Coating method and sheet

By optimizing the composition of the coating device and coating liquid, the problems of uneven coating and film thickness deviation were solved, and uniform coating of high thermal conductivity insulation layer was achieved, which is suitable for the heat dissipation requirements of electronic equipment.

CN118946414APending Publication Date: 2024-11-12NHK SPRING CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380030146.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-31
Filing Date
2023-01-11
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Existing coating methods often result in uneven coating and film thickness deviations when coating solutions with increased filler content form a coating film, affecting mass production.

Method used

A coating apparatus of a specific size, including a conveyor roller and a doctor blade coater, is used to control the viscosity of the coating liquid and the filler ratio, reduce the amount of coating liquid supplied in the gaps, and suppress resin flowability and filler sedimentation.

Benefits of technology

It effectively suppresses coating unevenness and film thickness deviation, improves coating uniformity and production efficiency, and is suitable for the formation of high thermal conductivity insulation layers.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118946414A_ABST
    Figure CN118946414A_ABST
Patent Text Reader

Abstract

The present invention provides a coating method which, when forming a coating film on the surface of a substrate using a coating liquid having an increased content of a filler, suppresses unevenness of the coating film and also suppresses variation in the thickness of the coating film. A coating method for forming a coating film (C) on the surface of a base material (W) using a coating device (1) provided with: a conveyance roller (2) for conveying the base material (W); a blade coater (3) which is arranged with a gap from the conveying roller (2) and is provided with a blade part (3b); and a liquid storage member (4), one end portion (4a) of which is positioned on the side of the transport roller (2) and which defines a liquid storage space (S) between the liquid storage member (4) and the transport roller (2), in the coating method, the coating liquid (L) contains a resin, a solvent, and a filler, the content of the filler is 65-95 parts by mass per 100 parts by mass of a mixture of the resin and the filler, the outer diameter D1 of the transport roller (2) is 50-270 mm, the outer diameter D2 of the blade coater (3) is 50-170 mm, and the outer diameter D2 of the blade coater (3) is 50-170 mm. The distance (D3) from the gap to the one end (4a) is 1-120 mm.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a coating method and a sheet material. Background Art

[0002] Various circuit substrates have been used since ancient times. For example, Patent Documents 1 and 2 show circuit substrates in which a circuit pattern is stacked on a base substrate via an insulating layer. The insulating layer has a function of ensuring the withstand voltage between the base substrate and the circuit pattern. In addition, by including a filler in the insulating layer, the thermal conductivity of the insulating layer can be ensured by the filler. With this circuit substrate, heat generated in an electronic component provided on the circuit pattern and transferred to the circuit pattern can be transferred to the base substrate via the insulating layer, and released from the base substrate to the outside.

[0003] The insulating layer can be obtained, for example, by preparing a sheet having a coating film of an insulating layer forming composition formed on the surface of a substrate such as a polyethylene terephthalate (PET) film, and thermally transferring the coating film of the sheet to a base substrate or a circuit pattern. A coating device and a coating method for forming a coating film on the surface of a substrate are disclosed, for example, in Patent Document 3.

[0004] [Prior art literature]

[0005] [Patent Document]

[0006] Patent Document 1: Japanese Patent Application Publication No. 2009-246079

[0007] Patent Document 2: Japanese Patent Application Publication No. 2013-254921

[0008] Patent Document 3: Japanese Patent No. 4857217 Summary of the invention

[0009] [Problems to be solved by the invention]

[0010] In recent years, with the development of high performance and miniaturization of electronic equipment, the heat generation of electronic parts has increased day by day, so the heat dissipation of the insulating layer has been taken seriously. In this regard, the inventors of the present application have repeatedly conducted research and found that by significantly increasing the content of fillers contained in the insulating layer forming composition compared with the past, it is possible to obtain an insulating layer with excellent heat dissipation. However, in the case of setting a coating film on the surface of the substrate by a coating liquid with such a content of fillers increased, in the existing coating method as shown in patent document 3, it is confirmed that the coating film is uneven in appearance, and the film thickness deviation of the coating film becomes larger, which is difficult in terms of mass production.

[0011] In view of such problems, the object of the present invention is to provide a coating method and a sheet obtained by the coating method, wherein the coating method can suppress unevenness of the coating film and film thickness deviation of the coating film when forming a coating film on the surface of a substrate using a coating liquid with an increased filler content.

[0012] [Technical means to solve the problem]

[0013] The present invention is a coating method, which uses a coating device to form a coating film of a coating liquid contained in a liquid storage member on the surface of a substrate, the coating device comprising: a conveying roller that delivers the wound long strip of the substrate; a scraper coater that is arranged above the conveying roller with a gap relative to the conveying roller and is cylindrical or cylindrical and has a scraper portion; and the liquid storage member, one end of which is located on the side of the conveying roller and divides a liquid storage space between the conveying roller and the conveying roller. In the coating method, the coating liquid contains a resin, a solvent and a filler, the content of the filler is 65 to 95 parts by mass relative to 100 parts by mass of a mixture of the resin and the filler, the outer diameter of the conveying roller is 50 mm to 270 mm, the outer diameter of the scraper coater is 50 mm to 170 mm, and the distance from the gap to the one end of the liquid storage member is 1 mm to 120 mm.

[0014] In the coating method, it is preferable that the content of the solvent is 10 parts by mass to 50 parts by mass based on 100 parts by mass of the mixture of the resin and the filler.

[0015] Furthermore, in the coating method, preferably, the coating liquid has a viscosity of 100 cP to 20,000 cP at a temperature of 25°C.

[0016] In the coating method, preferably, the filler is a mixture of boron nitride and aluminum oxide, and the content of the boron nitride is 60 parts by mass to 90 parts by mass based on 100 parts by mass of the mixture of the boron nitride and aluminum oxide.

[0017] Furthermore, the present invention is also a sheet including the substrate and the coating film.

[0018] [Effects of the Invention]

[0019] According to the coating method of the present invention, when a coating liquid having an increased filler content is used, unevenness of the coating film formed on the surface of the substrate can be suppressed, and variation in the film thickness of the coating film can also be suppressed. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 This is a diagram showing one embodiment of a coating device used in the coating method of the present invention.

[0021] Figure 2A This is a graph (grayscale image) related to the unevenness of the coating film.

[0022] Figure 2B This is a graph (grayscale image) related to the unevenness of the coating film.

[0023] Figure 2C is a graph related to the unevenness of the coating film ( Figure 2A Binarized image).

[0024] Figure 2D is a graph related to the unevenness of the coating film ( Figure 2B Binarized image).

[0025] Figure 3A This is a diagram (grayscale image) related to a cross section of a coating film obtained by SEM analysis.

[0026] Figure 3B This is a diagram (grayscale image) related to a cross section of a coating film obtained by SEM analysis.

[0027] Figure 3C This is a diagram related to the cross section of the coating film obtained by SEM analysis ( Figure 3A Binarized image).

[0028] Figure 3D This is a diagram related to the cross section of the coating film obtained by SEM analysis ( Figure 3B Binarized image). DETAILED DESCRIPTION

[0029] Hereinafter, one embodiment of the coating method of the present invention will be described with reference to the accompanying drawings. In addition, the figures shown in the accompanying drawings are schematic, and the thickness or width of each part, the ratio of each part to each other, etc. may be different from the actual implementation.

[0030] First, refer to Figure 1 The coating device 1 of this embodiment includes a conveying roller 2, a blade coater 3, and a liquid storage member 4, and forms a sheet including the substrate W and the coating film C by providing a coating film C on the surface of the substrate W in a long strip shape.

[0031] The conveying roller 2 is cylindrical or cylindrical, and is configured to rotate in the direction of the arrow shown in the figure by a motor (not shown) or the like. The substrate W is wound around the conveying roller 2, and the substrate W can be fed out as the conveying roller 2 rotates. The conveying roller 2 in this embodiment has a length that allows the maximum usable width of the substrate W to be about 1 m. In addition, the outer diameter D1 of the conveying roller 2 will be described later.

[0032] The blade coater 3 includes a main body 3a having a cylindrical or cylindrical shape and a blade 3b provided on the outer peripheral surface of the main body 3a. As shown in the figure, the cross-sectional shape of the blade 3b is wedge-shaped (sharp) and extends long along the axial direction of the main body 3a. The length of the blade coater 3 is set to the same degree as that of the conveying roller 2. In addition, the outer diameter D2 of the blade coater 3 will be described later.

[0033] As shown in the figure, the blade coater 3 is placed above the conveying roller 2, with the blade portion 3b being closest to the conveying roller 2, and is maintained in a state where a gap is left between the front end of the blade portion 3b and the outer peripheral surface of the conveying roller 2. In addition, the gap is set to such an extent that a coating film C of a predetermined thickness is formed on the surface of the substrate W when the substrate W is wound around the conveying roller 2 (for example, the thickness of the coating film C is about 200 μm).

[0034] As shown in the figure, the liquid storage member 4 is arranged in a state inclined with respect to the vertical direction, and one end 4a of the liquid storage member 4 is located on the side of the conveying roller 2. Figure 1 The symbol D3 shown indicates the distance from the gap to the one end 4a (the length of a chord connecting the portion closest to the scraper portion 3b to the portion closest to the one end 4a on the outer peripheral surface of the transport roller 2).

[0035] As shown in the figure, the coating device 1 includes a liquid storage space S defined by a conveying roller 2 and a liquid storage member 4. The liquid storage space S contains a coating liquid L for forming a coating film C. In addition, in a state where the coating liquid L is contained in the liquid storage space S, the lower part of the blade coater 3 is immersed in the coating liquid L.

[0036] Furthermore, the substrate W is formed of, for example, a PET film having releasability.

[0037] In addition, the coating liquid L contains resin, solvent and filler. As for the resin, if examples are given, thermosetting resins such as epoxy resin, phenol resin, melamine resin, urea resin, unsaturated polyester resin, alkyd resin, cyanate resin, etc. can be listed. In addition, the resin can also be other high thermal conductivity resins such as liquid crystal polymer, resin with mesogenic skeleton, polycarbonate, nylon, polyamide, etc. The resin can be used alone or in combination of two or more. In addition, the solvent can be, for example, a glycol ether solvent (as an example, ethyl carbitol, methyl carbitol, butyl carbitol, etc.). In addition, the filler is preferably a filler with excellent insulation and high thermal conductivity, for example, aluminum oxide, boron nitride, silicon dioxide, aluminum nitride, silicon nitride, magnesium oxide, etc. can be listed. As other substances contained in the coating liquid L, for example, additives (hardeners) that harden the resin as the main agent can be listed. The hardener can be selected according to the type of resin, and there is no particular limitation as long as it is a substance that reacts with it. For example, as a hardener when using epoxy resin, amine hardener, imidazole hardener, phenol hardener, etc. can be listed. In addition, in order to promote the hardening of the resin, a catalyst can also be added. For example, when using epoxy resin, phosphorus-based, thiol-based, tertiary amine-based, and imidazole-based catalysts can also be used. In addition, regarding the content of the resin contained in the coating liquid L, when a resin (main agent) and a hardener or catalyst (additive) are used together, the content of the resin is also calculated including the hardener or catalyst.

[0038] The content of the filler contained in the coating liquid L of the present embodiment is greatly increased compared with the content when the insulating layer is formed from the coating film C in the past. Specifically, the content of the filler is 65 to 95 parts by mass relative to 100 parts by mass of the mixture of the resin and the filler contained in the coating liquid L. By greatly increasing the content of the filler in this way, when the insulating layer of the circuit board is formed by the coating film C obtained from the coating liquid L, as an example, the thermal conductivity of the insulating layer can be set to 15 W / mk or more, and the insulating layer can have high thermal conductivity. In addition, when the quality or productivity when the coating film C is formed from the coating liquid L while ensuring the high thermal conductivity obtained as the insulating layer is considered, it is more effective to have the content of the filler be 70 to 90 parts by mass relative to 100 parts by mass of the mixture of the resin and the filler, and it is even more effective to have the content of the filler be 75 to 85 parts by mass. In addition, from the standpoint of the quality of the coating film C or the thermal conductivity of the insulating layer, it is preferable to use a mixture of boron nitride and aluminum oxide, for example. In such a case, the content of boron nitride is effectively 60 to 90 parts by mass, more effectively 65 to 85 parts by mass, and even more effectively 70 to 80 parts by mass based on 100 parts by mass of the mixture of boron nitride and aluminum oxide.

[0039] In view of the quality and productivity of the coating film C, the content of the solvent is preferably 10 to 50 parts by mass, more preferably 20 to 45 parts by mass, and even more preferably 30 to 40 parts by mass based on 100 parts by mass of the mixture of the resin and the filler.

[0040] Next, a coating method for forming a coating film C on the surface of a substrate W using the coating device 1 will be described. When the coating method is implemented, Figure 1 As shown, the substrate W is wound around the conveying roller 2, and the coating liquid L is stored in the liquid storage space S. Then, the conveying roller 2 is rotated in the direction of the arrow shown in the figure by driving a motor (not shown) or the like. As a result, the substrate W is sent out in the direction of the arrow shown in the figure, and the coating liquid L passes through the gap between the conveying roller 2 and the blade coater 3, thereby forming a coating film C on the surface of the substrate W.

[0041] In the conventional coating device 1, as in the comparative example described later, the diameter D1 of the conveying roller 2 is set to about 300 mm, the diameter D2 of the blade coater 3 is set to about 200 mm, and the distance D3 from the gap between the conveying roller 2 and the blade coater 3 to the end 4a is set to about 140 mm. When the coating film C is formed on the surface of the substrate W using the coating liquid L with an increased filler content by such a coating device 1, the coating film C is confirmed to be uneven in appearance, and the film thickness deviation of the coating film C becomes larger. If the coating film C is uneven, it is difficult to perform automatic foreign matter inspection by automatically detecting foreign matter contained in the coating film C by an appearance inspection machine or the like. In addition, if the film thickness deviation of the coating film C becomes larger, for example, when the coating film C is used for the insulating layer of the circuit substrate, it may be impossible to ensure uniform contact with the base substrate or the circuit pattern.

[0042] The unevenness or film thickness deviation of such coating C has been repeatedly studied, and it is speculated that one of the main reasons is that the coating liquid L used has a reduced resin content due to an increase in the filler content. That is, by sending out the substrate W, the coating liquid L is continuously supplied to the gap between the conveying roller 2 and the blade coater 3. Therefore, in the gap, the compressive force is strongly exerted by the coating liquid L supplied in sequence. Here, the inventor of the present application speculates that since the fluidity of the resin is higher than that of the filler, the compressive force exerts itself in a manner of squeezing the resin from the coating liquid L, which leads to the generation of unevenness and the deviation of the film thickness. In addition, it is speculated that since the filler content increases, the filler is easily settled in the liquid storage space S for accommodation, which is also one of the main reasons.

[0043] Therefore, the inventors of the present application believe that by reducing the amount of the coating liquid L supplied to the gap between the conveying roller 2 and the blade coater 3 as much as possible, the compressive force is reduced, and thus, even when the coating liquid L passes through the gap, the mixed state of the resin and the filler is not easily disturbed. In other words, it is believed that it is effective to reduce the amount of the coating liquid L supplied to the gap between the conveying roller 2 and the blade coater 3 by reducing the outer diameters of the conveying roller 2 and the blade coater 3. In addition, it is believed that in order to reduce the amount of the coating liquid L and suppress the sedimentation of the filler in the liquid storage space S, it is effective to make the liquid storage member 4 close to the conveying roller 2 to reduce the volume of the liquid storage space S.

[0044] Then, under this consideration, the study was repeated, and it was confirmed that when the outer diameter D1 of the conveying roller 2 was 50 mm to 270 mm, the outer diameter D2 of the blade coater 3 was 50 mm to 170 mm, and the distance D3 from the gap to the one end 4a was 1 mm to 120 mm, the unevenness generated in the coating C was suppressed, and the film thickness deviation of the coating C was also suppressed. In addition, the study was further repeated, and it was confirmed that in order to suppress the generation of such unevenness and suppress the film thickness deviation in the coating C, the outer diameter D1 of the conveying roller 2 is more preferably 75 mm to 250 mm, and more preferably 100 mm to 200 mm. In addition, it was confirmed that the outer diameter D2 of the blade coater 3 is more preferably 75 mm to 170 mm, and more preferably 100 mm to 150 mm. And it was confirmed that the distance D3 from the gap to the one end 4a is more preferably 1 mm to 100 mm, and more preferably 1 mm to 50 mm.

[0045] In addition, the inventors of the present application have studied the viscosity of the coating liquid L in addition to studying the diameter D1 of the conveying roller 2 in the coating device 1. The reason for this is that it is believed that by reducing the viscosity of the coating liquid L, it is possible to suppress the occurrence of uneven appearance in the coating film C. However, when the viscosity of the coating liquid L is reduced, sedimentation of the filler is confirmed in the formed coating film C. Therefore, the viscosity that can suppress the occurrence of unevenness and the sedimentation of the filler is repeatedly studied, and the following insight is obtained: if the viscosity of the coating liquid L is 100cP to 20000cP at a temperature of 25°C, the occurrence of unevenness and the sedimentation of the filler can be suppressed. In this regard, further repeated studies have been conducted, and it has been confirmed that the viscosity is more preferably 2000cP to 10000cP, and more preferably 4000cP to 6000cP. The viscosity is a value measured at a shear rate of 8 (1 / s) using a B-type viscometer (Brookfield rotational viscometer, digital viscometer DV2T (manufactured by Eikon Seiki Co., Ltd.)).

[0046] The following describes examples of the present invention, but the present invention is not limited to the examples.

[0047] <Example>

[0048] A PET film was prepared as the substrate W. In addition, a composition of a resin (main agent and additive (hardener)), a solvent, and a filler was prepared as the coating liquid L. The content of each component relative to the coating liquid L (parts by mass of each component when the coating liquid L is 100 parts by mass) is also shown.

[0049] [Main agent]

[0050] Bisphenol A epoxy resin (trade name EXA-850CRP; manufactured by DIC Corporation), 11.2 parts by mass

[0051] [Hardener]

[0052] 4,4'-Diaminodiphenyl sulfone (trade name: Seikacure S; manufactured by Wakayama Seika Kogyo Co., Ltd.), 4.2 parts by mass

[0053] [Solvent]

[0054] Ethyl carbitol (trade name: ethyl carbitol; manufactured by Sankyo Chemical Co., Ltd.), 27.6 parts by mass

[0055] [Filler (A)]

[0056] Boron nitride (BN) (trade name HP-40, agglomerated particles, average particle size (d50) 36 μm; manufactured by Mizushima Iron Alloy Co., Ltd.), 43 parts by mass

[0057] [Filler (B)]

[0058] Alumina (trade name AS20, round particle shape, average particle size (d50) 22 μm; manufactured by Showa Denko K.K.), 14 parts by mass

[0059] That is, in the prepared coating liquid L, the content of filler (A) and filler (B) is 78.7 parts by mass relative to 100 parts by mass of the mixture of resin (main component and hardener), filler (A) and filler (B), and the content of solvent is 38.1 parts by mass relative to 100 parts by mass of the mixture of resin (main component and hardener), filler (A) and filler (B). In addition, the content of filler (A) is 75.4 parts by mass relative to 100 parts by mass of the mixture of filler (A) and filler (B).

[0060] The viscosity of the coating liquid L was 4300 cP, which was measured at a shear rate of 8 (1 / s) using a B-type viscometer (Brookfield rotational viscometer, digital viscometer DV2T (manufactured by Eikon Seiki Co., Ltd.)).

[0061] In addition, the diameter D1 of the conveying roller 2 in the coating device 1, the diameter D2 of the blade coater 3, and the distance D3 from the gap between the conveying roller 2 and the blade coater 3 to the one end 4a are as shown in the comparative example and Examples 1 to 3 shown in Table 1 below. In addition, the coating device 1 of the comparative example and Examples 1 to 3 was used to form a coating film C using the substrate W and the coating liquid L, and the results are as shown in Table 1.

[0062] [Table 1]

[0063]

[0064] The evaluation in the column of "Appearance" in Table 1 is as follows.

[0065] ◎: Almost no unevenness was observed in the coating film C in terms of appearance.

[0066] ○: In terms of appearance, slight unevenness was observed in the coating film C.

[0067] ×: In terms of appearance, a lot of unevenness was observed in the coating film C.

[0068] As shown in Table 1, a large amount of unevenness was observed in the appearance of the coating film C obtained by the coating apparatus 1 of the comparative example. Figure 2A This is a photograph of the surface of the coating film C in the comparative example. Figure 2A The photo is represented by a gray image, Figure 2C will with Figure 2A The same photograph is binarized. In addition, the film thickness deviation of the coating C of the comparative example is also large. On the other hand, the coating C obtained by the coating device 1 of Example 1 and Example 2 is to the extent that a little unevenness is confirmed in appearance. In addition, the film thickness deviation of the coating C is also sufficiently small. Moreover, the coating C obtained by the coating device 1 of Example 3 is almost not confirmed in appearance (refer to Figure 2B ;also, Figure 2B A photograph showing the surface of coating film C as a gray image. Figure 2D will with Figure 2B The same photograph is binarized and shown.) In addition, the film thickness deviation of the coating film C is smaller than that of the embodiment 1 and the embodiment 2.

[0069] As described above, the sedimentation of the filler was confirmed in the formed coating film C according to the viscosity of the coating liquid L. Here, the coating device 1 of Example 3 was used, and the coating liquid L with a reduced viscosity (the amount of the solvent was increased, while the other components were kept as they were and the viscosity was 3300 cP) was used to form the coating film C, and the cross section was observed by scanning electron microscope (SEM), and the sedimentation of the filler (alumina) was confirmed (refer to Figure 3A ;also, Figure 3A The gray image shows the SEM observation photo. Figure 3C will with Figure 3A The same photograph is binarized). In contrast, SEM observation of the cross section of the coating film C obtained by using the coating liquid L (viscosity 4300 cP) and the coating device 1 of Example 3 showed no sedimentation of the filler, and the result was good (refer to Figure 3B ;also, Figure 3B The gray image shows the SEM observation photo. Figure 3D will with Figure 3B The same photo is binarized to represent it).

[0070] An embodiment of the present invention has been described above, but the present invention is not limited to the specific embodiment. Unless otherwise specified in the description, various modifications and changes can be made within the scope of the gist of the present invention as described in the claims. In addition, the effects in the embodiment are merely examples of the effects produced by the present invention, and are not intended to limit the effects brought about by the present invention to the effects described above.

[0071] For example, as the outer diameter D1 of the conveying roller 2 and the outer diameter D2 of the blade coater 3 are reduced, the rigidity of the conveying roller 2 and the blade coater 3 may be reduced, resulting in deflection. In this case, for example, a reinforcing roller for suppressing deflection may be provided on the side of the conveying roller 2 and the blade coater 3 where deflection occurs, and the coating film C may be formed using the coating device 1.

[0072] [Explanation of Symbols]

[0073] 1: Coating device

[0074] 2: Conveying roller

[0075] 3: Blade coater

[0076] 3b: Scraper

[0077] 4: Liquid storage component

[0078] 4a: One end

[0079] C: coating

[0080] L: coating liquid

[0081] S: Liquid storage space

[0082] W: Base material

Claims

1. A coating method, comprising: forming a coating film of a coating liquid contained in a liquid storage member on a surface of a substrate using a coating device, the coating device comprising: a conveying roller for delivering the wound long strip of the substrate; a scraper coater, which is arranged above the conveying roller with a gap relative to the conveying roller and is cylindrical or cylindrical and is provided with a scraper; and the liquid storage member, one end of which is located on the side of the conveying roller and divides a liquid storage space between the conveying roller and the liquid storage member, wherein the coating method comprises: The coating liquid includes a resin, a solvent, and a filler, wherein the content of the filler is 65 parts by mass to 95 parts by mass relative to 100 parts by mass of a mixture of the resin and the filler. The outer diameter of the conveying roller is 50 mm to 270 mm. The outer diameter of the blade coater is 50 mm to 170 mm. A distance from the gap to the one end portion of the liquid storage member is 1 mm to 120 mm.

2. The coating method according to claim 1, wherein: The content of the solvent is 10 parts by mass to 50 parts by mass based on 100 parts by mass of the mixture of the resin and the filler.

3. The coating method according to claim 1 or 2, wherein: The coating liquid has a viscosity of 100 cP to 20,000 cP at a temperature of 25°C.

4. The coating method according to any one of claims 1 to 3, wherein: The filler is a mixture of boron nitride and aluminum oxide, The content of the boron nitride is 60 parts by mass to 90 parts by mass based on 100 parts by mass of the mixture of the boron nitride and the aluminum oxide. 5 . A sheet comprising the substrate according to claim 1 and the coating film.