Oil-resistant irradiation crosslinking low-smoke halogen-free cable material with low irradiation dose and high crosslinking degree for locomotives and preparation method of oil-resistant irradiation crosslinking low-smoke halogen-free cable material

By adopting specific group distribution ratio and process flow in oil-resistant irradiated crosslinking low-smoke halogen-free cable materials for locomotives, high crosslinking degree at low irradiation doses are achieved, and the large irradiation dose in the prior art is solved The resulting problems of insufficient antioxidant consumption and crosslinking meet the thermal extension standards and reduce costs.

CN118978757APending Publication Date: 2024-11-19YANGZHOU HAONIANHUA POLYMER MATERIALS CO LTD

Patent Information

Application Number
CN202411211276.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-30
Publication Date
2024-11-19

Smart Images

  • Figure BDA0005020371180000081
    Figure BDA0005020371180000081
Patent Text Reader

Abstract

The invention discloses an oil-resistant irradiation crosslinking low-smoke halogen-free cable material with low irradiation dose and high crosslinking degree for locomotives and a preparation method of the cable material, and belongs to the technical field of cable materials. The cable material disclosed by the invention is prepared from the following components in parts by weight: 10 to 15 parts of base resin A, 5 to 15 parts of base resin B, 10 to 15 parts of compatilizer, 45 to 55 parts of flame retardant, 1.2 to 1.5 parts of antioxidant, 1.5 to 3.5 parts of assistant crosslinking agent and 0.03 to 0.08 part of initiator. The preparation method comprises the following steps: firstly, melting the initiator, adding into the base resin B, and stirring and mixing to obtain a premix of the base resin B; uniformly mixing the premix of the base resin B with the other components according to the proportion, and mixing and granulating through an extruder to obtain the cable material with low irradiation dose and high crosslinking degree. After the cable material prepared by the invention is extruded into a wire, the thermal extension standard requirement can be met only by performing low-dose irradiation treatment.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of cable materials, and in particular relates to an oil-resistant radiation-crosslinked low-smoke halogen-free cable material for locomotives with low radiation dose and high crosslinking degree and a preparation method thereof. Background Art

[0002] In order to meet the requirements of heat resistance, oil resistance, chemical solvent resistance, etc., wire and cable materials usually use silane cross-linking, chemical cross-linking, radiation cross-linking and other methods to form a network cross-linked structure of the material, so that the material has the characteristics of "infusibility and insolubility" to improve the stability of the material.

[0003] Compared with chemical crosslinking, silane crosslinking and other methods, radiation crosslinking has the advantages of high operability, stable crosslinking effect and fast crosslinking speed. However, there are still some problems to be solved in radiation crosslinking. For example, when irradiating some cable materials or cables with large wall thickness that require high crosslinking degree, a large dose is often required. Even at high radiation doses, it is impossible to achieve high crosslinking degree products because radiation crosslinking and radiation degradation reach a certain balance. For example, oil-resistant radiation crosslinked low-smoke halogen-free flame-retardant wires and cables for locomotives have poor oil resistance at low crosslinking degrees. Therefore, such cables require improved radiation crosslinking effects and thermal elongation controlled between 10 and 20%. With such high crosslinking degree requirements, if a large radiation dose is simply used for radiation processing, on the one hand, a large amount of antioxidants will be consumed, resulting in unqualified anti-aging performance of the product; on the other hand, even if the radiation dosage is enlarged to more than 30 Mrad, the radiation crosslinking and radiation degradation will reach a certain balance and the crosslinking degree cannot meet the requirements.

[0004] Therefore, in order to achieve a higher degree of cross-linking of cable materials under normal or low irradiation conditions, it is urgent to develop a cable material with a low irradiation dose and a high degree of cross-linking. Summary of the invention

[0005] The first purpose of the present invention is to propose an oil-resistant radiation-cross-linked low-smoke halogen-free flame-retardant cable material for locomotives that can have a higher degree of cross-linking at a lower radiation dose. After being extruded into a wire, only a lower dose of radiation treatment is required to meet the thermal extension standard requirements.

[0006] The second purpose of the present invention is to propose a method for preparing an oil-resistant radiation-crosslinked low-smoke halogen-free cable material for locomotives with low radiation dose and high crosslinking degree. The preparation process is simple and can be mass-produced.

[0007] In order to solve the above problems, the technical solution adopted by the present invention is as follows:

[0008] The invention discloses an oil-resistant radiation cross-linked low-smoke halogen-free cable material for locomotives with low radiation dose and high cross-linking degree. The proportions of the components are as follows by weight: 10 to 15 parts of base resin A, 5 to 15 parts of base resin B, 10 to 15 parts of compatibilizer, 45 to 55 parts of flame retardant, 1.2 to 1.5 parts of antioxidant, 1.5 to 3.5 parts of auxiliary cross-linking agent and 0.03 to 0.08 parts of initiator.

[0009] Furthermore, in terms of weight, the proportions of each component are as follows: 15 parts of base resin A, 10 parts of base resin B, 15 parts of compatibilizer, 45 parts of flame retardant, 1.2 parts of antioxidant, 1.5 parts of co-crosslinking agent, and 0.05 parts of initiator.

[0010] Furthermore, the base resin A is ethylene-vinyl acetate copolymer, the VA content of the ethylene-vinyl acetate copolymer is 28% to 33%, and the melt flow rate at 190°C@2.16kg is 0.02g / 10min to 4g / 10min.

[0011] Furthermore, the resin B is a highly branched polyethylene resin, and the density of the highly branched polyethylene resin is 0.916 g / cm 3 ~0.918g / cm 3 , the melt flow rate at 190℃@2.16kg is 5g / 10min~10g / 10min.

[0012] Furthermore, the compatibilizer is selected from one or more of PE-MAH grafted material, EVA-MAH grafted material and POE-MAH grafted material; the flame retardant is one or more of aluminum hydroxide, magnesium hydroxide, MCA and nano-montmorillonite.

[0013] Furthermore, the antioxidant is selected from one or more of pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], dilauryl 3,3'-thiodipropionate, diethylenethiobis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate] and 1,2-bis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionyl]hydrazine.

[0014] Furthermore, the auxiliary cross-linking agent is selected from one or more of trimethylolpropane triacrylate, trimethylolpropane trimethacrylate and triallyl isocyanurate.

[0015] Furthermore, the initiator is dicumyl peroxide.

[0016] Furthermore, when the oil-resistant radiation-crosslinked low-smoke halogen-free cable material for locomotives with low radiation dose and high crosslinking degree is extruded into wire and then radiation-crosslinked, the radiation dose is 6 Mrad.

[0017] Furthermore, the preparation method of any of the above-mentioned oil-resistant radiation-crosslinked low-smoke halogen-free cable materials for locomotives with low radiation dose and high crosslinking degree comprises the following steps:

[0018] (1) First, the initiator is pre-melted and evenly sprayed into the base resin B, and then stirred to fully mix the materials to obtain a premix of the base resin B;

[0019] (2) The premix of the base resin B prepared in step (1) is uniformly mixed with the base resin A, a compatibilizer, a flame retardant, an antioxidant, and a cross-linking agent according to a formula ratio, and the mixture is mixed and granulated through a two-stage extruder by forced feeding to obtain an oil-resistant radiation-crosslinked low-smoke halogen-free cable material for locomotives with a low radiation dose and a high cross-linking degree.

[0020] Compared with the prior art, the advantages of the present invention are as follows:

[0021] 1) The low-irradiation-dose and high-crosslinking-degree cable material prepared by the present invention, after being extruded into a wire, is irradiated using an electron accelerator and only requires a relatively low-dose (6 Mrad) irradiation treatment to meet the standard requirement of thermal elongation reaching 10-20%.

[0022] 2) The cable material prepared by the present invention has a higher gel content and a lower elongation at break attenuation compared with the prior art, and the reduced irradiation dose further reduces the subsequent processing costs of cable companies. DETAILED DESCRIPTION

[0023] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the specific implementation methods of the present invention are described in detail below in conjunction with specific embodiments.

[0024] The raw materials used in the following examples are:

[0025] Base resin A (UL00628 Lianhong Chemical) is ethylene-vinyl acetate copolymer (VA content is 28% to 33%, melt flow rate (190°C@2.16kg) is 0.02g / 10min to 4g / 10min);

[0026] Base resin B (SP1071C Japan Primen) is a highly branched polyethylene resin (density of 0.916 g / cm3 to 0.918 g / cm3, melt flow rate (190°C @ 2.16 kg) of 5 g / 10 min to 10 g / 10 min);

[0027] The compatibilizer is a mixture of one or more of PE-MAH grafted material, EVA-MAH grafted material, and POE-MAH grafted material;

[0028] The flame retardant is a mixture of one or more of aluminum hydroxide, magnesium hydroxide, MCA, and nano-montmorillonite.

[0029] The antioxidant is one or a mixture of tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate] pentaerythritol ester, 3,3'-dilauryl thiodipropionate, diethylenethiobis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], 1,2-bis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionyl]hydrazine

[0030] The crosslinking agent is a combination of one or more of trimethylolpropane triacrylate, trimethylolpropane trimethacrylate, and triallyl isocyanurate.

[0031] The initiator is dicumyl peroxide.

[0032] A radiation cross-linked cable material with low radiation dose and high cross-linking degree, wherein the proportions of the components are as follows by weight:

[0033] Base resin A (UL00628 Lianhong Chemical) 10-15 parts;

[0034] Base resin B (SP1071C Japan Primen) 5-15 parts;

[0035] Compatibilizer (N129-1 Ningbo Energy Light) 10-15 parts;

[0036] Flame retardant (OL-104LE0 American Albemarle) 45-55 parts;

[0037] 1.2 to 1.5 parts of antioxidants (pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate, dilauryl 3,3'-dithiodipropionate, diethylenethiobis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], 1,2-bis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionyl]hydrazine);

[0038] 1.5-3.5 parts of auxiliary crosslinking agent (trimethylolpropane triacrylate, trimethylolpropane trimethacrylate, triallyl isocyanurate);

[0039] Initiator (dicumyl peroxide) 0.03-0.08 parts.

[0040] The preparation method of the low radiation dose and high cross-linking degree cable material is as follows:

[0041] (1) Place the base resin B in a stainless steel shake tank, pre-melt the initiator (diisopropylbenzene peroxide) at 45°C, and evenly spray it into the base resin B. Then start the shake tank at a speed of 4 rpm to fully mix and absorb the materials for 1 hour to obtain a premix of the base resin B.

[0042] (2) The premix of base resin A and base resin B, compatibilizer, flame retardant, antioxidant and co-crosslinking agent are uniformly mixed according to the above formula ratio, and the mixture is mixed and granulated through a two-stage extruder by forced feeding to finally obtain a low-irradiation-dose and high-crosslinking-degree cable material.

[0043] Example 1

[0044] An oil-resistant radiation-crosslinked low-smoke halogen-free flame-retardant cable material for locomotives with low radiation dose and high crosslinking degree, wherein the proportions of the components are as follows by weight:

[0045] Base resin A (UL00628 Lianhong Chemical) 15 parts;

[0046] Base resin B (SP1071C Japan Prime) 10 parts;

[0047] Compatibilizer (N129-1 Ningbo Energy Light) 15 parts;

[0048] Flame retardant (OL-104LE0 American Albemarle) 45 parts;

[0049] 1.2 parts of antioxidant (pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate);

[0050] Antioxidant (diethylene sulfide bis[3-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate]) 0.5 parts;

[0051] 1.5 parts of auxiliary cross-linking agent (triallyl isocyanurate);

[0052] Initiator (dicumyl peroxide) 0.03 parts.

[0053] The preparation method of the oil-resistant radiation-crosslinked low-smoke halogen-free flame-retardant cable material for locomotives with low radiation dose and high crosslinking degree in this embodiment is as follows:

[0054] (1) Place resin base material B in a 250 L mixing shake tank, spray the pre-melted initiator evenly into the resin base material B, start the shake tank, set the temperature in the tank to 55° C., and mix evenly at a rotation speed of 4 rpm for 1 h to obtain a premix of base material resin B.

[0055] (2) The premix of base resin B is uniformly mixed with the remaining other components. Twin screw extruder and The single screw extruder is used for extrusion granulation. The temperature of the twin screw extruder is set to 135-140-140-145-145-150-155-155-155, and the temperature of the single screw extruder is set to 140-145-150-155. The single screw extruder adopts the die surface hot cutting process. The particles are cooled by air and vacuum packaged to obtain low radiation dose and high cross-linking cable materials.

[0056] (3) The cable material is extruded into a 2.5 square stranded conductor single core wire with a wall thickness of 0.7 mm and an outer diameter of 3.2 mm using an extruder with a screw diameter of 45 and an extrusion temperature of 110-125-140-150-155-155.

[0057] Example 2

[0058] An oil-resistant radiation-crosslinked low-smoke halogen-free flame-retardant cable material for locomotives with low radiation dose and high crosslinking degree, wherein the proportions of the components are as follows by weight:

[0059] Base resin A (UL00628 Lianhong Chemical) 15 parts;

[0060] Base resin B (SP1071C Japan Prime) 10 parts;

[0061] Compatibilizer (N129-1 Ningbo Energy Light) 15 parts;

[0062] Flame retardant (OL-104LE0 American Albemarle) 45 parts;

[0063] 1.2 parts of antioxidant (pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate);

[0064] Antioxidant (diethylene sulfide bis[3-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate]) 0.5 parts;

[0065] 1.5 parts of auxiliary cross-linking agent (triallyl isocyanurate);

[0066] Initiator (dicumyl peroxide) 0.05 parts;

[0067] The preparation method of the oil-resistant radiation-crosslinked low-smoke halogen-free flame-retardant cable material for locomotives with low radiation dose and high crosslinking degree in this embodiment is as follows:

[0068] (1) Place resin base material A in a 250 L mixing shake tank, spray the pre-melted initiator evenly into the resin base material A, start the shake tank, set the temperature in the tank to 55° C., and mix evenly at a rotation speed of 4 rpm for 1 h to obtain a premix of base material resin A.

[0069] (2) The premix of base resin A is uniformly mixed with the remaining other components. Twin screw extruder and The single screw extruder is used for extrusion granulation. The temperature of the twin screw extruder is set to 135-140-140-145-145-150-155-155-155, and the temperature of the single screw extruder is set to 140-145-150-155. The single screw extruder adopts the die surface hot cutting process. The particles are cooled by air and vacuum packaged to obtain low radiation dose and high cross-linking cable materials.

[0070] (3) The cable material is extruded into a 2.5 square stranded conductor single core wire with a wall thickness of 0.7 mm and an outer diameter of 3.2 mm using an extruder with a screw diameter of 45 and an extrusion temperature of 110-125-140-150-155-155.

[0071] Example 3

[0072] An oil-resistant radiation-crosslinked low-smoke halogen-free flame-retardant cable material for locomotives with low radiation dose and high crosslinking degree, wherein the proportions of the components are as follows by weight:

[0073] Base resin A (UL00628 Lianhong Chemical) 15 parts;

[0074] Base resin B (SP1071C Japan Primen) 15 parts;

[0075] Compatibilizer (N129-1 Ningbo Energy Light) 10 parts;

[0076] Flame retardant (OL-104LE0 American Albemarle) 45 parts;

[0077] 1.2 parts of antioxidant (pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate);

[0078] Antioxidant (diethylene sulfide bis[3-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate]) 0.5 parts;

[0079] 1.5 parts of auxiliary cross-linking agent (triallyl isocyanurate);

[0080] Initiator (dicumyl peroxide) 0.03 parts;

[0081] The preparation method of the oil-resistant radiation-crosslinked low-smoke halogen-free flame-retardant cable material for locomotives with low radiation dose and high crosslinking degree in this embodiment is as follows:

[0082] (1) Place resin base material B in a 250 L mixing shake tank, spray the pre-melted initiator evenly into the resin base material B, start the shake tank, set the temperature in the tank to 55° C., and mix evenly at a rotation speed of 4 rpm for 1 h to obtain a premix of base material resin B.

[0083] (2) The premix of base resin B is uniformly mixed with the remaining other components. Twin screw extruder and The single screw extruder is used for extrusion granulation. The temperature of the twin screw extruder is set to 135-140-140-145-145-150-155-155-155, and the temperature of the single screw extruder is set to 140-145-150-155. The single screw extruder adopts the die surface hot cutting process. The particles are cooled by air and vacuum packaged to obtain low radiation dose and high cross-linking cable materials.

[0084] (3) The cable material is extruded into a 2.5 square stranded conductor single core wire with a wall thickness of 0.7 mm and an outer diameter of 3.2 mm using an extruder with a screw diameter of 45 and an extrusion temperature of 110-125-140-150-155-155.

[0085] Comparative Example 1

[0086] A conventional radiation cross-linked cable material and a preparation method thereof, wherein the proportions of the components are as follows:

[0087] Base resin A (UL00628 Lianhong Chemical) 15 parts;

[0088] Base resin B (SP1071C Japan Primen) 15 parts;

[0089] Compatibilizer (N129-1 Ningbo Energy Light) 10 parts;

[0090] Flame retardant (OL-104LE0 American Albemarle) 45 parts;

[0091] 1.2 parts of antioxidant (pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate);

[0092] Antioxidant (diethylene sulfide bis[3-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate]) 0.5 parts;

[0093] 1.5 parts of auxiliary cross-linking agent (triallyl isocyanurate);

[0094] (1) Base resin A, base resin B, compatibilizer, flame retardant, antioxidant and cross-linking agent are uniformly mixed. Twin screw extruder and The single screw extruder is used for extrusion granulation, the temperature of the twin screw extruder is set at 135-140-140-145-145-150-155-155-155, and the temperature of the single screw extruder is set at 140-145-150-155. The single screw extruder adopts the die face hot cutting process, and the particles are cooled by air and vacuum packed to obtain the traditional irradiated cross-linked cable material.

[0095] (2) The cable material is extruded into a 2.5 square stranded conductor single core wire with a wall thickness of 0.7 mm and an outer diameter of 3.2 mm using an extruder with a screw diameter of 45 and an extrusion temperature of 110-125-140-150-155-155.

[0096] Comparative Example 2

[0097] An oil-resistant radiation-crosslinked low-smoke halogen-free flame-retardant cable material for locomotives with low radiation dose and high crosslinking degree and a preparation method thereof, wherein the proportions of the components are as follows:

[0098] Base resin A (UL00628 Lianhong Chemical) 15 parts

[0099] Base resin B (SP1071C Japan Primen) 10 parts

[0100] Compatibilizer (N129-1 Ningbo Energy Light) 15 parts

[0101] Flame retardant (OL-104LE0 American Albemarle) 45 parts

[0102] Antioxidant (pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate) 1.2 parts

[0103] Antioxidant (diethylene thiobis[3-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate]) 0.5 parts

[0104] 1.5 parts of cross-linking agent (triallyl isocyanurate)

[0105] Initiator (dicumyl peroxide) 0.03 parts

[0106] (1) Base resin A, base resin B, compatibilizer, flame retardant, antioxidant, co-crosslinking agent and initiator are uniformly mixed. Twin screw extruder and The single screw extruder is used for extrusion granulation, the temperature of the twin screw extruder is set at 135-140-140-145-145-150-155-155-155, and the temperature of the single screw extruder is set at 140-145-150-155. The single screw extruder adopts the die face hot cutting process, and the particles are cooled by air and vacuum packed to obtain the traditional irradiated cross-linked cable material.

[0107] (2) The cable material is extruded into a 2.5 square stranded conductor single core wire with a wall thickness of 0.7 mm and an outer diameter of 3.2 mm using an extruder with a screw diameter of 45 and an extrusion temperature of 110-125-140-150-155-155.

[0108] The cables prepared in the above Examples 1 to 3 and Comparative Example 1 were sent to the irradiation processing plant for irradiation according to the measurement of 6 Mrad. The wire samples after irradiation were sampled for thermal extension, gel content, tensile strength and elongation at break tests, wherein the thermal extension (200°C @ 15min @ 0.2MPa) was tested in accordance with GB / T2951.21, the gel content was tested in accordance with Appendix A of JB / T10437, and the tensile strength and elongation at break were tested in accordance with GB / T2951.11. The test results are shown in Table 1 below.

[0109] Table 1 Comparison of the properties of Examples 1 to 3 and Comparative Examples 1 and 2 after irradiation crosslinking

[0110]

[0111] As can be seen from Table 1, under low irradiation dosage, the thermal extension of Comparative Example 1 fails to meet the requirements, and the gel content is also low. Comparative Example 2 also has the problem of failing to meet the requirements for thermal extension. The main reason is that the initiator is not dispersed enough, and the ideal cross-linking effect cannot be achieved. In addition, the extruded wire of Comparative Example 2 is not smooth. The reason is that the initiator and the cross-linking agent are added at the same time and are not evenly dispersed, that is, they are mixed together, which easily leads to partial pre-cross-linking. Examples 1 to 3 can all meet the thermal extension requirements under a low irradiation dosage of 6 Mrad. The gel content also reflects the ideal effect of cross-linking, the tensile properties are suitable, and the extruded wire surface is smooth. Because the addition of the initiator is controlled, the above process has a good dispersion effect. The initiator promotes the generation of free radicals under low irradiation dosage conditions, effectively improving the efficiency of radiation cross-linking.

[0112] The cable material prepared by the present invention has a higher gel content than the comparative example. The gel in the cable can not only protect the internal wires of the cable from being corroded by the external environment during the cable manufacturing process, but also fill the gaps in the cable, improve the thermal conductivity and waterproof performance of the cable, and improve the anti-aging performance and pressure resistance of the cable. Therefore, the gel content determines the quality and reliability of the cable. A high gel content can extend the service life of the cable and reduce the cost of maintenance and replacement.

[0113] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A low-irradiation-dose, high-crosslinking-degree oil-resistant radiation-crosslinked low-smoke, halogen-free cable material for locomotives. It is characterized in that In terms of weight, the proportions of each component are as follows: 10 to 15 parts of base resin A, 5 to 15 parts of base resin B, 10 to 15 parts of compatibilizer, 45 to 55 parts of flame retardant, 1.2 to 1.5 parts of antioxidant, 1.5 to 3.5 parts of cross-linking agent, and 0.03 to 0.08 parts of initiator.

2. According to claim 1, the oil-resistant radiation-crosslinked low-smoke halogen-free cable material for locomotives with low radiation dose and high crosslinking degree, It is characterized in that In terms of weight, the proportions of each component are as follows: 15 parts of base resin A, 10 parts of base resin B, 15 parts of compatibilizer, 45 parts of flame retardant, 1.2 parts of antioxidant, 1.5 parts of co-crosslinking agent, and 0.05 parts of initiator.

3. According to claim 1, the oil-resistant radiation-crosslinked low-smoke halogen-free cable material for locomotives with low radiation dose and high crosslinking degree, It is characterized in that The base resin A is ethylene-vinyl acetate copolymer, the VA content of the ethylene-vinyl acetate copolymer is 28% to 33%, and the melt flow rate at 190°C@2.16kg is 0.02g / 10min to 4g / 10min.

4. According to claim 1, the oil-resistant radiation-crosslinked low-smoke halogen-free cable material for locomotives with low radiation dose and high crosslinking degree, It is characterized in that The resin B is a highly branched polyethylene resin, and the density of the highly branched polyethylene resin is 0.916 g / cm 3 ~0.918g / cm 3 , the melt flow rate at 190℃@2.16kg is 5g / 10min~10g / 10min.

5. According to claim 1, the oil-resistant radiation-crosslinked low-smoke halogen-free cable material for locomotives with low radiation dose and high crosslinking degree, It is characterized in that The compatibilizer is selected from one or more of PE-MAH grafted materials, EVA-MAH grafted materials and POE-MAH grafted materials; the flame retardant is one or more of aluminum hydroxide, magnesium hydroxide, MCA and nano-montmorillonite.

6. The oil-resistant radiation-crosslinked low-smoke halogen-free cable material for locomotives with low radiation dose and high crosslinking degree according to claim 1, It is characterized in that The antioxidant is selected from one or more of pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate, dilauryl 3,3'-thiodipropionate, diethylenethiobis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate] and 1,2-bis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionyl]hydrazine.

7. The oil-resistant radiation-crosslinked low-smoke halogen-free cable material for locomotives with low radiation dose and high crosslinking degree according to claim 1, It is characterized in that The auxiliary cross-linking agent is selected from one or more of trimethylolpropane triacrylate, trimethylolpropane trimethacrylate and triallyl isocyanurate.

8. The oil-resistant radiation-crosslinked low-smoke halogen-free cable material for locomotives with low radiation dose and high crosslinking degree according to claim 1, It is characterized in that The initiator is dicumyl peroxide.

9. The oil-resistant radiation-crosslinked low-smoke halogen-free cable material for locomotives with low radiation dose and high crosslinking degree according to any one of claims 1 to 8, It is characterized in that When the oil-resistant radiation-crosslinked low-smoke halogen-free cable material for locomotives with low radiation dose and high crosslinking degree is extruded into wire and then radiation-crosslinked, the radiation dose is 6 Mrad.

10. A method for preparing a low-irradiation-dose, high-crosslinking-degree oil-resistant radiation-crosslinked low-smoke, halogen-free cable material for locomotives as claimed in any one of claims 1 to 9, It is characterized in that Here are the steps: (1) First, the initiator is pre-melted and evenly sprayed into the base resin B, and then stirred to fully mix the materials to obtain a premix of the base resin B; (2) The premix of the base resin B prepared in step (1) is uniformly mixed with the base resin A, a compatibilizer, a flame retardant, an antioxidant, and a cross-linking agent according to a formula ratio, and the mixture is mixed and granulated through a two-stage extruder by forced feeding to obtain an oil-resistant radiation-crosslinked low-smoke halogen-free cable material for locomotives with a low radiation dose and a high cross-linking degree.

Citation Information

Patent Citations

  • Irradiation crosslinking halogen-free high flame-retardant cable material and preparation method thereof

    CN101914236A

  • Preparation method of shielding material with power of 110KV and above

    CN102850558A

  • Novel process for adding peroxide into PP melt-blown material

    CN112646208A

  • Eco friendly crosslinked flame retardant composition for wire and cable

    US20110278039A1

Cited By

  • Oil-resistant low-temperature-resistant irradiation crosslinking halogen-free low-smoke flame-retardant elastomer insulating material as well as preparation method and application thereof