 80% about 4 hours after the start of bubbling, and reached 95% about 9 hours after the start of bubbling. The final leaching rate was 96.7%. It was confirmed that under the above-mentioned suspension conditions, if bubbling is performed for about 10 hours, almost all of cobalt and nickel can be leached (re-dissolved) without adding hydrogen peroxide.
[0153] (2) When bubbling and adding hydrogen peroxide (Example (2) of the present invention)
[0154] Table 4 shows the test results of re-dissolving the precipitate containing cobalt sulfide and nickel sulfide by bubbling and hydrogen peroxide. The time (minutes) in the table represents the time elapsed from the start of blowing air. In addition, the pH, temperature, ORP, and air flow rate in the table are the values at each time point, the cumulative addition amount (sulfuric acid, NaOH, hydrogen peroxide) is the total addition amount at each time point, and the concentration and transfer rate represent the values at each time point. In addition, the transfer rate was calculated using the following formula.
[0155] Transfer rate (%) = 100 × (liquid volume × metal concentration) / {(liquid volume after filtration × metal concentration after filtration) + (liquid volume of cleaning liquid × metal concentration of cleaning liquid) + (weight of residue × metal content)}
[0156] In the formula, the value at each time point is used as the numerator, and the value at the end of the re-dissolution step is used as the denominator.
[0157] To 254.7 g (undried) of a precipitate containing cobalt sulfide and nickel sulfide, 2000 mL of distilled water was added, and the mixture was stirred while being heated to a liquid temperature of 60°C (Example B1). Next, 9 mL of sulfuric acid having a concentration of 47% by weight was added to bring the pH to below 3.0 (Example B2). Next, the change over time from the start of blowing air was confirmed, and sulfuric acid having a concentration of 47% by weight and a sodium hydroxide solution having a concentration of 25% by weight were appropriately added to bring the pH to 3.0 to 7.0, while blowing was performed for 240 minutes using an aspirator as a microbubble device (Example B3 to Example B10).
[0158] After that, the blowing of air was stopped, and 40 mL of hydrogen peroxide with a concentration of 30% by weight was added over 25 minutes to dissolve the sulfur residue (Example B11 to Example B14). The sulfur residue generated during the blowing and addition of hydrogen peroxide was separated into solid and liquid by filtration to obtain 2020 mL of leaching solution and 400 mL of cleaning solution. The cobalt and nickel contents of 1.30 g of the sulfur residue are shown in Table 5, and the cobalt and nickel concentrations of the cleaning solution are shown in Table 6. When the leaching rate is calculated with the total amount of cobalt and nickel in the reaction system as 100%, 98.4% of cobalt is leached and 99.5% of nickel is leached.
[0159] [Table 4]
[0160]
[0161] [Table 5]
[0162]
[0163] [Table 6]
[0164]
[0165] exist Figure 4In the example (2) of the present invention shown, the leaching rate of nickel reached about 90% about 4 hours after the start of bubbling. The leaching rate of cobalt reached about 80% about 4 hours after the start of bubbling. After that, by reacting it with hydrogen peroxide, the final leaching rate of nickel reached 99.5%. And the final leaching rate of cobalt reached 98.4%. Therefore, it was confirmed that in addition to bubbling, further adding hydrogen peroxide can leach (redissolve) almost all of cobalt and nickel in about 4.5 hours, and it was confirmed that by bubbling, the amount of hydrogen peroxide used is only a small amount of about 40 mL.
[0166] (3) When bubbling is not performed (conventional example)
[0167] Table 7 shows the test results of re-dissolving the precipitate containing cobalt sulfide and nickel sulfide with hydrogen peroxide. The time (minutes) in the table indicates the time elapsed from the start of adding hydrogen peroxide. In addition, the pH, temperature, and ORP in the table are the values at each time point, the cumulative addition amount (sulfuric acid, hydrogen peroxide, NaOH) is the total addition amount at each time point, and the concentration and transfer rate indicate the values at each time point. In addition, the transfer rate was calculated using the following formula.
[0168] Transfer rate (%) = 100 × (liquid volume × metal concentration) / {(liquid volume after filtration × metal concentration after filtration) + (liquid volume of cleaning liquid × metal concentration of cleaning liquid) + (weight of residue × metal content)}
[0169] In the formula, the value at each time point is used as the numerator, and the value at the end of the re-dissolution step is used as the denominator.
[0170] 1000 mL of distilled water was added to 169.7 g (undried) of a precipitate containing cobalt sulfide and nickel sulfide, and the mixture was stirred while being heated to a liquid temperature of 60°C (C1). Next, 14 mL of sulfuric acid having a concentration of 47% by weight was added to adjust the pH to 2.0 or less (C2). The change over time from the start of the addition of hydrogen peroxide was confirmed, and while sulfuric acid having a concentration of 47% by weight was appropriately added to adjust the pH to 2.0 or less, a hydrogen peroxide solution having a concentration of 30% by weight was added over 140 minutes (C3 to C9).
[0171] After that, a sodium hydroxide solution with a concentration of 25% by weight and sulfuric acid with a concentration of 47% by weight were added to make the pH reach about 5.0 (C10-C11). Next, the generated sulfur residue was separated into solid and liquid by filtration to obtain 1260 mL of leaching solution and 355 mL of washing solution. The cobalt and nickel contents of 4.26 g of sulfur residue are shown in Table 8, and the cobalt and nickel concentrations of the washing solution are shown in Table 9. If the leaching rate is calculated when the total amount of cobalt and nickel in the reaction system is set to 100%, 99.4% of cobalt is leached and 99.6% of nickel is leached. It was confirmed that although leaching can be performed sufficiently, a large amount of hydrogen peroxide is required compared with the example, and the processing cost becomes high.
[0172] [Table 7]
[0173]
[0174] [Table 8]
[0175]
[0176] [Table 9]
[0177]
[0178] Industrial Applicability
[0179] The method for separating cobalt and nickel of the present embodiment can accurately separate and recover the valuable metals contained in the lithium-ion secondary battery after use, especially cobalt and nickel from other metals, thereby effectively obtaining high-purity recycling resources from the lithium-ion secondary battery. Therefore, the method for separating cobalt and nickel of the present embodiment has beneficial industrial applicability.
Claims
1. A method for separating cobalt and nickel from a lithium-ion secondary battery, characterized in that: The method for separating cobalt and nickel comprises: A leaching step, immersing the electrode material of the lithium ion secondary battery in a treatment solution containing sulfuric acid and hydrogen peroxide to obtain a leaching solution; a copper precipitation step, adding a hydrogen sulfide compound to the leaching solution and stirring the solution to precipitate copper in the form of copper sulfide; Any one of the first treatment step or the second treatment step, wherein: The first treatment process includes: a first neutralization process, adding an alkali metal hydroxide to the mixed solution containing the precipitate obtained in the copper precipitation process to adjust the pH to obtain a first neutralized solution; and a first filtration process, performing solid-liquid separation on the first neutralized solution to obtain a first eluate containing cobalt and nickel and a residue containing copper sulfide. The second treatment process includes: a second filtration process, in which the mixed solution containing the precipitate obtained in the copper precipitation process is subjected to solid-liquid separation to obtain a second eluate containing cobalt and nickel and a residue containing copper sulfide; and a second neutralization process, in which an alkali metal hydroxide is added to the second eluate to adjust the pH to obtain a second neutralized solution; a cobalt-nickel separation step, adding a hydrogen sulfide compound to the first eluate obtained in the first treatment step or the second neutralized solution obtained in the second treatment step, stirring and performing solid-liquid separation to obtain a precipitate containing cobalt sulfide and nickel sulfide and a residual liquid containing lithium; and a redissolution step of dissolving cobalt and nickel contained in the precipitate in a suspension obtained by suspending the precipitate separated in the cobalt-nickel separation step in dilute sulfuric acid to obtain a cobalt-nickel solution containing cobalt and nickel, The re-dissolving step is a step of bubbling the suspension with an oxidizing gas containing oxygen using a fine bubble generator.
2. The method for separating cobalt and nickel according to claim 1, characterized in that: The pH of the suspension is set within a range of 2.0 to 7.
0.
3. The method for separating cobalt and nickel according to claim 1 or 2, characterized in that: The bubbling in the redissolution step is performed by bubbling the oxidizing gas at a flow rate of 0.1 L / min to 5 L / min inclusive through 1000 mL of the suspension for 50 minutes to 12000 minutes inclusive.
4. The method for separating cobalt and nickel according to claim 1 or 2, characterized in that: The oxygen concentration of the oxidizing gas used in the redissolution step is 20% by volume or more.
5. The method for separating cobalt and nickel according to claim 1 or 2, characterized in that: In the re-dissolution step, the pH of the suspension during bubbling is within a range of 3.0 to 7.
0.
6. The method for separating cobalt and nickel according to claim 1 or 2, characterized in that: In the re-dissolving step, hydrogen peroxide is added to the suspension.
7. The method for separating cobalt and nickel according to claim 1 or 2, characterized in that: The first treatment step is performed as a post-step of the copper precipitation step.
8. The method for separating cobalt and nickel according to claim 1 or 2, characterized in that: As a pre-process of the leaching process, a pulverizing and sorting process is further provided: the lithium ion secondary battery is pulverized and classified to obtain an electrode material containing at least cobalt, nickel, copper and lithium.
9. The method for separating cobalt and nickel according to claim 1 or 2, characterized in that: The method further comprises a solvent extraction step of adding an extractant solution to the cobalt-nickel solution to obtain a cobalt extract solution and a nickel extract solution.
10. The method for separating cobalt and nickel according to claim 1 or 2, characterized in that: As a pre-step of the pulverization and separation step, a heat treatment step of heating the lithium ion secondary battery for heat treatment is further included.