Electronic component

By coating the resin film formed by reacting amino-modified epoxy resin with an amine compound on the metal part of the electronic component, the problem of difficult maintenance of insulating properties of electronic components in the prior art under high temperature environment is solved, and high temperature durability is achieved and longevity effects.

CN118946691APending Publication Date: 2024-11-12NIHON PARKERIZING CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380030924.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-04-07
Filing Date
2023-04-03
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

It is difficult for existing electronic components to maintain insulating properties for a long time in high temperature environments, and the existing coating technology still has room for improvement in high temperature durability.

Method used

A resin film formed by reacting an amino-modified epoxy resin with an amine compound is used to coat the metal part of the electronic component to improve its high temperature durability. The resin consists of propylene oxide-added diepoxy resin, bisphenol compounds and dicarboxylic acids, and is applied through electrodeposition coating technology.

Benefits of technology

It realizes the excellent performance of high-temperature durability of electronic components in high-temperature environments, extends their service life, and improves resource utilization efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005062333050000021
    Figure BDA0005062333050000021
  • Figure BDA0005062333050000031
    Figure BDA0005062333050000031
  • Figure BDA0005062333050000081
    Figure BDA0005062333050000081
Patent Text Reader

Abstract

The present invention addresses the problem of providing an electronic component having excellent high-temperature durability. The problem is solved by an electronic component having a metal portion and a coating film on all or part of the metal portion, the coating film being obtained by reacting a specific epoxy resin (A1) with a specific amine compound (A2).
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to an electronic component. Background Art

[0002] In recent years, the use of a surface treatment agent containing a specific resin to form an excellent film on a metal material has been studied. For example, Patent Document 1 discloses that a film having excellent corrosion resistance and the like can be formed by treating a metal material surface with a cationic electrodeposition coating composition containing an amino-modified epoxy resin having a specific structure.

[0003] On the other hand, the use environment of electronic components used in various products is becoming more diverse. Under such circumstances, electronic components are required to meet high durability in the use environment. Patent document 2 discloses that in an electronic component using an insulator containing metal magnetic powder, by forming a resin coating on the insulator, an electronic component with excellent moisture resistance, chemical resistance, etc. can be obtained.

[0004] Prior art literature

[0005] Patent Literature

[0006] Patent Document 1: International Publication No. 2017 / 038631;

[0007] Patent document 2: International Publication No. 2016 / 013643. Summary of the invention

[0008] Problem that the invention aims to solve

[0009] As described above, electronic components are required to satisfy high durability in the use environment. For example, electronic components used in automobiles, etc. are required to maintain insulation and other properties for a long time even in a high temperature environment (high temperature durability). From the viewpoint of the above-mentioned high temperature durability, the electronic components formed with a coating film disclosed in Patent Document 2 still have room for improvement. The subject of the present invention is to provide an electronic component with excellent high temperature durability.

[0010] Solutions for solving problems

[0011] The present invention is as follows, etc.

[0012] [1] An electronic component comprising a metal portion, wherein the entire or a part of the metal portion has a film,

[0013] The above-mentioned film is obtained by reacting an epoxy resin (A1) with an amine compound (A2).

[0014] The epoxy resin (A1) includes an amino-modified epoxy resin or a salt thereof, wherein the amino-modified epoxy resin or a salt thereof is obtained by reacting a propylene oxide-added diepoxy resin (a1) represented by formula (1), a bisphenol compound (a2), a diepoxy resin (a3) ​​different from formula (1), and a dicarboxylic acid (a4) in which two carboxyl groups are bonded via at least one carbon atom.

[0015] [Chemical formula 1]

[0016]

[0017] [In formula (1), R 1 is an alkylene group having 3 to 10 carbon atoms which may have a substituent, a cyclohexylene group which may have a substituent, a phenylene group which may have a substituent, or -R a -R b -R c -, R a and R c is cyclohexylene or phenylene, R b is a methylene group which may have one or two substituents, and m and n are independently any integer of 1 to 20].

[0018] [2] The electronic component according to [1], wherein the electronic component is selected from electronic components constituting a motor, a bus bar, a reactor, an electric wire, and a sintered magnet.

[0019] [3] An electronic component comprising a metal portion, wherein the entire or a part of the metal portion has a film,

[0020] The film comprises a resin having a structural unit derived from an epoxy resin (A1) and a structural unit derived from an amine compound (A2),

[0021] The epoxy resin (A1) includes an amino-modified epoxy resin or a salt thereof, and the amino-modified epoxy resin or a salt thereof has:

[0022] Structural units derived from a propylene oxide-added diepoxy resin (a1) represented by formula (1);

[0023] A structural unit derived from a bisphenol compound (a2);

[0024] Structural units derived from a diepoxy resin (a3) ​​different from that of formula (1); and

[0025] a structural unit derived from a dicarboxylic acid (a4) in which two carboxyl groups are bonded via at least one carbon atom,

[0026] [Chemical formula 2]

[0027]

[0028] [In formula (1), R 1 is an alkylene group having 3 to 10 carbon atoms which may have a substituent, a cyclohexylene group which may have a substituent, a phenylene group which may have a substituent, or -R a -R b -R c -, R a and R c is cyclohexylene or phenylene, R b is a methylene group which may have one or two substituents, and m and n are independently any integer of 1 to 20].

[0029] Effects of the Invention

[0030] According to the present invention, an electronic component having a film excellent in high-temperature durability can be obtained. DETAILED DESCRIPTION

[0031] Hereinafter, an electronic component having a film on all or part of a metal portion and a method for manufacturing the electronic component according to an embodiment of the present invention will be described.

[0032] <Electronic components>

[0033] The electronic components that can be used in this embodiment are not particularly limited as long as they have metal parts and all or part of the surface is made of metal. Examples of the types of electronic components include electronic components that constitute motors (stators, rotors, leads, etc.), bus bars, reactors, wires, sintered magnets, etc.

[0034] As the metal constituting all or part of the surface of the electronic component, there is no particular restriction, and examples thereof include iron, iron alloy, aluminum, aluminum alloy, copper, copper alloy, etc. The above-mentioned metal can be constituted in the form of a film on the surface of all or part of the electronic component. As the film of the above-mentioned metal, specifically, films formed by sputtering, CVD, laser evaporation, inkjet, pattern plating transfer, Damascus method, etc. on the surface of materials such as wafers of various metal materials (including alloy materials); ceramics; glass; resin film; silicon, silicon carbide (SiC), sapphire, glass, gallium phosphide (GaP), gallium arsenide (GaAs), indium phosphide (InP), gallium nitride (GaN), etc. In addition, other films (for example, films of titanium or titanium alloys, etc.) can also be formed between the above-mentioned materials and the films of the above-mentioned metals by evaporation, sputtering, etc. As a titanium alloy, there is no particular restriction as long as it is a titanium alloy containing titanium and metal elements other than titanium but having the highest content of titanium. Specifically, titanium-palladium alloys specified in JIS H4600:2012, titanium-nickel-chromium-ruthenium-palladium alloys, titanium-tantalum alloys, titanium-palladium-cobalt alloys, titanium-nickel-ruthenium alloys, titanium-aluminum alloys, titanium-aluminum-vanadium alloys, etc. can be cited.

[0035] The size of the metal portion of the electronic component is not particularly limited and varies depending on the type of the electronic component, but typically is not a large component such as a car body.

[0036] As an example of its size, the major diameter is 1 mm or more, and may be 10 mm or more, and may be 1000 mm or less, and may be 500 mm or less, and may be 300 mm or less.

[0037] As specific examples of the electronic components, for example, the following electronic components can be cited.

[0038] International Publication No. 2019 / 077793 discloses a stator coil having an insulating coating material (6), wherein the insulating coating material (6) is composed of a mica layer (7) containing mica and a reinforcing layer (8) stacked on the mica layer (7) and containing filler particles (10) and a reinforcing material (11). The film of this embodiment can be applied to the stator coil.

[0039] Japanese Patent Application Publication No. 2019-116552 discloses an insulating sheet 1 that is filled in the gap between the stator core 12 and the stator coil 11 to insulate and fix the two. The film of this embodiment can be applied to the filling of the gap between the stator core 12 and the stator coil 11.

[0040] In Japanese Patent Gazette No. 2020-114179, regarding the retaining ring 13 and the coil end 12a of the stator 10 of the rotating electric machine, it is recorded that an elastic object (for example, insulating paper) can be sandwiched between the outer peripheral portion 13c of the retaining ring 13 and the inner peripheral portion 12b of the coil end 12a. As the above-mentioned elastic object, the membrane of this embodiment can be applied.

[0041] Japanese Patent Application Publication No. 2019-6924 describes a stator 20 including a stator core 21, a plurality of slots 15 provided on the inner periphery of the stator core 21, and a stator coil 60 wound around the slots 15, wherein the stator coil 60 is coated with a cured product of an insulating resin composition for electrical equipment. Japanese Patent Application Publication No. 2016-124878 describes coating the stator coil 60 with a resin composition 601. The film of this embodiment can be applied to the stator coil 60.

[0042] Japanese Patent Application Laid-Open No. 2015-171249 describes applying insulation coating to the stator core 11 used in the stepping motor 10. The film of the present embodiment can be applied to the stator core 11.

[0043] Japanese Patent Gazette No. 2021-60263 describes a dual-redundancy system rotary transformer using only one wheel-shaped stator (10) having a plurality of protruding magnetic poles (13). It is also described that in the dual-redundancy system rotary transformer, a pair of protruding magnetic poles (13) in each of the protruding magnetic poles (13) is insulated with a non-magnetic body (20) between the split cores (21) as one component. The non-magnetic body (20) between the split cores (21) can be applied to the membrane of the present embodiment.

[0044] Japanese Patent Application Laid-Open No. 2020-18080 discloses that a wheel-shaped insulating cap 4 is provided on the entire surface of the wheel-shaped stator 1 and each magnetic pole 2 to insulate the stator winding 10 wound around each magnetic pole 2. As the wheel-shaped insulating cap 4, the film of this embodiment can be applied.

[0045] Japanese Patent Application Publication No. 2020-145854 and Japanese Patent Application Publication No. 2020-145854 describe a stator having a motor core with a plurality of cores arranged in an annular shape and an air-core coil inserted into the core, wherein insulating paper is arranged between the core and the air-core coil. As a substitute for the insulating paper, the film of this embodiment can be applied.

[0046] International Publication No. 2021 / 153540 describes that the motor stator 30 is formed by laminating electromagnetic steel sheets, and includes a stator core 31, an insulator 34, and a field coil 35. As the insulator 34, the film of the present embodiment can be applied.

[0047] Japanese Patent Application Laid-Open No. 2021-118674 discloses an electric motor, and states that, as a preferred embodiment, the electric motor has an insulating material for insulating a stator core from a motor winding. As the insulating material, the film of the present embodiment can be applied.

[0048] Japanese Patent Application Laid-Open No. 2020-102898 states that the coil portion 20 constituting the stator 100 is formed by mutually joining a plurality of flat conductors 20a formed so that an insulating film 20c covers the periphery of a conductive member 20b. As the insulating film 20c, the film of this embodiment can be applied.

[0049] Japanese Patent Application Laid-Open No. 2021-52462 describes that a resin film 14 is formed on the outer peripheral surface of a cylindrical covering member 13 of a rotor 10. As the resin film 14, the film of the present embodiment can be applied.

[0050] Japanese Patent Application Publication No. 2019-176616 states that the stationary portion 3 of the motor MT includes a plate-shaped wiring member 36 and a conductive member (lead) 306 through which current flows, and the lead has a coating formed by an insulator. As the coating formed by the insulator, the film of this embodiment can be applied.

[0051] Japanese Patent Application Publication No. 2021-89890 discloses a terminal connection structure that connects the terminal parts of multiple devices in an electrically conductive state by means of an electrically conductive component arranged between the terminal parts. The bus bar 56 and bolts 84 used in the electrically conductive component 54 of the terminal connection structure can be applied to the film of this embodiment.

[0052] Japanese Patent Application Laid-Open No. 2021-48001 discloses a bus bar (insulating bus bar 10 ) having an insulating layer, which can be used as a wiring member for transmitting current in a power conversion device such as an inverter or a converter. The film of this embodiment can be applied as the insulating layer 2 of the insulating bus bar.

[0053] Japanese Patent Publication No. 2021-57139 discloses a busbar assembly having first and second busbars, which are arranged in the same plane with a gap between them and connected in an insulating state by an insulating resin layer, wherein the insulating resin layer includes a gap filling portion filled in the gap. In addition, an insulating resin material is described as an insulating resin layer 30 forming the busbar assembly, preferably using INSULEED (registered trademark). As the insulating resin material, the film of this embodiment can be applied.

[0054] Japanese Patent Publication No. 2019-153501 discloses an insulated flat conductor having a flat conductor and an insulating film covering the flat conductor. In addition, a coil using the insulated flat conductor is also disclosed. As the insulating coating, the film of this embodiment can be applied.

[0055] Japanese Patent Application Laid-Open No. 2019-197779 describes that the conductive wire 10 constituting the coil 1 of the reactor is covered with an insulating material. As the covering using the insulating material, the film of the present embodiment can be applied.

[0056] Japanese Patent Application Publication No. 2019-87540 discloses an insulated wire for a railway vehicle. The insulated wire has a structure in which a plurality of layers are arranged on the outer periphery of a conductor 110. Among these plurality of layers, the film of the present embodiment can be applied to the semiconductive layer 130 in contact with the conductor 110.

[0057] Japanese Patent Application Publication No. 2019-117793 discloses an insulated wire and cable for internal wiring of electronic devices. The insulated wire is formed of a conductor and an insulating layer coated on the outer periphery of the conductor and composed of a vinyl chloride resin composition, and the film of this embodiment can be applied as the insulating layer.

[0058] Japanese Patent Application Publication No. 2019-106387 discloses a multilayer insulated wire and a multilayer insulated cable suitable for railway vehicles, automobiles, equipment, etc. A double-layer insulated wire 10 as an embodiment of the multilayer insulated wire includes a conductor 11, an insulating inner layer 12 covered by the conductor 11, and an insulating outer layer 13 covered by the insulating inner layer 12. The film of this embodiment can be applied to the insulating inner layer 12.

[0059] Japanese Patent Application Laid-Open No. 2021-111448 discloses an enameled wire used in an electric motor such as an industrial electric motor. The enameled wire is composed of a conductor and an insulating film, and the film of this embodiment can be applied to the insulating film.

[0060] Japanese Patent Publication No. 2021-141011 discloses an electric coil for various electrical devices such as motors and transformers. An insulated copper wire is wound around the electric coil, and the insulated copper wire has a copper wire and an insulating film covering the surface of the copper wire. As the insulating film covering the surface of the copper wire, the film of this embodiment can be applied.

[0061] Japanese Patent Application Publication No. 2020-161410 discloses an insulated wire for a coil of a motor for a vehicle. The insulated wire has a conductive portion 1 and an insulating layer 2, wherein the conductive portion 1 has a plurality of bare wire portions, and the insulating layer 2 covers the outer periphery of the conductive portion 1. The insulating layer 2 can be applied to the film of the present embodiment.

[0062] Japanese Patent Publication No. 2021-153109 discloses a sintered magnet used for household appliances / industrial motors, electric vehicles (EVs), hybrid electric vehicles (HEVs) drive motors, electric power steering (EPS) motors and other products. It is recorded that the sintered magnet can be surface treated with a resin coating, and the film of this embodiment can be applied as the surface treatment.

[0063] <Membrane>

[0064] The electronic component of the present embodiment has a metal part, and a film is provided on the whole or part of the metal part. The film contains an amino-modified epoxy resin (hereinafter referred to as resin) or a salt thereof. The electronic component of the present embodiment can improve high temperature durability and achieve long life through the film, thereby achieving effective utilization of resources.

[0065] <Resin or its salt>

[0066] The resin of the present embodiment is described below. In addition, in the following, there are descriptions of groups containing hydrocarbon parts such as "alkyl", "alkylene", "alkenyl", "alkadienyl", "hydroxyalkyl", "alkylene glycol", and "alkanolamine". In this case, unless otherwise specified, the number of carbon atoms of the group is preferably 1 to 6 independently of each other. In addition, each raw material can be used alone or in combination of two or more.

[0067] The resin contained in the film in this embodiment includes a resin having a structural unit from an epoxy resin (A1) and a structural unit from an amine compound (A2). In addition, the epoxy resin (A1) has a structural unit from an propylene oxide-added diepoxy resin (a1) shown in formula (1), a structural unit from a bisphenol compound (a2), a structural unit from a diepoxy resin (a3) ​​different from formula (1), and a structural unit from a dicarboxylic acid (a4) in which two carboxyl groups are bonded via at least one carbon atom. Epoxy resin (A1) is also called an amino-modified epoxy resin.

[0068] [Chemical formula 3]

[0069]

[0070] [In formula (1), R 1 is an alkylene group having 3 to 10 carbon atoms which may have a substituent, a cyclohexylene group which may have a substituent, a phenylene group which may have a substituent, or -R a -R b -R c -, R a and R c is cyclohexylene or phenylene, R b is a methylene group which may have one or two substituents, and m and n are independently any integer from 1 to 20]

[0071] The resin is obtained by reacting an epoxy resin (A1) with an amine compound (A2). In addition, the epoxy resin (A1) is obtained by reacting a propylene oxide-added diepoxy resin (a1), a bisphenol compound (a2), a diepoxy resin (a3) ​​different from (a1), and a dicarboxylic acid (a4) in which two carboxyl groups are bonded via at least one carbon atom. Each raw material is described in detail below.

[0072] The propylene oxide-added diepoxy resin (a1) is a resin represented by formula (1). In formula (1), R 1 is an alkylene group having 3 to 10 carbon atoms which may have a substituent, a cyclohexylene group which may have a substituent, a phenylene group which may have a substituent, or -R a -R b -R c -. R a and R c R is cyclohexylene or phenylene. b is a methylene group which may have one or two substituents. m and n are independently any integer of 1 to 20.

[0073] Among them, as the substituents on the alkylene, cyclohexylene, phenylene and methylene groups having 3 to 10 carbon atoms, for example, alkyl, phenyl, etc. can be mentioned. Furthermore, these substituents can also be substituted by other functional groups (for example, alkyl, phenyl, etc.). In addition, the above-mentioned alkyl group can be any of linear, branched or cyclic. In addition, in this specification, unless otherwise specified, "substituent" refers to the above-mentioned alkyl, phenyl, etc.

[0074] In the above formula (1), R 1 For example, it is a dicyclohexylene group represented by the above formula (3), a diphenylene group represented by the above formula (4), or a phenylene group represented by the above formula (5). 2and Y 2 are independently a hydrogen atom, an alkyl group or a phenyl group. 3 and Y 3 are independently a hydrogen atom, an alkyl group or a phenyl group. 4 and Y 4 X is independently a hydrogen atom, an alkyl group, a phenyl group, an alkoxy group or a hydroxyl group. 2 , Y 2 , X 3 , Y 3 , X 4 and Y 4 The alkyl group of X is not particularly limited as long as it is linear or branched, and is preferably an alkyl group having 1 to 6 carbon atoms, and more preferably an alkyl group having 1 to 3 carbon atoms. 4 and Y 4 The alkoxy group is not particularly limited as long as it is linear or branched, but an alkoxy group having 1 to 6 carbon atoms is preferred, and an alkoxy group having 1 to 3 carbon atoms is more preferred.

[0075] [Chemical formula 4]

[0076]

[0077] As described above, m and n in the above formula (1) may be any integer from 1 to 20, preferably any integer from 1 to 5, more preferably both m and n are any integer from 1 to 3, and particularly preferably both m and n are 1.

[0078] The propylene oxide addition diepoxy resin (a1) of the formula (1) can be obtained by a known method. More specifically, it can be obtained by reacting propylene oxide with a 1 It can be obtained by adding or polyaddition of a polyol compound having hydroxyl groups at both ends, and reacting the obtained polyether compound (having hydroxyl groups at the ends) with epichlorohydrin to carry out diepoxidation.

[0079] More specifically, the polyol compound may be a linear or cyclic alkylene glycol having hydroxyl groups bonded to carbon atoms at both ends, such as 1,3-propylene glycol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 1,7-heptanediol, 1,8-octanediol, 1,9-nonanediol, 1,10-decanediol, and 1,4-cyclohexanediol; a polyphenol having two or more hydroxyl groups, such as catechol, resorcinol, hydroquinone, and pyrogallol; and a polyphenol compound or a hydrogenated product thereof, such as 2,2-bis(4-hydroxycyclohexyl)propane (hydrogenated bisphenol A), hydrogenated bisphenol F, hydrogenated bisphenol E, hydrogenated bisphenol B, hydrogenated bisphenol AP, hydrogenated bisphenol BP, bisphenol A, bisphenol F, bisphenol E, bisphenol B, bisphenol AP, and bisphenol BP.

[0080] The bisphenol compound (a2) is not particularly limited as long as it has two phenolic OH groups in one molecule, and examples thereof include bisphenol A, bisphenol F, bisphenol E, bisphenol B, bisphenol S, bisphenol AP, bisphenol BP, etc. Bisphenol A and bisphenol F are particularly preferred.

[0081] The diepoxy resin (a3) ​​is a compound having two epoxy groups in one molecule other than the above-mentioned propylene oxide addition diepoxy resin (a1). The epoxy equivalent of the diepoxy resin (a3) ​​is usually in the range of 170 to 500, preferably in the range of 170 to 400. The diepoxy resin (a3) ​​is preferably a compound represented by the above-mentioned formula (2). In formula (2), R 3 and R 4 X may be the same or different, and examples thereof include a single bond, an alkylene group, a phenylene group, and a cyclohexylene group. 1 and Y 1 Each independently represents a hydrogen atom or an alkyl group. 1 and Y 1 The alkyl group is not particularly limited as long as it is linear or branched, but is preferably an alkyl group having 1 to 6 carbon atoms, more preferably an alkyl group having 1 to 3 carbon atoms.

[0082] [Chemical formula 5]

[0083]

[0084] The diepoxy resin (a3) ​​can be obtained by reacting, for example, the above-mentioned polyol compound or an alkylene glycol having 2 or more carbon atoms and having the following groups bonded to the same carbon atom with an epihalohydrin (for example, epichlorohydrin), wherein the above-mentioned groups are: two hydroxyl groups; one hydroxyl group and a hydroxyalkyl group, a phenol group or a cyclohexanol group; one hydroxyalkyl group and a phenol group or a cyclohexanol group; one phenol group and a cyclohexanol group; or two hydroxyalkyl groups (which may be the same or different). Examples of the alkylene glycol include alkylene glycols having two hydroxyl groups bonded to the same carbon atom, such as 1,1-dihydroxyethane, 1,1-dihydroxypropane, and 2,2-dihydroxypropane; alkylene glycols having one hydroxyl group and one hydroxyalkyl group bonded to the same carbon atom, such as 2-hydroxypropanol and 2-hydroxybutanol; alkylene glycols having one or two hydroxyalkyl groups bonded to the same carbon atom, such as 2,2-(dihydroxymethyl)ethane, 2,2-(dihydroxyethyl)propane, 2,2-dimethyl-1,3-propanediol, 2,2-dimethyl-1,4-butanediol, and 3,3-diethyl-1,6-hexanediol; alkylene glycols having one hydroxyl group and one hydroxyalkyl group bonded to the same carbon atom, such as 4-(1-hydroxyethyl)phenol, 3-(1-hydroxyethyl)phenol, and 4-(1-hydroxypropyl)phenol; Alkylene glycols having a phenolic group; alkylene glycols having a hydroxyl group and a cyclohexanol group bonded to the same carbon atom, such as 4-(1-hydroxyethyl)cyclohexanol and 2-(1-hydroxyethyl)cyclohexanol; alkylene glycols having a hydroxyalkyl group and a phenolic group bonded to the same carbon atom, such as 4-hydroxyphenyl-2-propanol and 4-hydroxyphenyl-2-butanol; alkylene glycols having a hydroxyalkyl group and a cyclohexanol group bonded to the same carbon atom, such as 2-(4-hydroxycyclohexyl)-1-propanol and 2,2-dimethyl-2-(4-hydroxycyclohexyl)-1-ethanol; alkylene glycols having a phenolic group and a cyclohexanol group bonded to the same carbon atom, such as 2-(4-hydroxyphenyl)-2-(4-hydroxycyclohexyl)propane and 1-(4-hydroxyphenyl)-1-(4-hydroxycyclohexyl)propane; and the like.

[0085] In the production of the diepoxy resin (a3), in addition to the above-mentioned polyol compounds and the above-mentioned various alkylene glycols, for example, 4,4'-dihydroxybenzophenone, bis(4-hydroxyphenyl)-1,1-isobutane, bis(4-hydroxy-2-tert-butylphenyl)-2,2-propane, bis(4-hydroxy-3-tert-butylphenyl)-2,2-propane, bis(2-hydroxynaphthyl)methane, tetrakis(4-hydroxyphenyl)-1,1,2,2-ethane, 4,4'-dihydroxydiphenyl sulfone, 2,2-bis(4-hydroxyphenyl)hexafluoropropane, bis(4-hydroxyphenyl)-2,2-dichloroethylene, 2,2-bis(3-methyl-4-hydroxyphenyl)propane, etc. can be used.

[0086] The diepoxy resin (a3) ​​obtained from these raw materials may be used alone or in combination of two or more kinds in the production of the resin. When two or more kinds of diepoxy resins (a3) ​​are used to produce the resin, they may be added separately or simultaneously.

[0087] The dicarboxylic acid (a4) is a compound in which two carboxyl groups are bonded via at least one carbon atom. As shown in the following formula (6), a preferred dicarboxylic acid is a compound in which two carboxyl groups are bonded via a linear alkylene group (R) having 1 to 20 carbon atoms. 2 ) bonded compounds. In addition, the alkylene group (R 2 ) may have one or two or more substituents selected from alkyl, alkenyl, alkadienyl and methylene, or may have one or two or more substituents selected from alkyl, alkenyl, alkadienyl and methylene. 2 ) has 2 to 20 carbon atoms, a ring can be formed by adjacent carbon atoms of the alkylene group. The ring can have one or two or more substituents selected from alkyl and alkenyl groups, preferably alkyl and / or alkenyl groups. When the ring has two substituents, the two substituents may be the same or different. Examples of the ring include a cyclohexane ring, a cyclohexene ring, a benzene ring, and a bicyclic ring in which two carbon-carbon bonds are double bonds (for example, bicyclo[4.4.0]decane-1,7-diene, etc.). The alkylene group (R 2 ) may have an alkyl group, an alkenyl group or an alkadienyl group, or an alkyl group or an alkenyl group that a ring may have may be either linear or branched.

[0088] [Chemical formula 6]

[0089]

[0090] More preferred dicarboxylic acids (a4) are compounds having a cyclic and / or unsaturated bond. Particularly preferred dicarboxylic acids (a4) are compounds wherein, in the compound of formula (6), an alkylene group (R 2 ) has 2 to 18 carbon atoms; and the alkylene group (R 2 ) may have a methylene group, one or two alkyl groups having 5 to 9 carbon atoms, or two substituents selected from alkyl groups having 5 to 9 carbon atoms, alkenyl groups, and alkadienyl groups, or may be substituted by an alkylene group (R 2 ) constitute any of the above rings, and the ring may have two substituents which are each independently an alkyl, alkenyl or alkadienyl group having 5 to 9 carbon atoms.

[0091] Examples of the dicarboxylic acid (a4) include malonic acid, succinic acid, glutaric acid, 2,2-dimethylglutaric acid, 3,3-dimethylglutaric acid, adipic acid, 2,2-dimethyladipic acid, pimelic acid, suberic acid, azelaic acid, 2-ethylzelaic acid, sebacic acid, 1,9-nonanedicarboxylic acid, 1,10-decanedicarboxylic acid, 1,11-undecanedicarboxylic acid, 1,12-dodecanedicarboxylic acid, 1,13-tridecanedicarboxylic acid, 1,14-tetradecanedicarboxylic acid, 1,15-pentadecanedicarboxylic acid, 1,16-hexadecanedicarboxylic acid, 1,17-heptadecanedicarboxylic acid, 1,18-octadecanedicarboxylic acid, 1,19-nonadecanedicarboxylic acid, 1,20-eicosanedicarboxylic acid, itaconic acid, phthalic acid, dimer acid, 1,2-cyclohexanedicarboxylic acid, and 1,2-cyclohexenedicarboxylic acid.

[0092] In addition, examples of dimer acids that can be used as a raw material for the epoxy resin (A1) in the present embodiment include HARIDIMER 200, 250, or 270S (each commercially available from Harima Chemicals, Inc.); TSUNODYME 205, 216, 228, 395, or 346 (each commercially available from Tsukino Foods Co., Ltd.); Unydyme 14, 14R, T-17, 18, T-18, 22, T-22, 27, 35, M-9, M-15, M-35, or 40, or Century D-75, D-77, D-78, or D-1156, or Sylvatal 7001 or 7002 (each commercially available from Arizona Chemical Company); Empol 1016, 1003, 1026, 1028, 1061, 1062, 1008 or 1012 (each commercially available from BASF); hydrogenated dimer acid (average M n ~570; Sigma-Aldrich Corporation) etc.

[0093] The amine compound (A2) used in the present embodiment is a raw material for introducing amino groups into the epoxy resin (A1). Therefore, the amine compound (A2) contains at least one active hydrogen capable of reacting with an epoxy group. As the amine compound (A2), there is no particular limitation as long as it is an amine compound capable of introducing amino groups, and examples thereof include: monomethylamine, dimethylamine, monoethylamine, diethylamine, monoisopropylamine, diisopropylamine, monobutylamine, dibutylamine, monoethanolamine, diethanolamine, mono(2-hydroxypropyl)amine, di(2-hydroxypropyl)amine, monomethylaminoethanol, monoethylaminoethanol, ethylenediamine, propylenediamine, butylenediamine, hexamethylenediamine, tetraethylenepentamine, pentaethylenehexamine, diethylaminopropylamine, diethylenetriamine, etc., wherein alkanolamine is preferred. In addition, for primary amines, ketone iminated primary amines may also be used. In addition, these amine compounds may be used alone or in combination of two or more. When the resin is produced using two or more amine compounds (A2), the two or more amine compounds (A2) may be added separately or simultaneously.

[0094] <Method for producing resin or its salt>

[0095] <Method for producing epoxy resin (A1)>

[0096] Next, the method for producing the epoxy resin (A1) is described in detail. The epoxy resin (A1) can be produced by, for example, stirring a mixture of raw materials containing propylene oxide-added diepoxy resin (a1), bisphenol compound (a2), diepoxy resin (a3) ​​and dicarboxylic acid (a4) at a predetermined temperature to react. In addition, in order to promote the reaction, a reaction catalyst is preferably further added to the above mixture.

[0097] As a reaction catalyst, there is no particular limitation as long as it is a catalyst that promotes the reaction, and for example, tertiary amines such as dimethylbenzylamine, triethylamine, and tributylamine, quaternary ammonium salts such as tetraethylammonium bromide and tetrabutylammonium bromide, etc. can be used. Considering the progress of the reaction, it is desirable to control the synthesis temperature to be above 70° C. and below 200° C.

[0098] The epoxy equivalent of the epoxy resin obtained by the above-mentioned manufacturing method is, for example, preferably 1000 or more and 5000 or less, more preferably 1250 or more and 4000 or less, and particularly preferably 1500 or more and 3000 or less. The epoxy resin (A1) within this range can achieve more excellent liquid stability, and can manufacture a resin useful as a raw material for a cationic electrodeposition coating composition that can efficiently form a specified film thickness. In addition, the epoxy equivalent can be measured according to the potentiometric titration method of JIS K7236. The measurement can be carried out using a commercially available potentiometric titration device (for example, AT-610 manufactured by Kyoto Electronics Industries).

[0099] In the manufacture of epoxy resin (A1), the proportion of propylene oxide addition diepoxy resin (a1), bisphenol compound (a2), diepoxy resin (a3) ​​and dicarboxylic acid (a4) relative to the total mass of each raw material (a1) to (a4) is as follows. Propylene oxide addition diepoxy resin (a1) is preferably 1 to 50% by mass, more preferably 5 to 45% by mass, and most preferably 10 to 40% by mass. Dicarboxylic acid (a4) is preferably 1 to 20% by mass, more preferably 5 to 20% by mass, and most preferably 10 to 20% by mass. The remaining proportions depend on bisphenol compound (a2) and diepoxy resin (a3), and bisphenol compound (a2) and diepoxy resin (a3) ​​are preferably 1% by mass or more.

[0100] The above reaction can be carried out in a solvent by appropriately adding each raw material. As the solvent, there is no particular limitation as long as it is a solvent commonly used in the manufacture of resins, and examples thereof include hydrocarbon solvents such as toluene, xylene, and hexane; ester solvents such as methyl acetate and ethyl acetate; ketone solvents such as acetone, methyl ethyl ketone, and methyl isobutyl ketone; amide solvents such as dimethylformamide and dimethylacetamide; alcohol solvents such as methanol, ethanol, and isopropanol; ether alcohol solvents such as ethylene glycol monobutyl ether and ethylene glycol monohexyl ether, etc., which can be used alone or in combination of two or more.

[0101] <Resin production method>

[0102] Next, the method for manufacturing the resin is described in detail. As described above, the resin can be obtained by reacting an epoxy resin (A1) with an amine compound (A2). The reaction temperature and time are preferably carried out for 1 to 5 hours in a range of 70°C or more and 110°C or less. In the manufacture of the resin, it is preferred to adjust the amount of the amine compound (A2) so that the amine value of the resin is in the range of 5 mgKOH / g or more and 30 mgKOH / g or less. Therefore, the amine value of the obtained resin is preferably in the range of 5 mgKOH / g or more and 30 mgKOH / g or less, more preferably in the range of 5 mgKOH / g or more and 20 mgKOH / g or less, and particularly preferably in the range of 10 mgKOH / g or more and 20 mgKOH / g or less. In addition, the amine value, that is, the total amine value of the resin can be measured according to the potentiometric titration method of JIS K7237.

[0103] In addition, when unreacted epoxy groups exist even after adjusting the amine value, a compound capable of reacting with epoxy groups can be used to react with the unreacted epoxy groups. The compound that reacts with the unreacted epoxy groups is not particularly limited, and examples thereof include phenolic compounds, carboxylic acids, xylene formaldehyde resins, ε-caprolactone, and the like.

[0104] The reaction between the epoxy resin (A1) and the amine compound (A2) may use the same solvent as the solvent used in producing the epoxy resin (A1), but is not limited thereto, and other solvents may be used.

[0105] The resin can also be used in the form of a salt by neutralizing the amino groups contained in its structure with a neutralizing acid. As the neutralizing acid, there is no particular limitation as long as the amino groups in the resin can be cationized, and organic carboxylic acids such as formic acid, acetic acid, lactic acid, aminosulfonic acid, and methanesulfonic acid can be used. Among these, it is ideal to use a strong acid such as methanesulfonic acid that can make a more stable low amine value resin emulsion. These acids can be used alone or in combination. When using two or more acids, they can be added separately or simultaneously. In order to impart water dispersibility, the amino groups are cationized. Cationization can be performed on all amino groups or on a portion of the amino groups.

[0106] The resin or its salt contained in the film of the present embodiment may be in the original form or in the form of a cross-linked product, or may be in the form of a cross-linked product of the resin or its salt and a curing agent such as a polyisocyanate compound.

[0107] Examples of the polyisocyanate compound include toluene diisocyanate, xylylene diisocyanate, phenylene diisocyanate, diphenylmethane-2,4'-diisocyanate, diphenylmethane-4,4'-diisocyanate, polymeric MDI (crude MDI: polymethylene polyphenyl polyisocyanate), bis(isocyanatomethyl)cyclohexane, tetramethylene diisocyanate, hexamethylene diisocyanate, methylene diisocyanate, isophorone diisocyanate, etc. These polyisocyanate compounds may be used alone or in combination of two or more.

[0108] The thickness of the film is not particularly limited, but is generally within the range of 0.1 μm to 1000 μm. If the base metal is a magnetic metal, the thickness of the film can be measured by an electromagnetic induction film thickness gauge, and if the base metal is a non-magnetic metal, the thickness of the film can be measured by an overcurrent film thickness gauge.

[0109] <Method for manufacturing an electronic component having a film on all or part of a metal portion>

[0110] The electronic component having a film on all or part of the metal portion of the present embodiment can be obtained by forming a film on all or part of the metal portion of the target electronic component by a method such as electrodeposition coating using a surface treatment agent containing a resin or a salt thereof.

[0111] The surface treatment agent of the present embodiment contains a resin or a salt thereof in the form of an emulsion.

[0112] The emulsion can be obtained by, for example, dispersing the resin or its salt in water by a phase inversion emulsification method. The temperature during dispersion is not particularly limited, but is preferably 5° C. or higher and 50° C. or lower.

[0113] The emulsion may further include a curing agent. The curing agent is not particularly limited as long as it is a curing agent capable of crosslinking the resin, and examples thereof include blocked polyisocyanate compounds, amine compounds, melamine, etc. Blocked polyisocyanate compounds are particularly preferred. In addition, a curing catalyst may be included while including the curing agent. In the case of including both, the emulsion may be obtained by pre-mixing the resin or its salt, the curing agent and the curing catalyst, and then dispersing the mixture in water using a phase inversion emulsification method. When obtaining the emulsion, the resin, the curing agent and the curing catalyst may be mixed, and then the amino group may be neutralized to make the resin into a salt form.

[0114] The blocked polyisocyanate compound is an addition reaction product of the polyisocyanate compound and a blocking agent, and is preferably a nearly stoichiometric addition reaction product of the polyisocyanate compound and the blocking agent.

[0115] The blocking agent is a substance that blocks the isocyanate group of the polyisocyanate compound by addition, so that it can react with other compounds. The blocked polyisocyanate compound generated by blocking the isocyanate group with the blocking agent is stable at room temperature. In addition, as a blocked polyisocyanate compound, it is desirable that the blocking agent for blocking can be dissociated when the coating film formed by the cationic electrodeposition coating composition of the present invention is baked. In addition, the above-mentioned baking temperature is usually about 100 to 200°C.

[0116] As the blocking agent that meets these requirements, for example, there can be cited: lactam compounds such as ε-caprolactam and γ-butyrolactam; oxime compounds such as methyl ethyl ketone oxime and cyclohexanone oxime; phenol compounds such as phenol, p-tert-butylphenol, cresol, etc.; alcohols such as n-butanol and 2-ethylhexanol; ether alcohol compounds such as ethylene glycol monobutyl ether and ethylene glycol monohexyl ether, etc. These blocking agents can be used alone or in combination of two or more. In order to efficiently carry out the addition and dissociation reactions of the blocking agent and efficiently obtain the desired addition reaction product, the hydroxyl group in the modified epoxy resin can be reacted with the isocyanate group in the polyisocyanate compound in advance, and part or all of the other isocyanate groups in the polyisocyanate compound can be blocked with a blocking agent.

[0117] Furthermore, in order to more efficiently carry out the addition and dissociation reactions of the blocking agent, other catalysts different from the above-mentioned curing catalyst may be appropriately contained. As the catalyst, a commercially available catalyst may be appropriately used.

[0118] As the curing catalyst, known catalysts such as tin catalysts, bismuth catalysts, titanium catalysts, zirconium catalysts, amine catalysts, carboxylate catalysts, and trialkylphosphine catalysts can be used. These curing catalysts can be used alone or in combination of two or more.

[0119] The emulsion may further contain a phenolic structure-containing resin. The phenolic structure-containing resin refers to a resin containing a phenolic group that can have a substituent. As the substituent, for example, alkyl groups such as methyl and isopropyl; and phenolic groups, etc. can be cited. There is no particular restriction on the position of the substituent, but it is preferably ortho to the OH group of the phenolic group.

[0120] The resin containing a phenol structure can be produced by reacting a diepoxy compound (b1) and / or an epoxy resin (b2) having an epoxy equivalent of 170 to 500 with a bisphenol compound (b3) in the following equivalent ratio: that is, the equivalent ratio of [epoxy groups in the diepoxy compound (b1) and the epoxy resin (b2)] / [phenol groups in the bisphenol compound (b3)] = 0.5 to 0.85.

[0121] The diepoxy compound (b1) is a compound represented by the following general formula (7) and / or a compound represented by the following general formula (8).

[0122] [Chemical formula 7]

[0123]

[0124] In the above general formula (7), the two R 5 Each independently represents a hydrogen atom or an alkyl group having 1 to 6 carbon atoms, and r and s, which are the numbers of repeating units of the alkylene oxide structure portion, represent an integer of r+s=1 to 20.

[0125] In the above general formula (8), R 6 represents a hydrogen atom or an alkyl group having 1 to 6 carbon atoms, t represents an integer of 1 to 9, and u represents an integer of 1 to 50.

[0126] The epoxy resin (b2) is a compound other than the diepoxide compound (b1) having two or more epoxy groups in one molecule, a number average molecular weight in the range of 340 to 1500, preferably 340 to 1000, and an epoxy equivalent in the range of 170 to 500, preferably 170 to 400. The epoxy resin (b2) is obtained, for example, by the reaction of a polyphenol compound with an epihalohydrin.

[0127] In addition, the above-mentioned "number average molecular weight" can be calculated based on the elution time corresponding to the molecular weight of standard polystyrene by using gel permeation chromatography to analyze the epoxy resin (b2) according to the method described in JIS K 0124-83. "HLC8320GPC" (manufactured by Tosoh Corporation) was used for gel permeation chromatography. As columns, "TSKgel Super AWM-H" and "TSKgelguardcolumα" (both manufactured by Tosoh Corporation, trade names) were used. The analysis was carried out under the conditions of mobile phase: N,N-dimethylformamide, measurement temperature: 40°C, flow rate: 0.5 ml / min, using detector: RI (differential refractometer).

[0128] Examples of the polyphenol compound used in the production of the epoxy resin (b2) include bis(4-hydroxyphenyl)-2,2-propane [bisphenol A], bis(4-hydroxyphenyl)methane [bisphenol F], bis(4-hydroxycyclohexyl)methane [hydrogenated bisphenol F], 2,2-bis(4-hydroxycyclohexyl)propane [hydrogenated bisphenol A], 4,4′-dihydroxybenzophenone, bis(4-hydroxyphenyl)-1,1-ethane, bis(4-hydroxyphenyl)-1,1-isobutane, bis(4-hydroxy-2 or 3-tert-butyl-phenyl)-2,2-propane, bis(2-hydroxynaphthyl)methane, tetrakis(4-hydroxyphenyl)-1,1,2,2-ethane, 4,4′-dihydroxydiphenyl sulfone, phenol novolac, cresol novolac, and the like.

[0129] As the epoxy resin obtained by the reaction of a polyphenol compound and epichlorohydrin, an epoxy resin represented by the following general formula (9) derived from bisphenol A is particularly preferred.

[0130] [Chemical formula 8]

[0131]

[0132] [In the general formula (9), q represents an integer of 0 to 2.]

[0133] The bisphenol compound (b3) is a compound represented by the following general formula (10). In the general formula (10), R 7 , R 8 , R 9 , R 10 , R 11 , R 12 , R 13 , R 14 , R 15 and R 16 Each independently represents a hydrogen atom or an alkyl group having 1 to 6 carbon atoms. Examples of the bisphenol compound (b3) include bis(4-hydroxyphenyl)-2,2-propane [bisphenol A] and bis(4-hydroxyphenyl)methane [bisphenol F].

[0134] [Chemical formula 9]

[0135]

[0136] In addition, the manufacture of a resin containing a phenol structure can usually be obtained by the following method: a diepoxy compound (b1) and / or an epoxy resin (b2) having an epoxy equivalent of 170 to 500 is mixed with a bisphenol compound (b3), and tertiary amines such as N,N-dimethylbenzylamine and tributylamine; quaternary ammonium salts such as tetraethylammonium bromide and tetrabutylammonium bromide are appropriately used as reaction catalysts, and the mixture is reacted at a temperature range of 80 to 200°C, preferably 90 to 180°C, for 1 to 10 hours, preferably 1 to 8 hours, to obtain the resin.

[0137] The phenol structure-containing resin thus obtained has a hydroxyl value in the phenol structure of 20 to 112 mgKOH / g, preferably 25 to 110 mgKOH / g, and a number average molecular weight of 800 to 15,000, preferably 900 to 10,000.

[0138] The emulsion can be prepared, for example, by adding the neutralizing acid to a mixture of a resin and a curing agent (which may also contain a resin containing a phenolic structure), stirring and mixing, and then diluting with water. In order to impart water dispersibility, the amino group is cationized. Cationization can be performed on all or part of the amino groups.

[0139] The amount of the acid used in cationization is not particularly limited. If it is too little, the cations that impart water dispersibility may be reduced and an emulsion may not be formed. On the other hand, if it is too much, the conductivity of the emulsion may increase, and the appearance of the coating film formed by the surface treatment agent containing the emulsion may deteriorate. Therefore, it is preferred to appropriately adjust the amount of the acid so that the conductivity of the surface treatment agent is less than 1000 μS / cm.

[0140] The surface treatment agent can be prepared by stirring and mixing the liquid medium, pigment paste, organic solvent, surfactant, defoamer, etc. in the resin emulsion as needed. In addition, the surface treatment agent can be a high-concentration substance before dilution, or a low-concentration substance adjusted to a desired concentration by appropriately diluting the high-concentration substance with deionized water, etc.

[0141] The pH of the surface treatment agent is not particularly limited, but is preferably within the range of 2.0 to 8.0, and more preferably within the range of 3.0 to 6.0. There are no particular restrictions on the substances that can be used to adjust the pH, and known acids and bases can be used, such as formic acid, acetic acid, lactic acid, nitric acid, aminosulfonic acid, methanesulfonic acid, benzenesulfonic acid, etc.; and bases such as ammonia water, monoethanolamine, diethanolamine, triethanolamine, etc. can be used appropriately. In addition, the pH value in this specification represents the value measured at 25°C using a commercially available pH meter.

[0142] The surface treatment agent preferably has an electrical conductivity of less than 1000 μS / cm at 25° C. The electrical conductivity can be measured using a commercially available conductivity meter (eg, Multi-Function Water Quality Meter MM-60R manufactured by DKK East Asia).

[0143] The electronic component having a film on all or part of the metal part of the present embodiment can be obtained, for example, by immersing the coated object as a cathode in the above-mentioned surface treatment agent and then conducting an electroplating coating in which electricity is applied. As the applied voltage when the electricity is applied, it is usually in the range of 50V to 400V, preferably in the range of 100V to 300V, but it is not limited to these conditions. The surface treatment agent during the electroplating coating is usually in the range of 10 to 50°C, preferably in the range of 15 to 40°C, but it is not limited to these temperatures. In addition, after the electroplating coating, in order to solidify the formed film, a drying process is implemented. The drying of the film is preferably carried out in a temperature range of about 100°C to about 200°C, for example, at a surface temperature of the coated object, and more preferably in a temperature range of about 140°C to about 180°C. By drying and solidifying the film in this way, an electronic component having a film on all or part of the metal part of the present embodiment can be obtained. In addition, between the electroplating coating process and the drying process, a water washing process can be provided as needed. The water washing step can be performed using, for example, ultrafiltrate, reverse osmosis permeate, industrial water, pure water, or the like.

[0144] In addition, a degreasing process can also be performed before the electrodeposition coating process. The degreasing process can be performed by a known method using an appropriate degreasing agent according to the electronic component. In addition, as the degreasing agent, for example, known acidic degreasing agents, alkaline degreasing agents, solvent degreasing agents, etc. can be cited, but are not limited to these. As the degreasing method, there is no particular limitation, and for example, methods such as brush cleaning, spray cleaning (jet cleaning), and immersion (dip) cleaning can be cited. A water washing process for washing the surface of the electronic component with water can be performed after the degreasing process and before the electrodeposition coating process, and a drying process for further drying the surface of the electronic component can be performed after the water washing process and before the electrodeposition coating process. As a drying method, a known method can be applied.

[0145] Furthermore, a chemical conversion treatment process for forming a chemical conversion treatment film on the metal part of the electronic component can also be performed after the degreasing process, water washing process, drying process, etc. before the electrodeposition coating process and before the electrodeposition coating process. The chemical conversion treatment is performed by contacting the electronic component with a known chemical conversion treatment agent. In addition, the chemical conversion treatment method is not particularly limited, and a known method can be applied. In addition, a water washing process can be performed after the chemical conversion treatment process and before the electrodeposition coating process, and a drying process can also be performed after the water washing process and before the electrodeposition coating process.

[0146] Example

[0147] Hereinafter, the present invention will be described in more detail by manufacturing examples, embodiments and comparative examples, but the present invention is not limited thereto. In addition, the treated material, degreasing agent and coating used in the embodiments are arbitrarily selected from commercially available materials, and do not limit the actual use of the surface treatment composition, surface treatment treatment liquid and surface treatment method of the present invention. In addition, unless otherwise specified, % and part represent mass % and mass part, respectively. Hereinafter, a part of the raw materials used in the synthesis of epoxy resin (A1) is shown in Table 1.

[0148] [Table 1]

[0149] Table 1

[0150]

[0151] Production Example 1

[0152] In a separable flask with an internal volume of 2 liters equipped with a thermometer, a reflux cooler and a stirrer, 110.9 g of propylene oxide-added diepoxy resin (a1-1), 183.1 g of bisphenol compound (a2-1), 331.1 g of diepoxy resin (a3-1), 46.2 g of (dicarboxylic acid) a4-1 and 0.75 g of dimethylbenzylamine were added, and reacted at 130°C until the epoxy equivalent reached 2000, and 440.1 g of butyl cellosolve was added to terminate the reaction to obtain an epoxy resin (A1). In another separable flask with an internal volume of 2 liters equipped with a thermometer, a reflux cooler and a stirrer, 1000.0 g of the obtained epoxy resin (A1) was weighed, and 27.1 g of diethanolamine (A2-1) was added, and reacted at 90°C for 4 hours to obtain an amino-modified epoxy resin having a solid content of 70%. The amine value of the resin was 15.0 mgKOH / g. 650.0 g of the obtained amino-modified epoxy resin was weighed into a suitable container, mixed with 10.0 g of methanesulfonic acid, stirred evenly, and then 740.0 g of deionized water was added over about 10 minutes while stirring vigorously to obtain an emulsion with a solid content of 33%.

[0153] Production Examples 2 to 6, 8

[0154] Except having made the composition into the one shown in Table 2, it carried out similarly to Production Example 1, and produced the emulsion of Production Examples 2 to 6 and 8.

[0155] <Manufacture of blocked polyisocyanate curing agent (B)>

[0156] In a reaction container, 115.6 g of methyl isobutyl ketone was added to 678.4 g of COSMONATE M-200 (trade name, crude MDI manufactured by Mitsui Chemicals, Inc.), and after the temperature was raised to 70° C., 706.0 g of butyl cellosolve was slowly added dropwise, and after the addition was completed, the temperature was raised to 90° C. The reaction was carried out at 90° C. for 12 hours to obtain a blocked polyisocyanate type curing agent. Infrared absorption spectrum measurement was performed, and as a result, no absorption from unreacted isocyanate groups was observed, and it was confirmed that the isocyanate was completely blocked.

[0157] Production Example 7

[0158] An amino-modified epoxy resin was obtained in the same manner as in Preparation Example 1 except that the composition was as shown in Table 2. 650.0 g of the obtained amino-modified epoxy resin and 165.3 g of a blocked polyisocyanate compound were mixed, and 10.0 g of methanesulfonic acid was further added. After stirring uniformly, 1094.0 g of deionized water was added over about 10 minutes while stirring vigorously to obtain an emulsion having a solid content of 33%.

[0159] [Table 2]

[0160] Table 2

[0161]

[0162] <Production of surface treatment agent>

[0163] The emulsion of Production Example 1 was diluted with deionized water to a solid content of 16.0% to prepare a surface treatment agent.

[0164] Similarly, using the emulsions of Production Examples 2 to 8, surface treatment agents were produced.

[0165] Furthermore, an emulsion of an acrylic acid-ester copolymer (Nipol SX1706A (manufactured by Nippon Zeon Co., Ltd.)) was diluted to a solid content of 16.0% to prepare a surface treatment agent.

[0166] <Preparation of test panels>

[0167] A metal plate (any one of a cold-rolled steel plate (SPCC-SD), an aluminum alloy plate (A5052), and an oxygen-free copper plate (C1020P)) is subjected to a degreasing treatment (Fine Cleaner E2001, manufactured by Japan Parkersei Co., Ltd., trade name 43°C×2 minute spray treatment), and then washed with water to clean it. Next, the cleaned metal plate is used as a coating, and each surface treatment agent is used for 3 minutes of electroplating coating at 200V, and then washed with water. After washing with water, it is dried at 180°C (surface temperature of the coating) for 20 minutes to solidify it, and a test plate with a film thickness of 20μm is obtained. The emulsions and metal plates in the surface treatment agents used in each embodiment and comparative example are shown in Table 3.

[0168] <Evaluation test>

[0169] Various evaluation tests were performed using each of the prepared test plates. Table 3 shows the results of each evaluation test.

[0170] <Insulation test>

[0171] The dielectric breakdown voltage of the film of each test plate was measured using a withstand voltage tester (TOS9201, manufactured by Kikusui Electronics Industry Co., Ltd.). The measurement was performed under the conditions of setting the initial voltage to 50V, the voltage rise rate to 50V / second, and the cut-off current to 1.0mA. The insulation property of the film was evaluated by dividing the obtained dielectric breakdown voltage by the film thickness to obtain the dielectric breakdown voltage per unit film thickness.

[0172] <High temperature and high humidity test>

[0173] Each test plate was placed in a thermostat (ETAC HIFLEX, Kusumoto Chemical) with a set temperature of 85°C and a relative humidity of 85% for 3000 hours. The dielectric breakdown voltage per unit film thickness of the test plate before (initial) and after 3000 hours of standing in the thermostat was measured, and the ratio of the dielectric breakdown voltage of each film after 3000 hours of standing to the initial dielectric breakdown voltage was calculated (insulation retention rate after high temperature and high humidity test). Based on the obtained ratio, the high temperature and high humidity test was evaluated according to the following criteria, and those that achieved A or B were considered qualified.

[0174] A: The insulation retention rate after high temperature and high humidity test is 0.9 or more

[0175] B: The insulation retention rate after the high temperature and high humidity test is 0.6 or more and less than 0.9

[0176] C: Insulation retention after high temperature and high humidity test is less than 0.6

[0177] <Hot and cold cycle test>

[0178] Each test plate was placed in a temperature cycle tester (manufactured by ETAC Wintec Kusumoto Chemicals Co., Ltd.), and the temperature in the tester was changed in the order of 1. to 4. below (the temperature change of 1. to 4. was regarded as one cycle).

[0179] 1. Keep at -50℃ for 30 minutes

[0180] 2. Raise the temperature to 150°C

[0181] 3. Maintain at 150℃ for 30 minutes

[0182] 4. Cool to -50℃

[0183] The dielectric breakdown voltage per unit film thickness of the test plate before standing in the temperature cycle tester (initial) and at each time point after 1000 cycles of standing was measured, and the ratio of the dielectric breakdown voltage after 1000 cycles of standing to the initial dielectric breakdown voltage of each film was calculated (insulation retention rate after hot and cold cycle test). Based on the obtained ratio, the hot and cold cycle test was evaluated according to the following criteria, and those that were evaluated as A or B were considered qualified.

[0184] A: The insulation retention rate after the hot and cold cycle test is 0.9 or more

[0185] B: The insulation retention rate after the hot and cold cycle test is 0.6 or more and less than 0.9

[0186] C: Insulation retention after hot and cold cycle test is less than 0.6

[0187] <High temperature exposure test>

[0188] Each test plate was placed in an oven set at 150°C for 3000 hours. The dielectric breakdown voltage per unit film thickness of the test plate before (initial) and after 3000 hours of standing in the oven was measured, and the ratio of the dielectric breakdown voltage after 3000 hours of standing to the initial dielectric breakdown voltage of each film was calculated (insulation retention rate after high temperature exposure test). Based on the obtained ratio, the high temperature exposure test was evaluated according to the following criteria, and those with an evaluation of A or B were considered qualified.

[0189] A: The insulation retention rate after high temperature exposure test is 0.9 or above

[0190] B: The insulation retention rate after high temperature exposure test is 0.6 or more and less than 0.9

[0191] C: Insulation retention after high temperature exposure test is less than 0.6

[0192] [Table 3]

[0193]

[0194] Furthermore, although the present invention has been described in detail with reference to specific embodiments, it will be apparent to those skilled in the art that various changes and modifications can be made without departing from the spirit and scope of the present invention.

Claims

1. An electronic component comprising a metal portion, wherein a film is provided on the entire or a part of the metal portion; The film is obtained by reacting an epoxy resin (A1) with an amine compound (A2). The epoxy resin (A1) includes an amino-modified epoxy resin or a salt thereof, wherein the amino-modified epoxy resin or the salt thereof is obtained by reacting a propylene oxide-added diepoxy resin (a1) represented by formula (1), a bisphenol compound (a2), a diepoxy resin (a3) ​​different from formula (1), and a dicarboxylic acid (a4) in which two carboxyl groups are bonded via at least one carbon atom. In formula (1), R 1 It is an alkylene group having 3 to 10 carbon atoms which may have a substituent, a cyclohexylene group which may have a substituent, a phenylene group which may have a substituent, or -Ra-Rb-Rc-, wherein Ra and Rc are cyclohexylene or phenylene, Rb is a methylene group which may have one or two substituents, and m and n are independently any integer from 1 to 20.

2. The electronic component according to claim 1, in, The electronic components are selected from electronic components constituting a motor, bus bars, reactors, electric wires, and sintered magnets.

3. An electronic component comprising a metal portion, wherein a film is provided on the entire or a part of the metal portion, The film comprises a resin having a structural unit derived from an epoxy resin (A1) and a structural unit derived from an amine compound (A2), The epoxy resin (A1) includes an amino-modified epoxy resin or a salt thereof, wherein the amino-modified epoxy resin or a salt thereof has: Structural units derived from a propylene oxide-added diepoxy resin (a1) represented by formula (1); A structural unit derived from a bisphenol compound (a2); Structural units derived from a diepoxy resin (a3) ​​different from that of formula (1); and a structural unit derived from a dicarboxylic acid (a4) in which two carboxyl groups are bonded via at least one carbon atom,