Silver-containing anti-radiation spandex fabric and preparation method thereof

By immersing spandex fabric in aqueous solution of silver nitrate and fixing silver ions in polyurethane varnish, the problems of poor radiation resistance and weak metal bonding fastness of spandex fabric are solved, and strong anti-electromagnetic radiation performance is achieved, and after multiple washings, it is possible to achieve strong anti-electromagnetic radiation performance. Keep the effect.

CN118932700AInactive Publication Date: 2024-11-12WUHAN TEXTILE UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411004024.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-25
Publication Date
2024-11-12
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Spandex fabric has poor radiation resistance, and the bonding between metal and fabric is weak and easy to fall off, making it difficult to widely use in spandex fabrics.

Method used

After immersing the spandex fabric in the aqueous solution of silver nitrate and drying, it is further immersed in polyurethane varnish. The copper ions of amino groups and silver nitrate are coordinated by the copper ions of the amino group, and the polyurethane varnish is fixed on the surface of the fabric to enhance radiation resistance.

Benefits of technology

The good anti-electromagnetic radiation function of spandex fabric is achieved, the shielding performance at frequency points 300, 1000 and 2450MHz is significantly improved, and the radiation resistance is not weakened after multiple washings. The concentration of silver nitrate aqueous solution and finishing temperature have a beneficial effect on performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004962478160000041
    Figure BDA0004962478160000041
  • Figure BDA0004962478160000051
    Figure BDA0004962478160000051
Patent Text Reader

Abstract

The invention relates to a silver-containing anti-radiation spandex fabric and a preparation method thereof. The spandex fabric provided by the invention can be prepared by the following steps: firstly, immersing the spandex fabric into a silver nitrate aqueous solution, and drying after the reaction is finished; secondly, the treated spandex is soaked in polyurethane varnish, taken out and dried, and the anti-radiation spandex fabric is prepared. The anti-radiation spandex fabric prepared by the invention has a strong anti-electromagnetic radiation function, and when the frequency points are 300 MHz, 1000 MHz and 2450 MHz, the shielding effectiveness respectively reaches 41.370 dB, 44.681 dB and 49.385 dB; after five times of water washing, the anti-radiation function is still very stable and is not obviously weakened.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of fabric preparation, and in particular relates to a silver-containing radiation-proof spandex fabric and a preparation method thereof. Background Art

[0002] With the development of science and technology and people's increasing health awareness, consumers are increasingly pursuing functional clothing such as radiation protection, and functional fabrics have great development prospects. Spandex fabrics have good physical properties, low development costs, and good development prospects. At present, there are roughly three ways to improve the radiation protection performance of textiles: one is to directly use fibers with good radiation protection as raw materials to produce textiles, such as carbon fiber; the second is to add radiation protection substances during spinning to achieve the purpose of radiation protection; the third is to perform radiation protection finishing on the fabric, such as impregnating the fabric with radiation blocking agents, or applying radiation protection coatings on the fabric surface. However, these three manufacturing methods have their drawbacks and new solutions need to be sought.

[0003] Spandex fabrics are widely used, but their radiation protection performance is poor. Metals have radiation protection functions, but the bonding strength between metal and fabric is weak and easy to fall off, so metals are difficult to be widely used on spandex fabrics.

[0004] Therefore, in order to solve the above problems, it is urgent to find a method for implanting metal into spandex fabric to achieve the purpose of the radiation protection function of spandex fabric. Summary of the invention

[0005] In order to overcome the shortcomings of the prior art that the metal and fabric have weak bonding strength and are easy to fall off, the present invention provides a silver-containing radiation-proof spandex fabric and a preparation method thereof.

[0006] The first purpose of the present invention is to provide a silver-containing radiation-proof spandex fabric, which is achieved by the following scheme: first, the spandex fabric is immersed in a silver nitrate aqueous solution and dried after the reaction is completed; secondly, the treated spandex is immersed in polyurethane varnish, taken out, and dried to obtain the radiation-proof spandex fabric.

[0007] The second object of the present invention is to provide a method for preparing a silver-containing radiation-proof spandex fabric, the preparation method comprising the following steps:

[0008] (1) The spandex fabric is immersed in a 1-3 g / L silver nitrate aqueous solution for 30-60 min, the finishing temperature is controlled at 70-90° C., and the fabric is dried after the reaction is completed.

[0009] Preferably, the usage ratio of the spandex fabric to the silver nitrate aqueous solution is 1 g: (10-12) mL.

[0010] (2) Immersing the spandex treated in step (1) in polyurethane varnish for 10 to 20 minutes, taking it out, and drying it to obtain a radiation-proof spandex fabric.

[0011] Preferably, the usage ratio of the spandex fabric to the polyurethane varnish is 1 g: (20-30) mL.

[0012] The mechanism of the present invention is as follows: In view of the shortcomings of the prior art that the metal and fabric are weak in bonding and easy to fall off, the present invention converts the amino group (-NH 2 ) and copper ions of silver nitrate (Ag + ) coordination, polyurethane varnish will Ag + Fixed on the fabric surface, thus realizing the radiation protection function of spandex fabric.

[0013] The present invention has the following significant advantages:

[0014] (1) The bonding strength between metal and fabric is weak and easy to fall off; the inventors of the present application unexpectedly found that by using the impregnation finishing method, the amino group (-NH 2 ) and copper ions of silver nitrate (Ag + ) coordination, polyurethane varnish will Ag + The spandex fabric obtained by fixing it on the surface of the fabric has good radiation protection function; after repeated washing, the radiation protection function of the fabric remains unchanged.

[0015] (2) The radiation-proof spandex fabric prepared by the present invention has a strong anti-electromagnetic radiation function. When the frequency points are 300, 1000 and 2450 MHz, the shielding effectiveness reaches 41.370, 44.681 and 49.385 dB respectively; the appropriate concentration of silver nitrate aqueous solution and finishing temperature are conducive to improving the anti-electromagnetic radiation performance of the fabric. DETAILED DESCRIPTION

[0016] The above scheme is further described below in conjunction with specific examples. It should be understood that these examples are used to illustrate the present application and are not limited to the scope of the present application. The implementation conditions adopted in the examples can be further adjusted according to the conditions of the specific manufacturer, and the implementation conditions not specified are usually the conditions in conventional experiments.

[0017] Main raw material sources: Polyurethane varnish was purchased from Shandong Haiheng Industrial Coatings Co., Ltd.

[0018] Example 1

[0019] A silver-containing radiation-proof spandex fabric, which is prepared by the following method:

[0020] (1) 100 g of spandex fabric was immersed in 1100 mL of 2 g / L silver nitrate aqueous solution for 45 min, the finishing temperature was controlled at 80 °C, and the fabric was dried after the reaction was completed.

[0021] (2) 100 g of the spandex treated in step (1) was immersed in 2500 mL of polyurethane varnish for 15 min, then taken out and dried to obtain radiation-proof spandex fabric a.

[0022] Example 2

[0023] A silver-containing radiation-proof spandex fabric, which is prepared by the following method:

[0024] (1) 100 g of spandex fabric was immersed in 1000 mL of 1 g / L silver nitrate aqueous solution for 30 min, the finishing temperature was controlled at 70 °C, and the fabric was dried after the reaction was completed.

[0025] (2) 100 g of the spandex treated in step (1) was immersed in 2000 mL of polyurethane varnish for 10 min, then taken out and dried to obtain radiation-proof spandex fabric b.

[0026] Example 3

[0027] A silver-containing radiation-proof spandex fabric, which is prepared by the following method:

[0028] (1) 100 g of spandex fabric was immersed in 1200 mL of 3 g / L silver nitrate aqueous solution for 60 min, the finishing temperature was controlled at 90 °C, and the fabric was dried after the reaction was completed.

[0029] (2) 100 g of the spandex treated in step (1) was immersed in 3000 mL of polyurethane varnish for 20 min, taken out, and dried to obtain radiation-proof spandex fabric c.

[0030] Comparative Example A

[0031] Taking Example 1 as a comparison, in this comparative example A, the concentration of the silver nitrate aqueous solution is reduced, that is, the "2 g / L silver nitrate aqueous solution" in step (1) is adjusted to "0.02 g / L silver nitrate aqueous solution", and the other preparation methods are implemented according to the preparation method of Example 1 to obtain fabric d.

[0032] Comparative Example B

[0033] Taking Example 1 as a comparison, in this comparative example B, the finishing temperature is lowered, that is, "the finishing temperature is controlled to be 80°C" in step (1) is adjusted to "the finishing temperature is controlled to be 20°C", and the other preparation methods are implemented according to the preparation method of Example 1 to obtain fabric e.

[0034] Performance Testing:

[0035] The fabrics a, b, c, d, e prepared in the above-mentioned specific embodiments 1 to 3 and comparative examples A to B of the present invention and the unfinished spandex fabric f were selected; the finished fabrics a to e were washed 5 times, and then the radiation protection performance was tested with the unfinished spandex fabric f. The electromagnetic shielding effectiveness of the fabrics was tested with reference to GB / T 30142-2013 "Measurement Method for Shielding Effectiveness of Planar Electromagnetic Shielding Materials", and the test results are shown in the following table.

[0036]

[0037]

[0038] It can be seen from GB / T 30142-2013 "Measurement Method for Shielding Effectiveness of Planar Electromagnetic Shielding Materials" that at the same frequency point (MHz), the higher the shielding effectiveness (dB), the better the electromagnetic radiation protection performance of the fabric. It can be seen from the table that the radiation-proof spandex fabrics a, b, and c prepared in Examples 1 to 3 have significantly stronger radiation protection performance than the radiation-proof spandex fabrics d and e prepared in Comparative Examples A to B, and the unfinished spandex fabric f has the worst radiation protection performance; among them, for fabric a in Example 1, when the frequency points are 300, 1000, and 2450MHz, the shielding effectiveness reaches 41.370, 44.681, and 49.385dB, respectively; in addition, the concentration of silver nitrate aqueous solution and the finishing temperature have a great influence on the electromagnetic radiation protection performance of the radiation-proof spandex fabric, and the appropriate concentration of silver nitrate aqueous solution and the finishing temperature are conducive to improving the electromagnetic radiation protection performance of the fabric.

Claims

1. A method for preparing a silver-containing radiation-proof spandex fabric, characterized in that: The preparation method comprises the following steps: (1) immersing the spandex fabric in a 1-3 g / L silver nitrate aqueous solution for 30-60 min, controlling the finishing temperature to be 70-90° C., and drying after the reaction is completed; (2) Immersing the spandex treated in step (1) in polyurethane varnish for 10 to 20 minutes, taking it out, and drying it to obtain a radiation-proof spandex fabric.

2. The method for preparing a silver-containing radiation-proof spandex fabric according to claim 1, characterized in that: The usage ratio of the spandex fabric to the silver nitrate aqueous solution in step (1) is 1 g: (10-12) mL.

3. The method for preparing a silver-containing radiation-proof spandex fabric according to claim 1, characterized in that: The usage ratio of the spandex fabric to the polyurethane varnish in step (2) is 1 g: (20-30) mL.

4. A silver-containing radiation-proof spandex fabric, characterized in that: The invention is prepared by the method according to any one of claims 1 to 3.