Heparin anticoagulant coating based on medical catheter as well as preparation method and application of heparin anticoagulant coating

Through plasma treatment and silane coupling agent, the covalent grafting reaction of active amino groups combined with aldehyde heparin was solved, and the problem of insufficient heparin activity and applicability in the prior art was solved, and an efficient and stable heparin coating was achieved Preparation, significantly inhibits thrombosis and is suitable for a variety of medical catheters.

CN118949143APending Publication Date: 2024-11-15SHAOXING RES INST OF ZHEJIANG UNIV
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411005919.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-25
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The existing heparin coating preparation methods on medical catheters have high temperature treatment, which affects heparin activity and lacks applicability to various substrates, resulting in poor anticoagulation effect and insufficient processing mildness.

Method used

Use plasma treatment to activate medical catheters, form active amino groups through silane coupling agent and triethylamine, and then covalent grafting reaction with aldehyde heparin, and reduce them with sodium cyanoboride to form stable heparin anticoagulation coating layer to avoid high temperature treatment and ultraviolet light exposure.

Benefits of technology

It realizes the formation of a heparin coating with high graft density under mild conditions, significantly inhibits thrombosis, prolongs the use of catheter, reduces treatment costs and risks, and is suitable for a variety of matrix materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118949143A_ABST
    Figure CN118949143A_ABST
Patent Text Reader

Abstract

The invention discloses a heparin anticoagulant coating based on a medical catheter as well as a preparation method and application thereof. The preparation method comprises the following steps: soaking an activated catheter in a silane coupling agent solution for incubation, and cleaning after heat treatment to obtain a catheter containing active amino groups on the surface; and then immersing in a sodium chloride solution containing aldehyde heparin for grafting, reducing, washing, soaking in a borate buffer solution, washing, and freeze-drying to obtain the heparin anticoagulant coating. The catheter is subjected to heat treatment, active amino groups are connected to the surface of a base material through silicon-oxygen bonds, oxidized heparin with aldehyde groups is grafted to the surface of the catheter through Schiff base reaction, and therefore the stable heparin coating is obtained. A large amount of heparin can be covalently grafted on the surface of a base material, the preparation method is mild, the prepared heparin coating is good in anticoagulation effect, the coating shows lasting and stable anticoagulation performance, thrombus formation is remarkably inhibited, the experiment time of a medical catheter can be remarkably prolonged, and the treatment cost and risk of a patient are reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of medical materials, and in particular to a heparin anticoagulant coating based on a medical catheter, and a preparation method and application thereof. Background Art

[0002] Implants that are in direct contact with the blood environment must meet the requirements of blood compatibility. However, most medical catheters may cause vascular endothelial damage and blood flow changes when entering the body. During indwelling, they are recognized as foreign bodies by the body, and a series of complex reactions occur at the material-blood interface, including: non-specific adsorption of proteins to the implant surface within minutes, causing platelet adhesion, aggregation and activation, and coagulation factor activation pathways, producing insoluble fibrin networks and recruiting more platelets, red blood cells for deposition and aggregation, leading to coagulation and thrombosis; inflammatory cells infiltrate the implant surface and release cytokines to promote macrophage differentiation, etc., resulting in poor blood compatibility.

[0003] The introduction of anticoagulant coatings on the surface of materials has been proven to be an effective anticoagulant strategy, which improves the blood compatibility of materials and reduces various complications caused by thrombosis, such as catheter stenosis and local inflammatory reactions. In recent years, research work on improving the blood compatibility of material surfaces has emerged in an endless stream. Currently, commercialized anticoagulant coatings mainly include heparin coatings and phosphorylcholine coatings. Among them, heparin coatings are considered to be the most suitable coating technology for inhibiting thrombosis due to their excellent biocompatibility.

[0004] There are many ways to fix heparin in the coating, such as electrostatic self-assembly fixation, photochemical fixation, covalent bond fixation, ionic bond fixation, etc. Among them, the coating obtained by grafting heparin to the surface of the material through covalent bonds has a lasting and stable anticoagulant effect. For example, patent CN115990297A discloses a method of coating dopamine and APTMS (3-aminopropyltrimethoxysilane) on activated PTFE (polytetrafluoroethylene) to introduce active amino groups, then fix dense acrylic acid homopolymer, and then immerse it in a carboxyl-activated heparin solution for incubation to obtain a heparin coating. However, the processing time required for this technology is long, and the heat treatment temperature exceeds 95°C, which is easy to damage the substrate, and the scope of application is small.

[0005] CN117482305A discloses a heparin anticoagulant coating and its preparation method and application. The substrate is modified so that the substrate carries a thiol group; the heparin is modified with a carboxylic acid containing a double bond, an anhydride containing a double bond, an epoxy compound containing a double bond or an amide compound containing a double bond so that the heparin carries a double bond; the modified substrate is treated with a solution containing the modified heparin and an initiator so that the double bonds carried by the modified heparin and the thiol groups carried by the modified substrate undergo a thiol-ene click reaction under the action of the initiator, and a heparin anticoagulant coating is formed on the surface of the modified substrate. The preparation method of the above-mentioned heparin anticoagulant coating enables the heparin anticoagulant coating to be stably bound to the surface of the substrate while maintaining biological activity. However, this method first prepares a coating solution, then covers it on the substrate by coating, and solidifies it by long-term ultraviolet light irradiation.

[0006] Since most medical materials lack active groups on their surfaces that can be grafted with heparin and are limited by low tolerable processing temperatures, existing heparin grafting technology lacks universal applicability to medical catheters. Summary of the invention

[0007] The present invention aims to solve the problem that the preparation temperature of heparin-coated catheter is high and affects the activity of heparin, and provides a method for preparing a heparin anticoagulant coating with a high grafting density on the surface of a substrate. The method has a wide range of applicability to substrates, mild conditions, and broad market application prospects.

[0008] To achieve the above object, the technical solution adopted by the present invention is:

[0009] A method for preparing a heparin anticoagulant coating based on a medical catheter comprises the following steps:

[0010] Step 1, plasma treatment and activation of the medical catheter;

[0011] Step 2, immersing the activated catheter in a silane coupling agent solution for incubation, and washing after heat treatment to obtain a catheter with active amino groups on the surface;

[0012] Step 3, adding sodium nitrite and glacial acetic acid to the heparin sodium solution for reaction, adjusting the pH of the solution to alkaline after the reaction, and lyophilizing after dialysis to obtain aldehyde heparin;

[0013] Step 4, immersing the catheter obtained in step 2 in a sodium chloride solution containing aldehyde heparin, adding sodium cyanoborocyanide (NaCNBH) aqueous solution to the solution for reduction reaction after the grafting reaction, and the product is rinsed, soaked in borate buffer, rinsed, and freeze-dried to obtain the heparin anticoagulant coating.

[0014] In the present invention, plasma treatment is performed on the surface of an inert substrate to obtain hydroxyl groups, and active amino groups are connected to the substrate surface through silicon-oxygen bonds through heat treatment. Finally, oxidized heparin with aldehyde groups is grafted on the catheter surface through Schiff base reaction, thereby obtaining a stable heparin coating. This method first obtains a primer containing a large number of active amino groups on the surface of the substrate, providing sufficient sites for the covalent grafting of heparin, and then firmly fixes a large amount of heparin on the surface of the medical catheter. The preparation method is mild, does not require high temperature, and does not require ultraviolet light. The heparin coating prepared by this method has a good anticoagulant effect, and the coating exhibits a long-lasting and stable anticoagulant performance, significantly inhibits thrombosis, can significantly prolong the experimental time of the medical catheter, and reduce the treatment cost and risk of patients.

[0015] The gas used for the plasma treatment is one or more of hydrogen, oxygen and nitrogen, with a gas flow rate of 100-300 mL / min, a power of 150-300 W and a treatment time of 2-30 min.

[0016] The silane coupling agent solution is an ethanol solution of a silane coupling agent and triethylamine; wherein the volume concentration of the silane coupling agent is 0.4-1.0%, the volume ratio of the silane coupling agent to the triethylamine is 1:0.8-1.2, and the function of the triethylamine is to provide a weak alkaline environment and catalyze the silicon-oxygen reaction.

[0017] The silane coupling agent is γ-aminopropyltriethoxysilane (KH550) and / or Y-aminopropyltrimethoxysilane (KH540), which provides active amino groups on the surface of the substrate.

[0018] In step 2, the incubation is immersion at 30-60°C for 0.5-4h; the heat treatment is treatment at 50-60°C for 10min-2h. By incubating the substrate in the solution, the silane coupling agent is covalently bonded to its surface through the silicon-oxygen bond; after being taken out of the liquid surface, it is heated and cured at 50-60°C, so that the silane in the coating solution on the surface of the substrate is further hydrolyzed and polymerized, thereby anchoring the amino-containing silane on the surface of the substrate, so as to obtain uniform and large amounts of active amino groups.

[0019] The cleaning in step 2 is performed by ultrasonication in ethanol for 5-20 minutes.

[0020] In step 3, the mass volume concentration of heparin sodium in the heparin sodium solution is 2-5 mg / mL, the mass ratio of heparin sodium to sodium nitrite is 50-200:1, and the volume ratio of heparin sodium to glacial acetic acid is 50-150:1 (w / v).

[0021] The reaction in step 3 is carried out at room temperature for 1-6 hours, and the pH is adjusted to 6-9.

[0022] Step 4: The concentration of aldehyde heparin in the sodium chloride solution containing aldehyde heparin is 3-5% (w / v), and the concentration of sodium chloride is 0.9%-4% (w / v). At this concentration, the aldehyde heparin molecular chain can be stretched to expose its reaction sites, which is conducive to its covalent grafting to the substrate surface.

[0023] The mass ratio of the added sodium cyanoborocyanide to the aldehyde heparin is 1:40-80.

[0024] In step 4, the grafting reaction is carried out at 40-70°C for 1-60 minutes, and the reduction reaction is carried out at 40-70°C for 1-3 hours. The active amino groups on the substrate react covalently with the aldehyde groups on the aldehyde heparin to generate unstable imines, which are further reduced to stable amino groups by sodium cyanoborocyanide, thereby achieving covalent grafting of heparin on the surface of the substrate. The reaction conditions are mild and high temperature heating is not required.

[0025] The method of the present invention can be applied to a variety of base materials, and the medical catheter includes one or more of a polytetrafluoroethylene (PTFE) guide tube, a thermoplastic polyurethane (TPU) nasogastric feeding tube, a TPU balloon catheter, a medical polyetheramide (PEBAX) catheter, a polyvinyl chloride (PVC) nasogastric feeding tube, and the like.

[0026] The invention also provides a heparin anticoagulant coating prepared by the preparation method.

[0027] The present invention also provides application of the heparin anticoagulant coating in the preparation of implantable medical devices.

[0028] Compared with the prior art, the present invention has the following beneficial effects:

[0029] (1) The preparation method of the heparin anticoagulant coating of the present invention has mild conditions (not exceeding 70° C.), a simple preparation process, and can obtain a medical catheter surface with a large amount of heparin grafted thereon. The coating grafting is firm, durable, and stable, and can significantly inhibit thrombosis. It can significantly prolong the experimental time of the medical catheter, and reduce the treatment cost and risk of patients.

[0030] (2) The heparin anticoagulant coating of the present invention is suitable for medical catheters made of various base materials, has a wide range of applications, is easy to operate in the preparation method, has low production cost, and has broad market application prospects. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Figure 1 This is a schematic diagram of the assembly of the heparin anticoagulant coating of a medical catheter in Example 1.

[0032] Figure 2 The optical images are of Congo red staining of the medical catheters of Examples 1-3 and Comparative Examples 1-2 after amination treatment.

[0033] Figure 3The optical images are of the heparin anticoagulant coatings of the medical catheters of Examples 1-3 and Comparative Examples 1-2 after being stained with toluidine blue.

[0034] Figure 4 The SEM images of the heparin anticoagulant coatings of the medical catheters of Example 1 and Comparative Example 2 are shown.

[0035] Figure 5 Optical images of the anticoagulant performance test of the heparin anticoagulant coating of the medical catheter of Examples 1-2 and Comparative Example 1.

[0036] Figure 6 This is an optical image of the stability test of the heparin anticoagulant coating of the medical catheter of Example 1-2. DETAILED DESCRIPTION

[0037] In order to make the purpose, technical scheme and advantages of the present invention clearer, the present invention is further described in detail below in conjunction with embodiment. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention. Those skilled in the art can make modifications or equivalent substitutions based on the understanding of the technical scheme of the present invention without departing from the spirit and scope of the technical scheme of the present invention, and all should be included in the protection scope of the present invention.

[0038] The raw materials used in the following specific embodiments were purchased from the market. Heparin sodium was purchased from Beijing Bailingwei Technology Co., Ltd., and silane coupling agents KH550 and KH560 were purchased from Shanghai Yuanye Biotechnology Co., Ltd.

[0039] Example 1

[0040] (1) Substrate cleaning: The medical PTFE catheter was placed in a plasma cleaning machine for O2 plasma treatment. The treatment conditions were: O2 flow rate 100 mL / min, bombardment power 200 W, and bombardment time 600 s;

[0041] (2) Amination of substrate: The catheter was immersed in KH550 solution (95% ethanol as solvent, containing 7.5% KH550 and 5.0% triethylamine), incubated at 60°C for 1 h, taken out and placed in an oven for heating at 60°C for 1 h, and then placed in anhydrous ethanol for ultrasonic cleaning for 10 min.

[0042] (3) Heparin oxidation: 1 g of heparin sodium was dissolved in 250 mL of water, and 10 mL of sodium nitrite aqueous solution (1 mg / mL) and 8 mL of glacial acetic acid aqueous solution (500 μL of glacial acetic acid dissolved in 2 mL of water) were added dropwise, and the mixture was reacted at room temperature for 5 h under continuous stirring. The solution was adjusted to pH 9 with a NaOH aqueous solution. The solution after the reaction was collected in a dialysis bag and dialyzed at room temperature for 2 days. The dialyzed solution was collected, freeze-dried, and stored at 4°C to obtain aldehyde heparin.

[0043] (4) Heparin grafting: The aminated medical catheter is then placed in a sodium chloride solution containing aldehyde heparin (where the aldehyde heparin concentration is 4 mg / ml and the sodium chloride is 0.9% (g / ml)), and reacted at 60°C for 20 minutes. 16 μL of NaCNBH aqueous solution (2.5%, w / v) is added to the above solution with a pipette, and reacted at 60°C for 3 hours. The sample is rinsed with DI water and then immersed in a borate buffer solution. The sample is rinsed with DI water and freeze-dried. The schematic diagram of the assembly of the various layers of the heparin anticoagulant coating of the medical catheter is shown in the figure. Figure 1 shown.

[0044] Example 2

[0045] The difference between this embodiment and embodiment 1 is that a TPU catheter is selected as the medical catheter, and the O2 plasma treatment conditions are: O2 flow rate 100 mL / min, bombardment power 300 W, and bombardment time 480 s.

[0046] Example 3

[0047] The difference between this embodiment and embodiment 1 is that the medical catheter uses a PEBAX catheter; in addition, the amination treatment conditions are: immerse the catheter in a KH550 solution (95% ethanol as a solvent, containing 5.0% KH550, 5.0% triethylamine), soak at 37°C for 2 hours, and then soak at 60°C for 1 hour, take it out and place it in an oven to heat at 60°C for 1 hour, and then put it in anhydrous ethanol for ultrasonic cleaning for 10 minutes; when heparin is grafted, the amination medical TPU catheter is placed in a sodium chloride solution containing aldehyde heparin (wherein the concentration of aldehyde heparin is 2.5 mg / ml and the sodium chloride is 2% (g / ml), react at 60°C for 10 minutes, and then add 20 μL of NaCNBH aqueous solution (2%, w / v) to the above solution, react at 60°C for 2 hours, rinse the sample with DI water, and then soak it in a borate buffer solution, rinse the sample with DI water, and freeze-dry.

[0048] Comparative Example 1

[0049] The difference between this embodiment and embodiment 1 is that, only in step (2) of substrate amination, the catheter is immersed in a KH550 solution (95% ethanol as solvent, containing 5.0% KH550, 5.0% triethylamine), incubated at 30° C. for 1 hour, taken out and ultrasonically cleaned in anhydrous ethanol for 10 minutes, without heat treatment, and the other steps are the same to obtain an anticoagulant coating.

[0050] Comparative Example 2

[0051] The difference between this embodiment and embodiment 1 is that, only in step (2) of substrate amination, the catheter is immersed in a KH550 solution (95% ethanol as solvent, containing 5.0% KH550 and 5.0% triethylamine), incubated at 60° C. for 12 h, taken out and heated in an oven at 60° C. for 1 h, and then ultrasonically cleaned in anhydrous ethanol for 10 min.

[0052] Comparative Example 3

[0053] The difference between this embodiment and embodiment 1 is that only in step (2) of substrate amination, the catheter is immersed in a KH550 solution (95% ethanol as solvent, containing 5.0% KH550), which does not contain triethylamine, and the other steps are the same.

[0054] Sample testing

[0055] (1) Amination of medical catheter surfaces

[0056] The aminated medical catheters of Examples 1, 2, 3 and Comparative Examples 1, 2, 3 were incubated in a 1% (w / v) Congo red aqueous solution for 10 min, and the excess dye on the surface was washed off under running water, and the catheters were naturally dried. The appearance of the dyed medical catheters was photographed. The results are as follows: Figure 2 shown.

[0057] It can be seen that the aminated catheters prepared in Example 1 and Comparative Example 2 have good coating integrity and are obviously positive after Congo red staining, which indicates that these treatments can all aminate the substrate surface. However, the coatings prepared in Comparative Examples 1 and 3 are stained with Congo red, and the catheters are lighter in color and have uncolored parts, indicating that the treatments cannot stably and uniformly aminate the substrate surface, indicating that heat treatment and the alkaline environment created by triethylamine are both conducive to the grafting of silane.

[0058] (2) Integrity of heparin coating on medical catheter surface

[0059] The heparinized medical catheters of Examples 1, 2, 3 and Comparative Examples 1 and 2 were incubated in a 0.005% toluidine blue solution for 10 minutes, the excess dye was rinsed off, and the catheters were naturally dried. The appearance of the dyed medical catheters was photographed. The results are as follows: Figure 3 shown.

[0060] As can be seen from the figure, the heparin coatings of Examples 1, 2, 3 and Comparative Example 2 show obvious purple heterochromatic reaction, which is a unique color development reaction of heparin, and the color development of the coating is uniform and complete; while the heparin coating of Comparative Example 1 is almost not stained with purple after toluidine blue staining, which indicates that the amount of grafted heparin in the coating is small. This is because there are few active amino groups on the surface when the substrate is aminated, so the amount of heparin grafted by the Schiff base reaction is also less.

[0061] (3) Characterization of the thickness of heparin coating on the surface of medical catheters

[0062] The heparinized medical catheters of Example 1 and Comparative Example 2 were frozen and fractured by liquid nitrogen to obtain cross sections, and then gold was sprayed for 30 seconds. The cross sections were photographed by SEM to characterize the thickness of the coating. The results are shown in Figure 4 The thickness of the heparin coating of Example 1 is about 300 nm; the thickness of the heparin coating of Comparative Example 2 is greater than 1500 nm. Long-term heating may cause a large amount of polymerization of KH550 on the surface of the substrate, thereby increasing the thickness of the coating. If the coating is too thick, it may affect the performance of the original medical catheter, such as affecting the inner diameter of the catheter.

[0063] (4) Anticoagulant properties of heparin coating on medical catheter surface

[0064] The Chandler ring model was used to simulate physiological blood flow. The heparin-coated medical catheters in Examples 1, 2 and Comparative Example 1 were fixed at the same position of a medical silicone tube. Fresh rabbit blood was recalcified into the silicone tube. Subsequently, multiple test rings containing different samples were rotated in a 37°C water bath. After the experiment, each sample was gently washed in PBS, and the surface thrombus formation and adhesion were photographed with a camera.

[0065] Depend on Figure 5 It can be seen that there is almost no thrombus on the surface of the heparinized medical catheters in Examples 1 and 2, while there is thrombus on the surface of the catheter in Comparative Example 1. Combined with the research results of Congo red staining and toluidine blue staining, it can be seen that grafting a sufficient amount of heparin on the surface of the medical catheter can significantly inhibit the formation of thrombus and give the medical catheter a better anticoagulant effect.

[0066] (5) Stability of heparin coating on medical catheter surface

[0067] The heparin-coated medical catheter was placed in a medical extracorporeal circulation tube (mainly composed of polyvinyl chloride) and flowed at 4 L / min at 37°C. The anticoagulant performance of the heparin-coated medical catheter after 60 days of extracorporeal circulation was tested by the Chandler ring test. The results are shown in Figure 6 As can be seen from the figure, the heparin-coated medical catheters prepared in Examples 1 and 2 still have excellent anticoagulant properties after 60 days of extracorporeal circulation, which indicates that the heparin coating prepared by this method has good stability and can meet the clinical needs of long-term implantation or multiple uses of medical catheters.

[0068] In addition, similar experimental results have proved that the coatings obtained by the method of the present invention on a variety of medical catheters have excellent anticoagulant effect and stability, and the coating is only nanometer-level thick, indicating that the super heparin anticoagulant coating is universal for different medical catheters and has a broad market.

[0069] The embodiments described above provide a detailed description of the technical solutions of the present invention. It should be understood that the above are only specific embodiments of the present invention and are not intended to limit the present invention. Any modifications, supplements or similar substitutions made within the scope of the principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing a heparin anticoagulant coating based on a medical catheter, characterized in that: Includes steps: Step 1, plasma treatment and activation of the medical catheter; Step 2, immersing the activated catheter in a silane coupling agent solution for incubation, and washing after heat treatment to obtain a catheter with active amino groups on the surface; Step 3, adding sodium nitrite and glacial acetic acid to the heparin sodium solution for reaction, adjusting the pH of the solution to alkaline after the reaction, and lyophilizing after dialysis to obtain aldehyde heparin; Step 4, immersing the catheter obtained in step 2 in a sodium chloride solution containing aldehyde heparin, adding sodium cyanoborocyanide aqueous solution to the solution for reduction reaction after the grafting reaction, and the product is rinsed, soaked in borate buffer, rinsed, and freeze-dried to obtain the heparin anticoagulant coating.

2. The method for preparing a heparin anticoagulant coating based on a medical catheter according to claim 1, characterized in that: The gas used for the plasma treatment is one or more of hydrogen, oxygen and nitrogen, with a gas flow rate of 100-300 mL / min, a power of 150-300 W and a treatment time of 2-30 min.

3. The method for preparing a heparin anticoagulant coating based on a medical catheter according to claim 1, characterized in that: The silane coupling agent solution is an ethanol solution of a silane coupling agent and triethylamine; wherein the volume concentration of the silane coupling agent is 0.4-1.0%, and the volume ratio of the silane coupling agent to the triethylamine is 1:0.8-1.2; The silane coupling agent is γ-aminopropyltriethoxysilane and / or γ-aminopropyltrimethoxysilane.

4. The method for preparing a heparin anticoagulant coating based on a medical catheter according to claim 1, characterized in that: In step 2, the incubation is performed by soaking at 30-60° C. for 0.5-4 h; the heat treatment is performed at 50-60° C. for 10 min-2 h; and the cleaning in step 2 is performed by ultrasonication in ethanol for 5-20 min.

5. The method for preparing a heparin anticoagulant coating based on a medical catheter according to claim 1, characterized in that: In step 3, the mass volume concentration of heparin sodium in the heparin sodium solution is 2-5 mg / mL, the mass ratio of heparin sodium to sodium nitrite is 50-200:1, and the mass ratio of heparin sodium to glacial acetic acid is 50-150:1 (w / v); The reaction in step 3 is carried out at room temperature for 1-6 hours, and the pH is adjusted to 6-9.

6. The method for preparing a heparin anticoagulant coating based on a medical catheter according to claim 1, characterized in that: In step 4, the concentration of aldehyde heparin in the sodium chloride solution containing aldehyde heparin is 3-5% (w / v), and the concentration of sodium chloride is 0.9%-4% (w / v).

7. The method for preparing a heparin anticoagulant coating based on a medical catheter according to claim 1, characterized in that: In step 4, the grafting reaction is carried out at 40-70° C. for 1-60 min; and the reduction reaction is carried out at 40-70° C. for 1-3 h.

8. The method for preparing a heparin anticoagulant coating based on a medical catheter according to claim 1, characterized in that: The medical catheter includes one or more of a PTFE guide catheter, a TPU nasogastric feeding tube, a TPU balloon catheter, a medical PEBAX catheter, and a PVC nasogastric feeding tube.

9. The heparin anticoagulant coating prepared according to the preparation method according to any one of claims 1 to 8.

10. Use of the heparin anticoagulant coating according to claim 9 in the preparation of implantable medical devices.

Citation Information

Patent Citations

  • Dopamine-heparin composite anticoagulant coating and preparation method thereof

    CN114984332A

  • Heparin anticoagulation coating based on PTFE material and preparation method thereof

    CN115990297A

  • Hydrophilic anticoagulant coating as well as preparation method and application thereof

    CN117323473A

  • Polymeric based and surface treated metallic hybrid materials and fabrication methods thereof

    US20110166251A1

  • Method for making improved heparinized biomaterials

    US5767108A