Sodium supplementing agent, preparation method of sodium supplementing agent, positive plate, preparation method of positive plate and electrochemical device

By using water-absorbing materials to coat the sodium source material and introducing conductive agents in the sodium supplement agent, the problem of water sensitivity of the positive sodium supplement agent is solved, and the cycle stability and first discharge capacity of the battery are improved.

CN118943313AActive Publication Date: 2024-11-12CONTEMPORARY AMPEREX TECHNOLOGY CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202310538734.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-12
Publication Date
2024-11-12
Estimated Expiration
2043-05-12

AI Technical Summary

Technical Problem

Existing positive electrode sodium supplementation agents are sensitive to water and are prone to adsorbing water to form strong alkaline compounds, affecting battery cycle stability.

Method used

The sodium supplement agent is introduced as a cladding layer to coat the sodium-source material, reduce the contact between the sodium-source material and moisture, improve the migration rate of sodium ions through conductive agents, and control particle size and mixing conditions to optimize the sodium-source material.

Benefits of technology

It effectively reduces the generation of strong alkaline substances, improves the cycle stability and first discharge capacity of the battery, and enhances the migration efficiency of sodium ions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The invention discloses a sodium supplement and a preparation method thereof, a positive plate and a preparation method thereof, and an electrochemical device. The sodium supplementing agent comprises an inner core and a coating layer at least partially coating the inner core, the inner core comprises a sodium source material, and the material of the coating layer comprises a water-absorbing material. The inner core is at least partially coated in the coating layer, so that when the sodium supplementing agent is in contact with water during use, the water absorbing material of the coating layer firstly contacts with the water, the water is fixed in the water absorbing material, and the sodium source material of the inner core is coated by the water absorbing material of the coating layer, so that the contact between the sodium source material and the water is reduced; strong alkaline compounds formed on the surface of the positive electrode are reduced, and the influence on the battery cycling stability is weakened.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of battery technology, and in particular to a sodium supplement, a method for preparing the sodium supplement, a positive electrode sheet, a method for preparing the positive electrode sheet, and an electrochemical device. Background Art

[0002] Positive electrode sodium replenishment technology usually introduces sodium replenishers into the positive electrode materials. Traditionally, sodium powder, sodium salt, organic sodium-containing solutions, etc. are the main ones. The activity of metallic sodium makes it highly sensitive to water, making the positive electrode sodium replenisher more sensitive to moisture. When the sodium replenisher is mixed with the positive electrode material, it is easy to absorb moisture and form strong alkaline compounds on the positive electrode surface, which in turn affects the battery cycle stability. Summary of the invention

[0003] The present application is made in view of the above-mentioned problems, and its purpose is to provide a sodium supplement to reduce the absorption of water during the mixing process of the sodium supplement and the positive electrode material, reduce the formation of strong alkaline compounds on the positive electrode surface, and reduce the impact on the battery cycle stability.

[0004] In order to achieve the above-mentioned purpose, the embodiments of the present application provide a sodium supplement, a method for preparing the sodium supplement, a positive electrode sheet, a method for preparing the positive electrode sheet, and an electrochemical device.

[0005] In a first aspect, an embodiment of the present application provides a sodium supplement, comprising a core and a coating layer at least partially coating the core, wherein the core comprises a sodium source material, and the material of the coating layer comprises a water-absorbing material.

[0006] Therefore, in the technical solution of the embodiment of the present application, a water-absorbing material is added to the sodium supplement, and the core is at least partially coated in the coating layer, so that when the sodium supplement comes into contact with moisture during use, the first thing to come into contact with moisture is the water-absorbing material of the coating layer, and the moisture is fixed in the water-absorbing material, while the sodium source material of the core is coated by the water-absorbing material of the coating layer, thereby reducing the contact between the sodium source material and moisture, reducing the formation of strong alkaline compounds on the surface of the positive electrode, and reducing the impact on the battery cycle stability.

[0007] In any embodiment, the mass ratio of the sodium source material to the water-absorbing material is (1-5):1. Optionally, the mass ratio of the sodium source material to the water-absorbing material is (2-3):1. When the mass ratio of the sodium source material is higher than that of the water-absorbing material, sufficient sodium source can be used for the irreversible sodium loss of the first discharge, thereby improving the cycle stability of the battery. When the mass ratio of the sodium source material to the water-absorbing material is less than 1:1, the proportion of the sodium source material is relatively small, the sodium supplement effect is not obvious, and the sodium in the electrode needs to be consumed, which reduces the capacity of the battery. At the same time, the proportion of the water-absorbing material is relatively high, making the water-absorbing material coated on the outer layer of the sodium source material too thick, making it difficult for sodium ions to escape, and the sodium supplement effect is not good. When the mass ratio of the sodium source material to the water-absorbing material is greater than 5:1, the proportion of the water-absorbing material is relatively small, which is not conducive to fully reacting with water. Part of the sodium source material will react with the water that is not absorbed by the water-absorbing material to produce a strong alkaline substance, which will corrode the electrode and reduce the capacity of the electrode.

[0008] In any embodiment, the coating layer also includes a conductive agent. Since the water-absorbing material is usually a material with weak conductivity, the sodium source material is coated in the water-absorbing material, and the migration rate of sodium ions is slowed down. The conductive agent and silica gel are interpenetrated with each other, so that the sodium source material coated in the water-absorbing material can migrate out quickly. The conductive agent introduced on the outer surface of the sodium supplementer provides a channel for the migration of the sodium source material, thereby improving the migration rate of the sodium source material in the sodium supplementer.

[0009] In any embodiment, the mass of the sodium source material and the water-absorbing material is M1, and the mass of the conductive agent is M2, wherein M1:M2 is (1.5-8):1; optionally, M1:M2 is (2-5):1. The sum of the masses of the sodium source material and the water-absorbing material is greater than the mass of the conductive agent, so that while increasing the release of sodium ions, the remaining conductive agent can be reduced, the amount of inert substances can be reduced, and the interference with the electrode can be reduced. When M1:M2 is less than 1.5:1, the mass of the conductive agent is too much, and after the sodium ions are released, more inert substances remain, affecting the performance of the electrode. When M1:M2 is greater than 8:1, the mass of the conductive agent is too little, the ability of sodium ions to migrate is insufficient, and the release efficiency of sodium ions is low.

[0010] In any embodiment, the conductive agent includes but is not limited to at least one of conductive carbon black, conductive graphite, acetylene black and Ketjen black. The above conductive agents can increase the migration rate of sodium ions and improve the initial discharge capacity of the electrochemical device.

[0011] In any embodiment, the water-absorbing material includes but is not limited to at least one of silica gel, porous carbon and activated alumina. The above water-absorbing materials can absorb water while coating the sodium source material, thereby reducing the generation of strong alkaline substances by the reaction between the sodium source material and water.

[0012] In any embodiment, the sodium source material includes but is not limited to at least one of Na2O, Na2CO3, NaF and Na2S. The above sodium source materials can be used to better supplement the sodium source for the first discharge of the electrode and compensate for the irreversible sodium loss of the electrode.

[0013] In any embodiment, the particle size of the sodium supplement is 1 to 200 μm, and optionally, the particle size of the sodium supplement is 100 to 150 μm. By controlling the particle size of the sodium supplement, water molecules can be adsorbed in the water-absorbing material, while providing a channel for the escape of sodium ions. When the particle size of the sodium supplement is less than 1 μm, the particle size of the sodium supplement is too small, the specific surface area of ​​the sodium supplement increases, and it is easy to agglomerate and cannot play an effective role. When the particle size of the sodium supplement is greater than 200 μm, the particle size of the sodium supplement is too large, which affects the escape of internal sodium ions and is not conducive to sodium supplementation.

[0014] In a second aspect, the present application provides a method for preparing a sodium supplement, which is used to prepare the sodium supplement of the first aspect of the present application, comprising the following steps:

[0015] The material of the inner core is mixed with the molten material of the coating layer, and granulated after solidification to obtain the sodium supplement.

[0016] The sodium supplement is obtained by mixing the core material with the molten coating material, solidifying and granulating, so that the core sodium source material is at least partially coated in the coating water-absorbing material, reducing the contact between the sodium source material and moisture, reducing the generation of strong alkaline substances, and reducing corrosion to the electrode.

[0017] In any embodiment, the step of mixing the material of the core with the molten material of the coating layer, and granulating after solidification to obtain the sodium supplement comprises:

[0018] Mixing a sodium source material and a conductive agent to obtain a first mixture;

[0019] The water-absorbing material is melted and then mixed with the first mixture to obtain a second mixture. The second mixture is solidified and granulated to obtain a sodium supplement.

[0020] The sodium source material and the conductive agent are first mixed so that the sodium source material contacts the conductive agent, thereby providing a channel for the escape of sodium ions. At the same time, the sodium source material and the conductive agent are at least partially coated in a water-absorbing material to protect the sodium source material and reduce the generation of strong alkaline substances when the sodium source material contacts water.

[0021] In any embodiment, the step is to melt the water-absorbing material and mix it with the first mixture to obtain a second mixture, and then solidify the second mixture and granulate it to obtain a sodium supplement.

[0022] After the water-absorbing material is melted, the speed of mixing with the first mixture is 1000-8000 r / min. Optionally, after the water-absorbing material is melted, the speed of mixing with the first mixture is 3000-6000 r / min. By controlling the mixing speed, the sodium supplement material and the conductive agent can be evenly dispersed in the water-absorbing material, thereby improving the sodium supplement effect. When the mixing speed is less than 1000 r / min, the mixing uniformity is poor. When the mixing speed is greater than 8000 r / min, due to excessive shear force, adverse side reactions will occur, thereby producing substances that are not conducive to sodium supplementation; and / or,

[0023] After the water-absorbing material is melted, the time for mixing with the first mixture is 10 to 60 minutes. Optionally, after the water-absorbing material is melted, the time for mixing with the first mixture is 20 to 40 minutes. By controlling the mixing time, the sodium supplement material and the conductive agent can be evenly dispersed in the water-absorbing material, thereby improving the sodium supplement effect. When the mixing time is less than 10 minutes, the mixing uniformity is poor. When the mixing time is greater than 60 minutes, the mixing time is too long, affecting the production capacity. And / or,

[0024] Granulation after solidifying the second mixture includes stirring granulation, wherein the granulation speed is 1000-8000r / min, optionally, the granulation speed is 3000-6000r / min; by controlling the speed during granulation, the particle size of the sodium supplement can be controlled, thereby both absorbing water in the water-absorbing material and providing a migration channel for the sodium ions to escape. When the granulation speed is less than 1000r / min, the particle size of the sodium supplement is likely to be too large, making it difficult for sodium ions to escape and the sodium supplementation effect is not good. When the granulation speed is greater than 8000r / min, the particle size of the sodium supplement is likely to be too small, causing water molecules to migrate in the sodium supplement, combine with the sodium supplement material, generate strong alkaline substances, and corrode the electrode. And / or,

[0025] Granulation after solidifying the second mixture includes stirring granulation, wherein the granulation time is 3 to 10 minutes, and optionally, the granulation time is 4 to 6 minutes. The particle size of the sodium supplement can be controlled by controlling the granulation time, so that water can be adsorbed in the water-absorbing material and a migration channel can be provided for the sodium ions to escape. When the granulation time is greater than 10 minutes, the particle size of the sodium supplement is likely to be too small, causing water molecules to migrate in the sodium supplement, combine with the sodium supplement material, generate a strong alkaline substance, and corrode the electrode. When the granulation time is less than 3 minutes, the particle size of the sodium supplement is likely to be too large, making it difficult for sodium ions to escape, and the sodium supplement effect is not good.

[0026] In any embodiment, the step of mixing the sodium source material with the conductive agent to obtain a first mixture,

[0027] The method of mixing the sodium source material with the conductive agent includes grinding and mixing, and the mixing time is 5 to 30 minutes, and optionally, the mixing time is 8 to 15 minutes. By controlling the mixing time of the sodium source material and the conductive agent, the sodium source material and the conductive agent can be fully mixed, thereby providing a channel for the escape of sodium ions, which is convenient for sodium supplementation. When the mixing time is less than 5 minutes, the mixing is uneven, and the sodium source material and the conductive agent are not in sufficient contact. When the mixing time is greater than 30 minutes, side reactions will occur, which is not conducive to sodium supplementation.

[0028] In any embodiment, the temperature for melting the water-absorbing material is 200-300°C, and optionally, the temperature for melting the water-absorbing material is 240-260°C. By controlling the melting temperature of the water-absorbing material, the sodium-supplementing material can be at least partially coated in the molten water-absorbing material, thereby reducing the contact between the sodium-supplementing material and water, reducing the production of strong alkaline substances, and reducing corrosion to the electrode. When the melting temperature is lower than 200°C, the water-absorbing material cannot be completely melted, and the coating property is poor. When the melting temperature is higher than 300°C, the water-absorbing material may produce irreversible side reactions, generate substances that are not conducive to coating, and reduce the protection of the sodium source material.

[0029] In a third aspect, an embodiment of the present application provides a positive electrode sheet, comprising the sodium supplement agent of the first aspect of the present application and a positive electrode material.

[0030] In any embodiment, the positive electrode material includes a positive electrode active material, a conductive material, and a binder.

[0031] In any embodiment, the mass ratio of the positive electrode active material, the conductive material, the binder and the sodium supplement is (70-90): (3-20): (3-20): (3-20), optionally, the mass ratio of the positive electrode active material, the conductive material, the binder and the sodium supplement is (80-85): (5-10): (5-10): (5-10). By controlling the mass ratio of the positive electrode active material, the conductive material, the binder and the sodium supplement, a better sodium supplement effect can be obtained. When the sodium supplement is too much, after the sodium supplement is completed, the water-absorbing material left is an inert substance and no longer participates in the transmission of charge. The sodium supplement accounts for a large proportion, so there are too many remaining inert substances. The sodium in the sodium supplement can only be removed but not embedded, and the occupied volume is too large, which is not conducive to improving the capacity of the electrode and affects the performance of the electrode. When the sodium supplement is too little, during the sodium supplement process, the sodium source of the sodium supplement is insufficient, and the sodium in the electrode needs to be consumed, which affects the performance of the electrode.

[0032] In any embodiment, the positive electrode active material includes but is not limited to at least one of sodium vanadium phosphate, sodium manganate, sodium vanadium manganese phosphate, sodium cobaltate, sodium Prussian blue, and sodium vanadium fluorophosphate. A positive electrode with high activity can be obtained by using the above positive electrode active materials.

[0033] In any embodiment, the binder includes but is not limited to polyvinylidene fluoride, vinylidene fluoride-hexafluoropropylene copolymer, vinylidene fluoride-tetrafluoroethylene copolymer, vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene copolymer, vinylidene fluoride-pentafluoropropylene copolymer, vinylidene fluoride-pentafluoropropylene-tetrafluoroethylene copolymer, vinylidene fluoride-perfluoromethyl vinyl ether-tetrafluoroethylene copolymer, vinylidene fluoride-chlorotrifluoroethylene copolymer, polytetrafluoroethylene, polychlorotrifluoroethylene, tetrafluoroethylene-perfluoroalkyl vinyl ether copolymer, ethylene-tetrafluoroethylene copolymer, ethylene-chlorotrifluoroethylene copolymer and tetrafluoroethylene-hexafluoropropylene copolymer. The positive electrode active material, the conductive agent and the sodium supplement material can be bonded to the current collector by the above-mentioned binder to provide good performance for the electrode.

[0034] In any embodiment, the conductive material includes but is not limited to at least one of conductive carbon black, superconducting carbon black, conductive graphite, acetylene black, Ketjen black, graphene and carbon nanotubes. The conductive material can obtain good conductivity and improve the capacity of the electrode.

[0035] In a fourth aspect, an embodiment of the present application provides a method for preparing a positive electrode sheet, which is used to prepare the positive electrode sheet of the third aspect of the present application, comprising the following steps:

[0036] The sodium supplement material and the positive electrode material are mixed in a solvent, coated on the surface of the positive electrode current collector, and dried, cold pressed and cut to obtain the positive electrode sheet.

[0037] By mixing the sodium supplement material with the positive electrode material and coating it on the surface of the positive electrode current collector, a positive electrode sheet containing the sodium supplement agent can be obtained, thereby reducing the irreversible sodium loss in the positive electrode sheet.

[0038] In any embodiment, the solvent includes N-methylpyrrolidone. Using N-methylpyrrolidone can well mix the sodium supplement material with the positive electrode material, which is convenient for sodium supplementation.

[0039] In a fifth aspect, an embodiment of the present application provides an electrochemical device, comprising the positive electrode sheet of the third aspect of the present application.

[0040] In any embodiment, the electrochemical device comprises a capacitor, a primary battery, or a secondary battery. DETAILED DESCRIPTION

[0041] The following specifically discloses the implementation methods of the sodium supplement, the preparation method of the sodium supplement, the solar power generation device, and the power consumption device of the present application. However, there may be cases where unnecessary detailed descriptions are omitted. For example, there are cases where detailed descriptions of well-known matters and repeated descriptions of actually the same structures are omitted. This is to avoid the following description from becoming unnecessarily lengthy and to facilitate the understanding of those skilled in the art. In addition, the following description is provided for those skilled in the art to fully understand the present application and is not intended to limit the subject matter described in the claims.

[0042] "Scope" disclosed in the present application is limited in the form of lower limit and upper limit, and a given range is limited by selecting a lower limit and an upper limit, and the selected lower limit and upper limit define the boundary of a special range. The scope limited in this way can be including end values ​​or not including end values, and can be arbitrarily combined, that is, any lower limit can be combined with any upper limit to form a scope. For example, if the scope of 60-120 and 80-110 is listed for a specific parameter, it is understood that the scope of 60-110 and 80-120 is also expected. In addition, if the minimum range values ​​1 and 2 are listed, and if the maximum range values ​​3, 4 and 5 are listed, the following scope can be all expected: 1-3, 1-4, 1-5, 2-3, 2-4 and 2-5. In the present application, unless otherwise specified, the numerical range "ab" represents the abbreviation of any real number combination between a and b, wherein a and b are real numbers. For example, the numerical range "0-5" means that all real numbers between "0-5" are listed in this document, and "0-5" is just an abbreviation of these numerical combinations. In addition, when a parameter is expressed as an integer ≥ 2, it is equivalent to disclosing that the parameter is, for example, an integer of 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.

[0043] Unless otherwise specified, all embodiments and optional embodiments of the present application can be combined with each other to form a new technical solution.

[0044] Unless otherwise specified, all technical features and optional technical features of this application can be combined with each other to form a new technical solution.

[0045] If there is no special explanation, all steps of the present application can be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), which means that the method may include steps (a) and (b) performed sequentially, or may include steps (b) and (a) performed sequentially. For example, the method may further include step (c), which means that step (c) may be added to the method in any order. For example, the method may include steps (a), (b) and (c), or may include steps (a), (c) and (b), or may include steps (c), (a) and (b), etc.

[0046] If there is no special explanation, the "include" and "comprising" mentioned in this application represent open-ended or closed-ended expressions. For example, the "include" and "comprising" may represent that other components not listed may also be included or only the listed components may be included or only the listed components may be included.

[0047] If not specifically stated, in this application, the term "or" is inclusive. For example, the phrase "A or B" means "A, B, or both A and B". More specifically, any of the following conditions satisfies the condition "A or B": A is true (or exists) and B is false (or does not exist); A is false (or does not exist) and B is true (or exists); or both A and B are true (or exist).

[0048] When a sodium-ion battery is discharged for the first time, a benign film called positive electrode interface (CEI) will be formed on the surface of the positive electrode, consuming some sodium ions. After these sodium ions form the CEI film, they can no longer be used for the extraction and embedding of sodium ions. For the positive electrode, these sodium ions are irreversible sodium loss, which will reduce the capacity of the battery and make the actual capacity of the battery lower than the theoretical capacity.

[0049] Therefore, there are endless sodium supplementation technologies for the positive electrode. For example, a method for preparing a positive electrode sodium supplement, wherein the sodium supplement is mainly sodium powder, sodium salt, organic sodium solution, etc. However, the activity of metallic sodium leads to its high sensitivity to water, making the positive electrode sodium supplement more sensitive to moisture. The sodium supplement is easy to absorb moisture during the mixing process with the positive electrode material, forming a strong alkaline compound on the positive electrode surface, thereby affecting the battery cycle stability. The preparation method of the sodium supplement mostly uses aqueous solvents or physical mixing methods, which cannot avoid the adsorption of moisture.

[0050] Unexpectedly, by setting the sodium supplementer as a sodium source material at least partially coated by a water-absorbing material, the sodium source material is coated in the water-absorbing material, thereby reducing the contact between the sodium source material and water, reducing ultrasonic strong alkaline substances, and improving battery stability.

[0051] Based on this, the present application provides a sodium supplement, a method for preparing the sodium supplement, a positive electrode sheet, a method for preparing the positive electrode sheet, and an electrochemical device.

[0052] In a first aspect, an embodiment of the present application provides a sodium supplement, comprising a core and a coating layer at least partially coating the core, wherein the core comprises a sodium source material, and the material of the coating layer comprises a water-absorbing material.

[0053] Therefore, in the technical solution of the embodiment of the present application, a water-absorbing material is added to the sodium supplement, and the core is at least partially coated in the coating layer, so that when the sodium supplement comes into contact with moisture during use, the first thing to come into contact with moisture is the water-absorbing material of the coating layer, and the moisture is fixed in the water-absorbing material, while the sodium source material of the core is coated by the water-absorbing material of the coating layer, thereby reducing the contact between the sodium source material and moisture, reducing the formation of strong alkaline compounds on the surface of the positive electrode, and reducing the impact on the battery cycle stability.

[0054] In any embodiment, the mass ratio of the sodium source material to the water-absorbing material is (1-5):1. Optionally, the mass ratio of the sodium source material to the water-absorbing material is (2-3):1. When the mass ratio of the sodium source material is higher than that of the water-absorbing material, sufficient sodium source can be used for the irreversible sodium loss of the first discharge, thereby improving the cycle stability of the battery. When the mass ratio of the sodium source material to the water-absorbing material is less than 1:1, the proportion of the sodium source material is relatively small, the sodium supplement effect is not obvious, and the sodium in the electrode needs to be consumed, which reduces the capacity of the battery. At the same time, the proportion of the water-absorbing material is relatively high, making the water-absorbing material coated on the outer layer of the sodium source material too thick, making it difficult for sodium ions to escape, and the sodium supplement effect is not good. When the mass ratio of the sodium source material to the water-absorbing material is greater than 5:1, the proportion of the water-absorbing material is relatively small, which is not conducive to fully reacting with water. Part of the sodium source material will react with the water that is not absorbed by the water-absorbing material to produce a strong alkaline substance, which will corrode the electrode and reduce the capacity of the electrode.

[0055] In any embodiment, the coating layer also includes a conductive agent. Since the water-absorbing material is usually a material with weak conductivity, the sodium source material is coated in the water-absorbing material, and the migration rate of sodium ions is slowed down. The conductive agent and silica gel are interpenetrated with each other, so that the sodium source material coated in the water-absorbing material can migrate out quickly. The conductive agent introduced on the outer surface of the sodium supplementer provides a channel for the migration of the sodium source material, thereby improving the migration rate of the sodium source material in the sodium supplementer.

[0056] In any embodiment, the mass of the sodium source material and the water-absorbing material is M1, and the mass of the conductive agent is M2, wherein M1:M2 is (1.5-8):1; optionally, M1:M2 is (2-5):1. The sum of the masses of the sodium source material and the water-absorbing material is greater than the mass of the conductive agent, so that while increasing the release of sodium ions, the remaining conductive agent can be reduced, the amount of inert substances can be reduced, and the interference with the electrode can be reduced. When M1:M2 is less than 1.5:1, the mass of the conductive agent is too much, and after the sodium ions are released, more inert substances remain, affecting the performance of the electrode. When M1:M2 is greater than 8:1, the mass of the conductive agent is too little, the ability of sodium ions to migrate is insufficient, and the release efficiency of sodium ions is low.

[0057] In any embodiment, the conductive agent includes but is not limited to at least one of conductive carbon black, conductive graphite, acetylene black and Ketjen black. The above conductive agents can increase the migration rate of sodium ions and improve the initial discharge capacity of the electrochemical device.

[0058] In any embodiment, the water-absorbing material includes but is not limited to at least one of silica gel, porous carbon and activated alumina. The above water-absorbing materials can absorb water while coating the sodium source material, thereby reducing the generation of strong alkaline substances by the reaction between the sodium source material and water.

[0059] In any embodiment, the sodium source material includes but is not limited to at least one of Na2O, Na2CO3, NaF and Na2S. The above sodium source materials can be used to better supplement the sodium source for the first discharge of the electrode and compensate for the irreversible sodium loss of the electrode.

[0060] In any embodiment, the particle size of the sodium supplement is 1 to 200 μm, and optionally, the particle size of the sodium supplement is 100 to 150 μm. By controlling the particle size of the sodium supplement, water molecules can be adsorbed in the water-absorbing material, while providing a channel for the escape of sodium ions. When the particle size of the sodium supplement is less than 1 μm, the particle size of the sodium supplement is too small, the specific surface area of ​​the sodium supplement increases, and it is easy to agglomerate and cannot play an effective role. When the particle size of the sodium supplement is greater than 200 μm, the particle size of the sodium supplement is too large, which affects the escape of internal sodium ions and is not conducive to sodium supplementation.

[0061] In a second aspect, the present application provides a method for preparing a sodium supplement, which is used to prepare the sodium supplement of the first aspect of the present application, comprising the following steps:

[0062] The material of the inner core is mixed with the molten material of the coating layer, and granulated after solidification to obtain the sodium supplement.

[0063] The sodium supplement is obtained by mixing the material of the inner core with the material of the molten coating layer, granulating the mixture after solidification, so that the sodium source material is at least partially coated in the water-absorbing material, thereby reducing the contact between the sodium source material and moisture, reducing the generation of strong alkaline substances, and reducing corrosion to the electrode.

[0064] In any embodiment, the step of mixing the material of the core with the molten material of the coating layer, and granulating after solidification to obtain the sodium supplement comprises:

[0065] Mixing a sodium source material and a conductive agent to obtain a first mixture;

[0066] The water-absorbing material is melted and then mixed with the first mixture to obtain a second mixture. The second mixture is solidified and granulated to obtain a sodium supplement.

[0067] The sodium source material and the conductive agent are first mixed so that the sodium source material contacts the conductive agent, thereby providing a channel for the escape of sodium ions. At the same time, the sodium source material and the conductive agent are at least partially coated in a water-absorbing material to protect the sodium source material and reduce the generation of strong alkaline substances when the sodium source material contacts water.

[0068] In any embodiment, the step is to melt the water-absorbing material and mix it with the first mixture to obtain a second mixture, and then solidify the second mixture and granulate it to obtain a sodium supplement.

[0069] After the water-absorbing material is melted, the speed of mixing with the first mixture is 1000-8000 r / min. Optionally, after the water-absorbing material is melted, the speed of mixing with the first mixture is 3000-6000 r / min. By controlling the mixing speed, the sodium supplement material and the conductive agent can be evenly dispersed in the water-absorbing material, thereby improving the sodium supplement effect. When the mixing speed is less than 1000 r / min, the mixing uniformity is poor. When the mixing speed is greater than 8000 r / min, due to excessive shear force, adverse side reactions will occur, thereby producing substances that are not conducive to sodium supplementation; and / or,

[0070] After the water-absorbing material is melted, the time for mixing with the first mixture is 10 to 60 minutes. Optionally, after the water-absorbing material is melted, the time for mixing with the first mixture is 20 to 40 minutes. By controlling the mixing time, the sodium supplement material and the conductive agent can be evenly dispersed in the water-absorbing material, thereby improving the sodium supplement effect. When the mixing time is less than 10 minutes, the mixing uniformity is poor. When the mixing time is greater than 60 minutes, the mixing time is too long, affecting the production capacity; and / or,

[0071] Granulation after solidifying the second mixture includes stirring granulation, wherein the granulation speed is 1000-8000r / min, optionally, the granulation speed is 3000-6000r / min; by controlling the speed during granulation, the particle size of the sodium supplement can be controlled, thereby both absorbing water in the water-absorbing material and providing a migration channel for the sodium ions to escape. When the granulation speed is less than 1000r / min, the particle size of the sodium supplement is likely to be too large, making it difficult for sodium ions to escape and the sodium supplementation effect is not good. When the granulation speed is greater than 8000r / min, the particle size of the sodium supplement is likely to be too small, causing water molecules to migrate in the sodium supplement, combine with the sodium supplement material, generate strong alkaline substances, and corrode the electrode; and / or,

[0072] Granulation after solidifying the second mixture includes stirring granulation, wherein the granulation time is 3 to 10 minutes, and optionally, the granulation time is 4 to 6 minutes. The particle size of the sodium supplement can be controlled by controlling the granulation time, so that water can be adsorbed in the water-absorbing material and a migration channel can be provided for the sodium ions to escape. When the granulation time is greater than 10 minutes, the particle size of the sodium supplement is likely to be too small, causing water molecules to migrate in the sodium supplement, combine with the sodium supplement material, generate a strong alkaline substance, and corrode the electrode. When the granulation time is less than 3 minutes, the particle size of the sodium supplement is likely to be too large, making it difficult for sodium ions to escape, and the sodium supplement effect is not good.

[0073] In any embodiment, the step of mixing the sodium source material with the conductive agent to obtain a first mixture,

[0074] The method of mixing the sodium source material with the conductive agent includes grinding and mixing, and the mixing time is 5 to 30 minutes, and optionally, the mixing time is 8 to 15 minutes. By controlling the mixing time of the sodium source material and the conductive agent, the sodium source material and the conductive agent can be fully mixed, thereby providing a channel for the escape of sodium ions, which is convenient for sodium supplementation. When the mixing time is less than 5 minutes, the mixing is uneven, and the sodium source material and the conductive agent are not in sufficient contact. When the mixing time is greater than 30 minutes, side reactions will occur, which is not conducive to sodium supplementation.

[0075] In any embodiment, the temperature for melting the water-absorbing material is 200-300°C, and optionally, the temperature for melting the water-absorbing material is 240-260°C. By controlling the melting temperature of the water-absorbing material, the sodium-supplementing material can be at least partially coated in the molten water-absorbing material, thereby reducing the contact between the sodium-supplementing material and water, reducing the production of strong alkaline substances, and reducing corrosion to the electrode. When the melting temperature is lower than 200°C, the water-absorbing material cannot be completely melted, and the coating property is poor. When the melting temperature is higher than 300°C, the water-absorbing material may produce irreversible side reactions, generate substances that are not conducive to coating, and reduce the protection of the sodium source material.

[0076] In a third aspect, an embodiment of the present application provides a positive electrode sheet, comprising the sodium supplement agent of the first aspect of the present application and a positive electrode material.

[0077] In any embodiment, the positive electrode material includes a positive electrode active material, a conductive material, and a binder.

[0078] In any embodiment, the mass ratio of the positive electrode active material, the conductive material, the binder and the sodium supplement is (70-90): (3-20): (3-20): (3-20), optionally, the mass ratio of the positive electrode active material, the conductive material, the binder and the sodium supplement is (80-85): (5-10): (5-10): (5-10). By controlling the mass ratio of the positive electrode active material, the conductive material, the binder and the sodium supplement, a better sodium supplement effect can be obtained. When the sodium supplement is too much, after the sodium supplement is completed, the water-absorbing material left is an inert substance and no longer participates in the transmission of charge. The sodium supplement accounts for a large proportion, so there are too many remaining inert substances. The sodium in the sodium supplement can only be removed but not embedded, and the occupied volume is too large, which is not conducive to improving the capacity of the electrode and affects the performance of the electrode. When the sodium supplement is too little, during the sodium supplement process, the sodium source of the sodium supplement is insufficient, and the sodium in the electrode needs to be consumed, which affects the performance of the electrode.

[0079] In any embodiment, the positive electrode active material includes but is not limited to at least one of sodium vanadium phosphate, sodium manganate, sodium vanadium manganese phosphate, sodium cobaltate, sodium Prussian blue, and sodium vanadium fluorophosphate. A positive electrode with high activity can be obtained by using the above positive electrode active materials.

[0080] In any embodiment, the binder includes but is not limited to polyvinylidene fluoride, vinylidene fluoride-hexafluoropropylene copolymer, vinylidene fluoride-tetrafluoroethylene copolymer, vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene copolymer, vinylidene fluoride-pentafluoropropylene copolymer, vinylidene fluoride-pentafluoropropylene-tetrafluoroethylene copolymer, vinylidene fluoride-perfluoromethyl vinyl ether-tetrafluoroethylene copolymer, vinylidene fluoride-chlorotrifluoroethylene copolymer, polytetrafluoroethylene, polychlorotrifluoroethylene, tetrafluoroethylene-perfluoroalkyl vinyl ether copolymer, ethylene-tetrafluoroethylene copolymer, ethylene-chlorotrifluoroethylene copolymer and tetrafluoroethylene-hexafluoropropylene copolymer. The positive electrode active material, the conductive agent and the sodium supplement material can be bonded to the current collector by the above-mentioned binder to provide good performance for the electrode.

[0081] In any embodiment, the conductive material includes but is not limited to at least one of conductive carbon black, superconducting carbon black, conductive graphite, acetylene black, Ketjen black, graphene and carbon nanotubes. The conductive material can obtain good conductivity and improve the capacity of the electrode.

[0082] In a fourth aspect, an embodiment of the present application provides a method for preparing a positive electrode sheet, which is used to prepare the positive electrode sheet of the third aspect of the present application, comprising the following steps:

[0083] The sodium supplement material and the positive electrode material are mixed in a solvent, coated on the surface of the positive electrode current collector, and dried, cold pressed and cut to obtain the positive electrode sheet.

[0084] By mixing the sodium supplement material with the positive electrode material and coating it on the surface of the positive electrode current collector, a positive electrode sheet containing the sodium supplement agent can be obtained, thereby reducing the irreversible sodium loss in the positive electrode sheet.

[0085] In any embodiment, the solvent includes N-methylpyrrolidone. Using N-methylpyrrolidone can well mix the sodium supplement material with the positive electrode material, which is convenient for sodium supplementation.

[0086] In a fifth aspect, an embodiment of the present application provides an electrochemical device, comprising the positive electrode sheet of the third aspect of the present application.

[0087] In any embodiment, the electrochemical device includes, but is not limited to, a capacitor, a primary battery, or a secondary battery.

[0088] When the electrochemical device is a button-type full battery, it also includes an electrolyte and a negative electrode sheet, and the electrolyte includes but is not limited to a NaClO4 solution.

[0089] The technical solution of the present invention is further described in detail below in conjunction with specific embodiments. It should be understood that the following embodiments are only used to explain the present invention, and are not used to limit the present invention.

[0090] The parameters of the sodium supplements of Examples 1 to 35 of the present application and Comparative Examples 1 to 3 are according to the parameters in Table 1.

[0091] Table 1 Parameters of sodium supplements in Examples 1 to 35 and Comparative Examples 1 to 3

[0092]

[0093]

[0094]

[0095] Embodiment 36

[0096] A method for preparing a sodium supplement comprises the following steps:

[0097] The material of the inner core is mixed with the molten material of the coating layer, and granulated after solidification to obtain the sodium supplement.

[0098] Embodiment 37

[0099] A method for preparing a sodium supplement comprises the following steps:

[0100] Mixing a sodium source material and a conductive agent to obtain a first mixture;

[0101] The water-absorbing material is melted and then mixed with the first mixture to obtain a second mixture. The second mixture is solidified and granulated to obtain a sodium supplement.

[0102] Embodiment 38

[0103] Grinding and mixing the sodium source material and the conductive agent to obtain a first mixture;

[0104] The water-absorbing material is melted and then mixed with the first mixture to obtain a second mixture. The second mixture is solidified and granulated to obtain a sodium supplement.

[0105] The preparation methods of the sodium supplements of Examples 39 to 75 of the present application are the same as those of Example 38, except that the parameters are as shown in Table 2.

[0106] Table 2 Preparation parameters of sodium supplements of Examples 36 to 75 and Comparative Examples 4 to 5

[0107]

[0108]

[0109] Comparative Example 4

[0110] A method for preparing a sodium supplement comprises the following steps:

[0111] The water-absorbing material is mixed with the sodium source material to obtain a sodium supplement.

[0112] Comparative Example 5

[0113] A method for preparing a sodium supplement comprises the following steps:

[0114] The water-absorbing material is melted and mixed with the sodium source material to obtain a sodium supplement.

[0115] Embodiment 76

[0116] A positive electrode sheet comprises a sodium supplement and a positive electrode material.

[0117] Embodiment 77

[0118] A positive electrode sheet comprises a sodium supplement and a positive electrode material, wherein the positive electrode material comprises a positive electrode active substance, a conductive material and a binder.

[0119] The positive electrode materials of Examples 78 to 88 of the present application differ from those of Example 77 in the parameters shown in Table 3.

[0120] Table 3 Parameters of positive electrode materials of Examples 78 to 88

[0121]

[0122] The sodium supplements of Examples 1 to 35 and Comparative Examples 1 to 3 were prepared into button-type full batteries, the sodium supplements prepared by the preparation methods of the sodium supplements of Examples 36 to 75 and Comparative Examples 4 to 5 were prepared into button-type full batteries, and the positive electrodes of Examples 76 to 88 were prepared into button-type full batteries, and the following tests were performed:

[0123] Electrical performance test

[0124] First cycle efficiency: The battery is charged and discharged for the first time at 20mAg-1 in the voltage range of 2.5-4.4V (vs.Na+ / Na). First efficiency = first discharge capacity / first charge capacity.

[0125] Cycle performance: The sodium ion battery was subjected to cyclic charge and discharge test at 20 mAg-1 in the voltage range of 2.0 to 4.4 V for 300 cycles to obtain the initial charge and discharge capacity and the charge and discharge capacity after different numbers of cycles. The cycle capacity retention rate = discharge capacity / charge capacity.

[0126] The statistical experimental results are shown in Table 4.

[0127] Table 4 Performance measurement of sodium supplements of Examples 1 to 88 and Comparative Examples 1 to 5

[0128]

[0129]

[0130]

[0131]

[0132] As can be seen from Table 4, through Examples 1 to 4 and Comparative Examples 1 to 3, it can be seen that by adding sodium source material and water-absorbing material to the sodium supplement, the sodium source material is at least partially coated in the water-absorbing material, the cycle performance of the battery is significantly improved, and the difference between charging and discharging is significantly reduced. Among them, although the sodium source in Examples 1 to 3 is easy to combine with hydrogen ions to generate water or carbon dioxide gas during the charging and discharging process, affecting the cycle performance of the material, the water-absorbing material acrylic resin in Example 1 is less water-absorbing than silica gel, and the calcium silicate and calcium oxide in Examples 2 to 3 will introduce additional metal ions, the electrical properties of Examples 1 to 3 are still better than those of Comparative Examples 1 to 3.

[0133] It can be seen from Examples 4 to 10 that a suitable mass ratio of the sodium source material to the water-absorbing material can improve the cycle performance of the battery.

[0134] It can be seen from Examples 11 to 15 that different conductive agents and sodium source materials can improve the cycle performance of the battery, and the best effect is achieved when the water-absorbing material is silica gel.

[0135] It can be seen from Examples 17 to 25 that different M1:M2 will have an effect on the cycle performance of the battery. The sum of the masses of the sodium source material and the water-absorbing material is greater than the mass of the conductive agent, which can reduce the remaining conductive agent while improving the release of sodium ions, reduce the amount of inert substances, and reduce interference with the electrode. When M1:M2 is less than 1.5:1, the mass of the conductive agent is too much, and after the sodium ions are released, more inert substances remain, affecting the performance of the electrode. When M1:M2 is greater than 8:1, the mass of the conductive agent is too little, the ability of sodium ions to migrate is insufficient, and the sodium ion release efficiency is low.

[0136] It can be seen from Examples 26 to 35 that different sodium supplement particle sizes have an effect on the cycle performance of the battery. By controlling the particle size of the sodium supplement, water molecules can be adsorbed in the water-absorbing material, while providing a channel for the escape of sodium ions. When the particle size of the sodium supplement is less than 1 μm, the particle size of the sodium supplement is too small, the specific surface area of ​​the sodium supplement increases, and it is easy to agglomerate and cannot play an effective role. When the particle size of the sodium supplement is greater than 200 μm, the particle size of the sodium supplement is too large, which affects the escape of internal sodium ions and is not conducive to sodium supplementation.

[0137] It can be seen from Examples 36 to 38 and Comparative Examples 4 to 5 that the coating of the sodium source material with the water-absorbing material has a greater impact on improving the cycle performance of the battery. Compared with Comparative Example 4, Examples 36 to 38 can all improve the cycle performance of the battery.

[0138] It can be seen from Examples 39 to 44 that the mixing speed has a certain influence on the cycle performance of the battery. By controlling the mixing speed, the sodium supplement material and the conductive agent can be evenly dispersed in the water-absorbing material, thereby improving the sodium supplement effect. When the mixing speed is less than 1000r / min, the mixing uniformity is poor. When the mixing speed is greater than 8000r / min, due to the excessive shear force, unfavorable side reactions will occur, thereby producing substances that are not conducive to sodium supplementation.

[0139] It can be seen from Examples 45 to 50 that the mixing time has a certain influence on the cycle performance of the battery. By controlling the mixing time, the sodium supplement material and the conductive agent can be evenly dispersed in the water-absorbing material, thereby improving the sodium supplement effect. When the mixing time is less than 10 minutes, the mixing uniformity is poor.

[0140] It can be seen from Examples 51 to 56 that the rotation speed of granulation has a certain influence on the cycle performance of the battery.

[0141] It can be seen from Examples 57 to 62 that the granulation time has a certain influence on the cycle performance of the battery.

[0142] It can be seen from Examples 63 to 68 that the grinding and mixing time has a certain influence on the cycle performance of the battery.

[0143] It can be seen from Examples 69 to 75 that the melting temperature has a certain influence on the cycle performance of the battery.

[0144] It can be seen from Examples 77 to 88 that the ratio of positive electrode active material: conductive material: the binder: sodium supplement has a certain influence on the cycle performance of the battery. By controlling the mass ratio of the positive electrode active material, the conductive material, the binder and the sodium supplement, a better sodium supplement effect can be obtained. When there is too much sodium supplement, after the sodium supplement is completed, the water-absorbing material left is an inert substance and no longer participates in the transmission of charge. The sodium supplement accounts for a large proportion, so there are too many remaining inert substances. The sodium in the sodium supplement can only be removed but not embedded, and the volume occupied is too much, which is not conducive to improving the capacity of the electrode and affects the performance of the electrode. When there is too little sodium supplement, during the sodium supplement process, the sodium source of the sodium supplement is insufficient, and the sodium in the electrode needs to be consumed, which affects the performance of the electrode.

[0145] In summary, in the sodium supplement proposed in the present application, a water-absorbing material is added to the sodium supplement, and the sodium source material is at least partially coated in the water-absorbing material, so that when the sodium supplement comes into contact with moisture during use, the first thing to come into contact with moisture is the water-absorbing material of the coating layer, and the moisture is fixed in the water-absorbing material, while the sodium source material in the core is coated by the water-absorbing material of the coating layer, thereby reducing the contact between the sodium source material and moisture, reducing the formation of strong alkaline compounds on the surface of the positive electrode, and reducing the impact on the battery cycle stability.

[0146] The above are only preferred embodiments of the present invention, and do not limit the patent scope of the present invention. For those skilled in the art, the present invention may have various changes and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the patent protection scope of the present invention.

Claims

1. A sodium supplement, characterized in that The invention comprises an inner core and a coating layer at least partially coating the inner core, wherein the inner core comprises a sodium source material, and the coating layer comprises a water-absorbing material.

2. The sodium supplement as claimed in claim 1, characterized in that The mass ratio of the sodium source material to the water-absorbing material is (1-5):

1. Optionally, the mass ratio of the sodium source material to the water-absorbing material is (2-3):

1.

3. The sodium supplement according to claim 1 or 2, characterized in that The coating layer also includes a conductive agent.

4. The sodium supplement as claimed in claim 3, characterized in that The mass of the sodium source material and the water-absorbing material is M1, and the mass of the conductive agent is M2, wherein: M1:M2 is (1.5~8):1; optionally, M1:M2 is (2~5):

1.

5. The sodium supplement according to claim 3 or 4, characterized in that The conductive agent includes at least one of conductive carbon black, conductive graphite, acetylene black and Ketjen black.

6. The sodium supplement according to any one of claims 1 to 5, characterized in that The water-absorbing material includes at least one of silica gel, porous carbon and activated alumina.

7. The sodium supplement according to any one of claims 1 to 6, characterized in that The sodium source material includes at least one of Na2O, Na2CO3, NaF and Na2S.

8. The sodium supplement according to any one of claims 1 to 7, characterized in that The particle size of the sodium supplement is 1 to 200 μm. Optionally, the particle size of the sodium supplement is 100 to 150 μm.

9. A method for preparing the sodium supplement according to any one of claims 1 to 8, characterized in that: The following steps are involved: The material of the inner core is mixed with the molten material of the coating layer, and granulated after solidification to obtain the sodium supplement.

10. The method for preparing the sodium supplement according to claim 9, characterized in that: The steps of mixing the core material with the molten coating material, solidifying and granulating to obtain the sodium supplement include: Mixing a sodium source material and a conductive agent to obtain a first mixture; The water-absorbing material is melted and then mixed with the first mixture to obtain a second mixture. The second mixture is solidified and granulated to obtain a sodium supplement.

11. The method for preparing the sodium supplement according to claim 10, characterized in that: The step comprises: melting the water-absorbing material and mixing it with the first mixture to obtain a second mixture; solidifying the second mixture and granulating it to obtain a sodium supplement; After the water-absorbing material is melted, the rotation speed of mixing with the first mixture is 1000-8000 r / min. Optionally, after the water-absorbing material is melted, the rotation speed of mixing with the first mixture is 3000-6000 r / min; and / or, After the water-absorbing material is melted, the time for mixing with the first mixture is 10 to 60 minutes. Optionally, after the water-absorbing material is melted, the time for mixing with the first mixture is 20 to 40 minutes; and / or, Granulating the solidified second mixture includes stirring granulation, wherein the granulation speed is 1000-8000 r / min, and optionally, the granulation speed is 3000-6000 r / min; and / or, Granulating the second mixture after solidification includes stirring granulation, wherein the granulation time is 3 to 10 minutes, and optionally, the granulation time is 4 to 6 minutes.

12. The method for preparing the sodium supplement according to claim 10 or 11, characterized in that: Step: mixing the sodium source material with the conductive agent to obtain a first mixture, The sodium source material and the conductive agent are mixed by grinding and mixing for 5 to 30 minutes, and optionally for 8 to 15 minutes.

13. The method for preparing the sodium supplement according to any one of claims 10 to 12, characterized in that: The temperature for melting the water-absorbing material is 200-300°C. Optionally, the temperature for melting the water-absorbing material is 240-260°C.

14. A positive electrode sheet, characterized in that: It comprises the sodium supplement agent as described in any one of claims 1 to 8 and a positive electrode material.

15. The positive electrode sheet according to claim 14, characterized in that: The positive electrode material includes a positive electrode active material, a conductive material, and a binder.

16. The positive electrode sheet according to claim 15, characterized in that: The mass ratio of the positive electrode active material, the conductive material, the binder and the sodium supplement is (70-90):(3-20):(3-20):(3-20), optionally, The mass ratio of the positive electrode active material, the conductive material, the binder and the sodium supplement is (80-85):(5-10):(5-10):(5-10).

17. The positive electrode sheet according to claim 15 or 16, characterized in that: The positive electrode active material includes at least one of sodium vanadium phosphate, sodium manganate, sodium vanadium manganese phosphate, sodium cobaltate, sodium Prussian blue, and sodium vanadium fluorophosphate.

18. The positive electrode sheet according to any one of claims 15 to 17, characterized in that: The binder includes at least one of polyvinylidene fluoride, vinylidene fluoride-hexafluoropropylene copolymer, vinylidene fluoride-tetrafluoroethylene copolymer, vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene copolymer, vinylidene fluoride-pentafluoropropylene copolymer, vinylidene fluoride-pentafluoropropylene-tetrafluoroethylene copolymer, vinylidene fluoride-perfluoromethyl vinyl ether-tetrafluoroethylene copolymer, vinylidene fluoride-chlorotrifluoroethylene copolymer, polytetrafluoroethylene, polychlorotrifluoroethylene, tetrafluoroethylene-perfluoroalkyl vinyl ether copolymer, ethylene-tetrafluoroethylene copolymer, ethylene-chlorotrifluoroethylene copolymer and tetrafluoroethylene-hexafluoropropylene copolymer.

19. The positive electrode sheet according to any one of claims 15 to 18, characterized in that: The conductive material includes at least one of conductive carbon black, superconducting carbon black, conductive graphite, acetylene black, Ketjen black, graphene and carbon nanotubes.

20. A method for preparing a positive electrode sheet according to any one of claims 14 to 19, characterized in that: The following steps are involved: The sodium supplement material and the positive electrode material are mixed in a solvent, coated on the surface of the positive electrode current collector, and dried, cold pressed and cut to obtain the positive electrode sheet.

21. The method for preparing a positive electrode sheet according to claim 20, characterized in that: The solvent includes N-methylpyrrolidone.

22. An electrochemical device, characterized in that: Comprising the positive electrode sheet as described in any one of claims 14 to 19.

23. The electrochemical device according to claim 22, characterized in that The electrochemical device includes a capacitor, a primary battery, or a secondary battery.

Citation Information

Patent Citations

  • Silicon-oxygen pre-lithiated negative electrode and preparation method and application thereof

    CN113488612A

  • Lithium supplement material, positive pole piece and preparation method of positive pole piece

    CN114639812A

  • Current collector and manufacturing method thereof

    CN114899410A